Method for continuously preparing large-particle rare earth fluorocarbonate and co-producing nano spherical silicon dioxide by using fluorine-silicon mixed waste acid
Through the continuous concurrent precipitation technology of fluorosilic mixed waste acid, the precise control of large-grain fluorocarbonate rare earths is achieved, solving the problems of long process and low fluorination efficiency in traditional methods, and improving product quality and production efficiency.
Patent Information
- Application Number
- CN202411113559.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-14
AI Technical Summary
The traditional fluorocarbonate rare earth production methods have problems such as long process time, uneven reaction, local fluorination, amorphous precipitation, many impurities entrainment and low fluorination efficiency, resulting in lattice defects of the polishing powder, uneven aggregate size and polishing accuracy. Low.
Fluorosilicone mixed waste acid and ammonia water are stirred and mixed, and alkaline fluorine-containing solution and monobasic alkaline mixed solution are combined to form composite precipitation solution A, and nucleation and dielectric are induced in a continuous precipitation device through continuous co-current precipitation reaction. The four units of growth, control endpoint and maturation crystal form are achieved to achieve precise control of large-grain fluorocarbonate rare earths.
The crystal form of fluorocarbonate rare earths has been intact, large particles and uniform fluorination, avoiding impurities inheritance, improving fluorination efficiency and product quality, and is suitable for high-value utilization in the rare earth and phosphorus chemical industries.
Smart Images

Figure CN118993131A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of rare earths, and in particular to a method for continuously preparing large-particle rare earth fluoride carbonate and co-producing nano-spherical silicon dioxide by using fluorine-silicon mixed waste acid. Background Art
[0002] There are two traditional methods for producing rare earth fluorocarbonate. One is fluorination followed by carbon precipitation, that is, first the fluorinating agent is subjected to fluorination reaction with part of the rare earth solution, and then carbonate is used for complete precipitation; the other is carbon precipitation followed by fluorination, that is, first the rare earth solution and carbonate are completely precipitated, and then partially fluorinated with a fluorinating agent after washing. Regardless of the process, it is a two-step reaction, which leads to problems such as long process time, uneven reaction or partial fluorination, amorphous precipitation, many impurities and low fluorination efficiency. At the same time, rare earth fluorocarbonate is widely used as a precursor of fluorine-containing rare earth polishing powder material. Rare earth fluorocarbonate synthesized by traditional preparation methods leads to lattice defects in the back-end polishing powder, uneven agglomerate size, and low polishing accuracy and rate.
[0003] The invention patent with patent publication number CN110885637B discloses a method for preparing a fluorinated rare earth polishing powder and a fluorinated rare earth polishing liquid. A high-energy ball mill is used to fully mix rare earth carbonate and rare earth fluoride, and additives are added, spray drying and other treatment methods are used to prepare the fluorinated rare earth polishing powder, so that the precursors are mixed evenly, and a high cutting rate is achieved under the premise of ensuring that the optical glass surface has no surface defects such as scratches. However, the ball milling process is a mechanochemical effect, and the crystal lattice structure cannot be completely uniform, and free fluoride ions and fluorides are generated to cause polishing scratch defects. In addition, a small amount of fluoride will be hydrolyzed to release fluoride ions during the ball milling process. Therefore, the fluoride-containing wastewater directly evaporates in the spray drying process to produce HF acid gas to corrode the equipment, and the equipment ages seriously over a long period of time.
[0004] The invention patent with patent publication number CN112724839B discloses a system and method for preparing rare earth polishing powder, which utilizes a wet ball milling device, a dehydration and drying device, and a modification device to prepare fluorinated rare earth carbonate, so that the rare earth carbonate is first refined and then modified, so that the grain size of the rare earth carbonate precursor is uniform and the fluorination reaction is complete, but the particle size and morphology are completely controlled by the rare earth carbonate. The process is cumbersome, and the rare earth carbonate needs to go through stirring, sand milling, ball milling, and modification processes, which is time-consuming and inefficient.
