Coal-based negative electrode material and preparation method and application thereof
By extrusion coating and high-temperature graphitization of carbon-containing raw materials and mesophase asphalt powder, coal-based graphite anode material with nano-carbon microsphere structure was prepared, which solved the problem of insufficient performance of existing lithium-ion battery anode materials. High capacity and high efficiency electrochemical performance is achieved and cost-effective.
Patent Information
- Application Number
- CN202310573779.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-19
- Publication Date
- 2024-11-22
AI Technical Summary
The performance of the existing lithium-ion battery negative electrode materials is insufficient, especially in terms of first discharge capacity, first efficiency and circulation performance. The material cost is high, the process is complicated, and the stability of the graphite substrate surface coating layer leads to poor battery cycling stability.
The carbon-containing element raw material and mesophase asphalt powder are mixed. After extrusion coating, high-temperature carbonization and high-temperature graphitization, a coal-based graphite structure negative electrode material containing nanocarbon microspheres is prepared, and an integrated structure is formed through chemical reactions to improve the Electrochemical properties of materials.
The first discharge capacity, first efficiency and cycling performance of the material have been significantly improved. The first discharge capacity is higher than 350mAh/g, the first efficiency is higher than 94%, the cycle performance is excellent, the cost is low and the resources are abundant.
Smart Images

Figure HDA0004241906150000011
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery materials, and in particular to a coal-based negative electrode material and a preparation method and application thereof. Background Art
[0002] At present, the main material for negative electrodes of lithium-ion batteries is graphite. The precursor of graphite is natural graphite ore or coke-like substances. Due to the many defects on the surface of graphite, it cannot be directly used as a negative electrode material. It is generally prepared into a "core-shell" structure through surface modification technology or a secondary particle structure through granulation technology, thereby improving the material's rate and cycle performance.
[0003] CN102522561A discloses a "core-shell" structure of a coal-based material, which is prepared by mixing a binder with a coal-based material in liquid phase and then carbonizing it at high temperature, wherein the core is graphitized anthracite and the shell is amorphous carbon. This method uses liquid phase coating, which has a high cost and the first coulomb efficiency of the material will also be reduced.
[0004] CN111146417A discloses a "secondary particle" structure of a coal-based material. Anthracite is first activated with KOH and graphitized at high temperature to obtain a porous graphite material, which is then mixed with a binder liquid phase and coated and then prepared by spray drying. The secondary particle structure is a structure formed by porous graphitized anthracite particles coated and bonded by an organic precursor. The method has cumbersome procedures (a large amount of water washing is required after KOH activation, wasting water resources) and high costs. Since the material is porous, it is difficult to ensure the processing performance of the battery terminal.
[0005] In addition, from 2021 to 2022, the prices of negative electrode coke materials have been rising, and the materials are in short supply, and there is an urgent need to find alternatives with excellent performance.
[0006] CN102299308A reports a lithium ion battery negative electrode material and a preparation method thereof, wherein the material is a composite material composed of carbon nanotubes and / or carbon nanofibers formed by in-situ growth directly on the surface of a graphite substrate by a chemical vapor deposition method, and carbon nanotubes and / or carbon nanofibers mixed between graphite substrates. The use of the material as a lithium ion battery graphite negative electrode material improves the discharge capacity, rate performance, liquid absorption and cycle performance of the lithium ion battery. However, the specific surface area of the material obtained by the method is large, and the surface coating layer formed by vapor deposition alone is relatively loose, which will make the stability of the SEI film formed during the charge and discharge process poor, consume more electrolyte, and cause the battery to have poor high temperature cycle stability. Summary of the invention
[0007] In view of this, the main purpose of the present invention is to provide a coal-based negative electrode material and its preparation method and application. A coal-based graphite structured negative electrode material containing nano-carbon microspheres is prepared for the first time using carbon-containing raw materials and intermediate phase asphalt as raw materials. The first discharge capacity, first efficiency and cycle performance of the material are greatly improved.
[0008] To achieve the above-mentioned purpose of the invention, the first aspect of the present invention provides a method for preparing a coal-based negative electrode material, comprising the following steps: mixing crushed carbon-containing raw materials with intermediate phase asphalt powder, and after mixing, sequentially subjecting the mixture to extrusion coating, high-temperature carbonization treatment, pulverization treatment and high-temperature graphitization treatment to obtain a negative electrode material, wherein the mass ratio of the carbon-containing raw materials to the intermediate phase asphalt powder is 2-4:1.
[0009] Furthermore, the carbon-containing raw material is selected from one or more of anthracite and petroleum coke.
[0010] Furthermore, the ash content of the anthracite is less than 10%.
[0011] Furthermore, the carbon-containing raw material is crushed to D50=5-50 μm, preferably 8-15 μm.
[0012] Furthermore, the particle size D50 of the mesophase asphalt powder is less than 10 μm.
[0013] Furthermore, the temperature of the high temperature carbonization treatment is 800-1300°C.
[0014] Furthermore, the pulverizing process crushes the material to D50=8-15 μm.
[0015] Furthermore, the high temperature graphitization temperature is greater than 2800°C.
[0016] The second aspect of the present invention provides a coal-based negative electrode material prepared by the above method, wherein the surface of the material has nano-carbon microspheres with a particle size of 1-100 nm.
[0017] The third aspect of the present invention also provides the application of the coal-based negative electrode material prepared by the above method, which is used to manufacture lithium-ion batteries.
[0018] Compared with the prior art, the present invention has the following advantages:
[0019] The present invention mixes crushed carbon-containing raw materials with mesophase asphalt powder, and after mixing, sequentially undergoes extrusion coating, high-temperature carbonization treatment, crushing treatment and high-temperature graphitization treatment to obtain a negative electrode material; wherein, the mesophase asphalt is uniformly dispersed on the surface of the material by extrusion coating, so that the mesophase building units are dispersed, and their polymerization to form mesophase spheres is blocked during high-temperature graphitization, thereby forming nano-carbon microspheres; therefore, the carbon-containing raw materials and asphalt of the present invention form an integrated structure through chemical reaction, so that the surface of the material contains nano-carbon microspheres (particle size 1-100nm), and after electrochemical testing, the first discharge capacity, first efficiency and cycle performance of the material are greatly improved, that is, it has a high capacity of >350mAh / g, a high efficiency of >94%, excellent cycle performance, and a capacity retention rate of >99% after 50 cycles at 0.2C. Furthermore, the present invention uses anthracite as a carbon precursor, anthracite resources are abundant, and the price is low, taking into account both low cost and better electrochemical performance.
[0020] Other features and advantages of the present invention will be described in detail through the following detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the following specific embodiments, they are used to explain the present invention but do not constitute a limitation of the present invention. In the accompanying drawings:
[0022] Figure 1 (a) and (b) are the SEM images of the coal-based negative electrode material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0023] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0024] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0025] In the following examples and comparative examples:
[0026] (1) Main raw materials
[0027] Anthracite is selected from low-ash high-quality anthracite with an ash content of less than 10%, and the raw materials have not been chemically treated for ash removal.
[0028] The asphalt is mesophase asphalt powder with a softening point of about 250 degrees and is purchased from outside.
[0029] (2) Characterization and testing
[0030] The method for obtaining the lithium removal capacity is as follows: coal-based graphite, polyvinylidene fluoride (PVDF), acetylene carbon black (Super P) are mixed with N-methylpyrrolidone (NMP) in a mass ratio of 92:5:3 to form a slurry, and the slurry is evenly coated on a copper foil current collector with a thickness of 0.012 mm. After vacuum drying at 80°C for 24 hours, after the solvent is completely evaporated, a circular electrode sheet with a diameter of about 12 mm is punched. In an MBraun2000 glove box (Ar atmosphere, H2O and O2 concentrations less than 0.1uL / L), button cells are assembled, metal lithium sheets are used for the electrodes, Celgard2400 composite diaphragms are used for the diaphragms, and 1M LPF6 / EC+DMC+EMC solution is used for the electrolyte. After the battery is assembled, it is left to stand for 24 hours for electrochemical testing. The charge and discharge performance test was conducted using a CT2001 battery tester (Blue Electric Electronics Co., Ltd.), with a charge and discharge voltage range of 0.0 to 1.5 V. The first-week charge and discharge capacity test was conducted at 0.1 C, and the cycle test was conducted at 0.2 C. De-lithium capacity: The battery was discharged at 0.1 C, and the capacity when discharged to 0.005 V was recorded as the lithium insertion capacity. The first-week charging test was then conducted at a current density of 0.1 C, and the capacity when charged to 1.5 V was recorded as the de-lithium capacity.