[0005] The invention patent with patent publication number CN104387988B discloses a method for preparing ultrafine fluorinated cerium-based polishing powder, which adopts a coprecipitation method to react a rare earth salt solution with a mixed solution of a carbonate precipitant and a fluorinating agent to prepare ultrafine fluorinated cerium-based polishing powder. The invention has the advantages of low reaction temperature, short reaction and aging time, but the precursor particle size is small, there is a problem of difficulty in filtering, and the raw material concentration is low, only 100-150g / L, and the output per unit time is low. Summary of the invention
[0006] In view of the above problems, the purpose of the present invention is to provide a method for continuously preparing large-particle rare earth fluoride carbonate and co-producing nano-spherical silica using fluorine-silicon mixed waste acid. The present invention first stirs and mixes the fluorine-silicon mixed waste acid with an ammonia solution, and then compounding the alkaline fluorine-containing solution with a monobasic alkaline mixed solution to obtain a composite precipitation solution A. Finally, the composite precipitation solution A and a soluble rare earth salt solution B are continuously added to a continuous precipitation reaction device for reaction, and large-particle rare earth fluoride carbonate is obtained after solid-liquid separation. The continuous precipitation reaction of the present invention includes four units: an induced nucleation unit, a dielectric growth unit, an endpoint control unit, and a mature crystal unit, which realizes precise control of each stage of fluorine carbonate rare earth from nucleation, growth to crystallization, and has obvious advantages such as intact precipitation crystal form, large particles, and uniform fluorination. At the same time, the co-production of SiO 2 The single crystal morphology is spherical, high in purity and has a wide range of applications. The present invention further combines the treatment of fluorine-silicon mixed waste acid produced in the rare earth and phosphorus chemical industries with the development of rare earth fluoride functional materials, and proposes an industrially feasible technical solution for the high-value utilization of fluorine / silicon resources.
[0007] The present invention achieves the above-mentioned purpose through the following technical solutions.
[0008] The present invention provides a method for continuously preparing large-particle rare earth fluoride carbonate and co-producing nano-spherical silicon dioxide by using fluorine-silicon mixed waste acid, comprising the following steps:
[0009] (1) Removal of silicon from fluorine-silicon mixed waste acid: Mixing the fluorine-silicon mixed waste acid with ammonia water to obtain an alkaline fluorine-containing solution and nano-spherical silica;
[0010] (2) Compounding the precipitant: compounding the alkaline fluorine-containing solution obtained in step (1) with a monobasic alkaline mixed solution to obtain a composite precipitation solution A;
[0011] (3) Continuous co-current precipitation: the composite precipitation solution A obtained in step (2) is subjected to a continuous precipitation reaction with the soluble rare earth salt solution B;
[0012] (4) solid-liquid separation: filtering the mature slurry obtained in step (3) to obtain a filter cake and a filtrate, wherein the filtrate is an ammonium salt aqueous solution or a sodium salt aqueous solution, and the filter cake is large particles of rare earth fluorocarbonate;
[0013] The particle size D of the large particle fluorocarbonate rare earth 50 ≥28μm, particle size range is (D 90 -D 10 ) / D 50 ≤1.5; the primary particle size D of the nano-spherical silica 50 ≤300nm, particle size range is (D 90 -D 10 ) / D 50 ≤1.5;
[0014] In step (3), the continuous precipitation reaction includes inducing nucleation, dielectric growth, controlling the endpoint and aging crystallization process in sequence.
[0015] Preferably, in step (1), the fluorine-silicon mixed waste acid is selected from waste acid containing fluorine silicic acid or waste acid containing hydrofluoric acid and fluorine silicic acid, the content of fluorine element in the fluorine-silicon mixed waste acid is 90-250 g / L, and the content of silicon element is 0.5-10 wt %; the pH value of the alkaline fluorine-containing solution obtained by stirring and mixing the fluorine-silicon mixed waste acid with ammonia water is controlled to be 7.2-9.5.
[0016] Preferably, in step (2), the monobasic alkaline mixed solution is selected from a mixed solution of carbonate and alkali solution, the carbonate is selected from at least one of ammonium bicarbonate, ammonium carbonate, sodium bicarbonate, sodium carbonate liquid or solid; the alkali solution is selected from at least one of ammonia water or sodium hydroxide solution; - The alkaline fluoride solution and HCO 3 - The molar ratio of the monobasic alkaline mixed solution is (0.267~1):1.
[0017] Preferably, in step (3), the soluble rare earth salt solution is selected from one of rare earth chlorides, rare earth sulfates, rare earth nitrates and rare earth acetates, and the temperature of the entire continuous precipitation reaction process is 25 to 80°C.
[0018] Preferably, in step (3), the continuous precipitation reaction is carried out in a continuous precipitation reaction device, and the composite precipitation solution A and the soluble rare earth salt solution B are continuously added to the continuous precipitation reaction device, and the continuous precipitation reaction device is divided into four units, namely, an induced nucleation unit, a dielectric growth unit, an endpoint control unit and a aging crystal form, which respectively carry out induced nucleation, dielectric growth, endpoint control and aging crystallization processes, and each unit is fed from the bottom of the reaction device, and the reaction time of each unit is ≥30min.
[0019] The continuous precipitation reaction device is divided into 7 stages. The reaction slurry of each stage flows to the next stage, but not all of the slurry flows into the next stage. There will be bottom liquid left at the bottom, and the raw materials will continuously flow into the bottom liquid of the previous round in the device.