[0031] Capacity retention rate: read the first delithiation specific capacity and the 100th delithiation specific capacity, and calculate the 100th delithiation specific capacity / first delithiation specific capacity × 100%.
[0032] The present invention provides a method for preparing a coal-based negative electrode material, comprising the following steps: mixing crushed carbon-containing raw materials with mesophase asphalt powder, and then subjecting the mixture to extrusion coating, high-temperature carbonization treatment, pulverization treatment and high-temperature graphitization treatment to obtain a negative electrode material, wherein the mass ratio of the carbon-containing raw materials to the mesophase asphalt powder is 2-4:1.
[0033] During the research process of the present invention, the inventors found that the carbon-containing raw material (such as coal) and asphalt are extruded, and the asphalt is bonded to the surface of the carbon-containing raw material. When the asphalt is in an appropriate amount, the carbon-containing raw material blocks its polymerization to form intermediate phase spheres during high-temperature graphitization, thereby forming nano-carbon microspheres; on the contrary, if the main component is asphalt, the carbon-containing raw material will not play a blocking role and nano-carbon microspheres cannot be formed.
[0034] In the present invention, the carbon-containing raw material is selected from one or more of anthracite and petroleum coke. In a specific example, the above-mentioned carbon-containing raw material is crushed to D50 = 5-50μm, preferably 8-15μm, such as 8μm, 9μm, 10μm, 11μm, 12μm, 13μm, 14μm, 15μm or other values within this range. This treatment can be carried out using a conventional pulverizer. If the particle size of the above-mentioned carbon-containing raw material is too small, the yield will be low, the cost will be high, the battery end processing performance will be poor, and the capacity will also be low; if the particle size is too large, the rate performance will also be poor.
[0035] In the present invention, the particle size D50 of the mesophase asphalt powder is less than 10 μm, for example, 3 μm, 4 μm, 5 μm, 6 μm, 7 μm, 8 μm, 9 μm, etc.
[0036] In the present invention, the mass ratio of the above-mentioned pulverized carbon-containing raw material to the mesophase pitch powder is 2-4:1, such as 2:1, 2.5:1, 3:1, 3.5:1, 4:1 or other values within this range. Within the above-mentioned mass ratio range, it is suitable to obtain a nano-carbon microsphere structure on the surface of the material, which significantly improves the capacity and first efficiency cycle of the material. According to characterization, the particle size D50 of the material of the present invention is 8-12μm, and the particle size of the nano-carbon microspheres on the surface of the material is 1-100nm.
[0037] It is understandable that when the crushed carbon-containing raw material is mixed with the mesophase asphalt powder, auxiliary measures can be used to fully mix them. For example, in a specific example, the carbon-containing raw material and the mesophase asphalt powder are placed in a mixer and rotated at high speed to mix them.
[0038] In the present invention, the extrusion coating method is not particularly limited, and the commonly used extrusion device and corresponding processing technology in the industry can be used.
[0039] In the present invention, the temperature of the high temperature carbonization treatment is 800-1300°C, such as 800°C, 850°C, 900°C, 950°C, 1000°C, 1050°C, 1100°C, 1150°C, 1200°C, 1300°C or other values within the range. The treatment can adopt conventional carbonization equipment and operation steps in the industry, such as a box-type atmosphere protection furnace or a box-type resistance furnace.
[0040] In the present invention, the material treated by high temperature carbonization is further pulverized, preferably 8-15 μm, such as 8 μm, 9 μm, 10 μm, 11 μm, 12 μm, 13 μm, 14 μm, 15 μm or other values within this range. This treatment can be carried out using a conventional pulverizer. If the particle size of the pulverized material is too small, the yield will be low, the cost will be high, the processing performance of the battery end will be poor, and the capacity will also be low; if the particle size is too large, the rate performance will also be poor.
[0041] In the present invention, the high temperature graphitization temperature is greater than 2800°C, such as 2900°C, 2950°C, 3000°C, 3050°C, 3100°C, etc. The treatment can adopt conventional graphitization equipment and operation steps in the industry, such as an industrial Acheson graphitization furnace. High temperature treatment is the process of converting the precursor into negative electrode graphite. If the temperature is too low, graphite cannot be formed, and the capacity and first efficiency will also be reduced.
[0042] The present invention is further described below with detailed exemplary embodiments, but these embodiments do not constitute any limitation to the present invention.
[0043] Example 1
[0044] The anthracite raw material is crushed to D50 = 9 μm, and then mixed with the intermediate phase asphalt powder (about 8 μm) at a mass ratio of 2:1, and evenly mixed using a high-speed VC mixer at a speed of 1250 rpm. After that, an extruder is used for extrusion coating, high-temperature carbonization at 1150°C is performed, and the material is crushed to 9 μm, and then graphitized at 3000°C to obtain a coal-based negative electrode material.
[0045] The electrochemical performance of the material is characterized as follows:
[0046] Coal-based negative electrode material, conductive carbon black and binder were mixed in a mass ratio of 92:3:5, stirred evenly and coated on copper foil, and dried at 110°C for 12h. The obtained electrode was used as the positive electrode, and the lithium sheet was used as the negative electrode to assemble a button battery;
[0047] The assembled battery was subjected to constant current charge and discharge test on LAND, with the voltage range set to 0.005-1.5 V. Electrochemical performance test: 0.1C capacity 352 mAh / g, first efficiency 94.1%, 0.2C cycle 50 weeks capacity retention rate 99.3%.
[0048] Example 2
[0049] The anthracite was crushed and mixed with the mesophase asphalt in a mass ratio of 4:1, and the rest was the same as in Example 1 to obtain a coal-based negative electrode material.
[0050] The electrochemical performance test of the material showed that the capacity at 0.1C was 351 mAh / g, the first efficiency was 94.2%, and the capacity retention rate at 0.2C cycle for 50 weeks was 98.9%.
[0051] Example 3
[0052] The anthracite was crushed and mixed with the mesophase asphalt in a mass ratio of 3:1, and the rest was the same as in Example 1 to obtain a coal-based negative electrode material.
[0053] The electrochemical performance test of the material showed that the capacity at 0.1C was 350 mAh / g, the first efficiency was 94.8%, and the capacity retention rate at 0.2C cycle for 50 weeks was 98.3%.
[0054] Example 4
[0055] The anthracite raw material was crushed to D50=12 μm, and mixed with mesophase asphalt at a mass ratio of 3:1. The carbonization temperature was 1050° C., and the rest was the same as in Example 1.
[0056] The electrochemical performance test of the material showed that the capacity at 0.1C was 349 mAh / g, the first efficiency was 94.3%, and the capacity retention rate at 0.2C cycle for 50 weeks was 97.9%.
[0057] Example 5
[0058] The anthracite raw material was crushed to D50=15 μm, and mixed with mesophase pitch at a mass ratio of 2:1. The carbonization temperature was 900° C., and the rest was the same as in Example 1.
[0059] The electrochemical performance test of the material showed that the capacity at 0.1C was 351 mAh / g, the first efficiency was 94.5%, and the capacity retention rate at 0.2C cycle for 50 weeks was 97.1%.
[0060] Comparative Example 1
[0061] The anthracite raw material was crushed to D50=9 μm, carbonized at 1150°C, and then graphitized at 3000°C to obtain a graphitized sample.
[0062] The electrochemical performance is characterized as follows:
[0063] The graphitized sample, conductive carbon black and binder were mixed in a mass ratio of 92:3:5, stirred evenly and coated on copper foil, and dried at 110°C for 12h. The obtained electrode was used as the positive electrode and the lithium sheet as the negative electrode to assemble a button battery.
[0064] The assembled battery was subjected to constant current charge and discharge test on LAND, with the voltage range set to 0.005-1.5 V. Electrochemical performance test: 0.1C capacity 345 mAh / g, first efficiency 93.9%, 0.2C cycle 50 weeks capacity retention rate 87%.
[0065] Comparative Example 2
[0066] The mesophase pitch is crushed to D50=9 μm, and then subjected to high temperature carbonization at 1150°C, and then subjected to high temperature graphitization at 3000°C.
[0067] Comparative Example 3
[0068] Similar to Example 1, except that the anthracite raw material is crushed to D50=9 μm and then mixed with the mesophase pitch powder in a mass ratio of 2:3.
[0069] The electrochemical performance test of the material showed that the capacity at 0.1C was 348.9 mAh / g, the first efficiency was 93.8%, and the capacity retention rate after 50 cycles at 0.2C was 98.9%.
[0070] In summary, the surfaces of the materials obtained in Examples 1-5 of the present invention contain nano-carbon microspheres. After electrochemical testing, the first discharge capacity, first efficiency and cycle performance of the materials are greatly improved.
[0071] Comparative Example 1 is to directly graphitize the anthracite after crushing it, and it is impossible to obtain particles with nano-carbon microspheres on the surface. Comparative Example 2 is to directly graphitize the mesophase asphalt after crushing it, and it is also impossible to obtain particles with nano-carbon microspheres on the surface. Comparative Example 3 is to crush the anthracite and mix it with the mesophase asphalt in a mass ratio of 2:3, and the surface of the coal-based negative electrode material obtained by the process does not contain nano-carbon microsphere particles.
[0072] Obviously, the above embodiments of the present invention are merely examples for clearly explaining the present invention, and are not intended to limit the implementation methods of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is impossible to list all implementation methods here. All obvious changes or modifications derived from the technical solution of the present invention are within the spirit scope of the present invention.
Claims
1. A method for preparing a coal-based negative electrode material, characterized in that: The method comprises the following steps: mixing crushed raw materials containing carbon elements with mesophase asphalt powder, and then subjecting the mixture to extrusion coating, high-temperature carbonization treatment, pulverization treatment and high-temperature graphitization treatment to obtain negative electrode materials, wherein the mass ratio of the raw materials containing carbon elements to the mesophase asphalt powder is 2-4:
1.
2. The method for preparing a coal-based negative electrode material according to claim 1, characterized in that: The carbon-containing raw material is selected from one or more of anthracite and petroleum coke.
3. The method for preparing a coal-based negative electrode material according to claim 2, characterized in that: The anthracite has an ash content of less than 10%.
4. The method for preparing a coal-based negative electrode material according to claim 1 or 2, characterized in that: The carbon-containing raw material is crushed to D50=5-50 μm, preferably 8-15 μm; and / or the mesophase asphalt powder particle size D50 is less than 10 μm.
5. The method for preparing a coal-based negative electrode material according to any one of claims 1 to 4, characterized in that: The temperature of the high temperature carbonization treatment is 800-1300°C.
6. The method for preparing a coal-based negative electrode material according to any one of claims 1 to 5, characterized in that: The pulverization process crushes the material to D50=8-15 μm.
7. The method for preparing a coal-based negative electrode material according to any one of claims 1 to 6, characterized in that: The high temperature graphitization temperature is greater than 2800°C.
8. A coal-based negative electrode material prepared by the method according to any one of claims 1 to 7.
9. The coal-based negative electrode material according to claim 8, characterized in that: The surface of the material is provided with nano carbon microspheres with a particle size of 1-100 nm.
10. Use of the coal-based negative electrode material prepared by the method according to any one of claims 1 to 7, wherein the coal-based negative electrode material is used to manufacture lithium-ion batteries.
Citation Information
Patent Citations
Preparation method of core-shell type mesocarbon microbeads
CN113845114A
Coal-based negative electrode material and preparation method and application thereof
CN115472826A
Graphite negative electrode material and preparation method and application thereof
CN115472828A
Method for preparing composite graphite, composite graphite and lithium ion battery
WO2017050260A1