[0020] Preferably, the induced nucleation unit is set as a first-stage reaction device, the composite precipitation solution A and the soluble rare earth salt solution B are added to the first-stage reaction device in parallel to carry out a rare earth fluorocarbonate induced nucleation reaction, and the obtained first-stage seed slurry automatically overflows to the next-stage reaction device;
[0021] The dielectric growth unit is set as a 2-4 stage reaction device, the composite precipitation solution A is added into the 2-4 stage reaction device to carry out dielectric growth reaction of rare earth fluoride carbonate crystal nuclei, and the grown slurry automatically overflows to the next stage reaction device;
[0022] The control endpoint unit is set as a 5-6 stage reaction device, equipped with an online detection pH meter, a monobasic alkaline mixed solution and / or a 1-stage seed slurry is added to the 5-6 stage reaction device to perform a rare earth complete precipitation reaction, and the obtained complete precipitation slurry automatically overflows to the next stage reaction device;
[0023] The ripening crystal unit is configured as a 7-stage reaction device, and the overflow slurry of the previous stage undergoes a ripening reaction to obtain rare earth fluorocarbonate ripening slurry.
[0024] Preferably, in the first-stage reaction device, anions (F - +HCO 3 - ) of the composite precipitation solution A and the cation RE 3+ The relative molar ratio of the soluble rare earth salt solution B is (0.23-2.56):1; in the 2-4 stage reaction device, the total amount of anions (F - +HCO 3 - ) of the composite precipitation solution A and the total cation RE 3+ The molar ratio of the soluble rare earth salt solution B is (0.44~2.77):1.
[0025] Preferably, the endpoint of the complete precipitation reaction is controlled at a pH value of 6.2 to 8.0.
[0026] The present invention also provides large-particle rare earth fluoride carbonate and nano-spherical silicon dioxide prepared according to the above method.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] (1) The present invention avoids the problems of the traditional liquid phase preparation of rare earth fluoride carbonate fluoride crystal form being controlled by the front end, uneven fluorination, and low fluorination rate and the presence of free fluorine caused by physical and mechanical methods. The liquid phase continuous parallel flow precipitation technology is adopted to divide the entire precipitation process into four units according to the reaction mechanism: induced nucleation, dielectric growth, complete precipitation and ripening crystallization. Further, with the help of process kinetic control, the rare earth fluoride carbonate crystal form is intact, the particles are large, and the fluorination efficiency is high.
[0029] (2) The present invention avoids the problem of the traditional two-step synthesis method that impurities in the fluorocarbonate rare earth are inherited by the front-end product. According to the difference in solubility product between high-valent rare earth and low-valent conventional impurity fluoride under acidic conditions, the process pH value is controlled by a parallel flow method, so that the impurities can be removed simultaneously to obtain high-quality fluorocarbonate rare earth.
[0030] (3) The present invention adopts F - , HCO 3 - and OH - The composite precipitant reacts in liquid phase to introduce OH - It can increase the concentration of liquid alkali in the precipitant and improve the reaction efficiency. - Replacement of part of HCO 3 - , reducing CO 2 Emissions equate to reduced energy consumption and lower wet processing costs.
[0031] (4) The present invention is suitable for high-value utilization of fluorine-silicon mixed waste acid generated in the rare earth and phosphorus chemical industries. The process has the advantages of saving raw material costs, fluorine-silicon wastewater treatment costs, greatly improving continuous production output, and stabilizing product quality. The economic and social benefits are very significant. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0033] Figure 1 It is the process flow chart of Example 1;
[0034] Figure 2 This is a schematic diagram of the continuous precipitation reaction process of Example 1;
[0035] Figure 3 In the embodiment, (a) is SiO prepared in step (1) of Example 1. 2(b) is an electron microscope image of a solid, and (b) is an electron microscope image of lanthanum cerium fluorocarbonate prepared in step (4) of Example 1. DETAILED DESCRIPTION
[0036] Now, various exemplary embodiments of the present invention are described in detail, and this detailed description should not be considered as a limitation of the present invention, but should be understood as a more detailed description of certain aspects, characteristics and embodiments of the present invention. It should be understood that the terms described in the present invention are only for describing specific embodiments and are not used to limit the present invention.
[0037] In addition, for the numerical range in the present invention, it is understood that each intermediate value between the upper and lower limits of the range is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0038] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0039] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.
[0040] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0041] In the following examples, room temperature refers to 25 to 35°C. 10 "D" is the accumulation of a sample, which refers to the particle size value corresponding to the cumulative distribution percentage from small to large in the particle size distribution reaching 10%. Its physical meaning is that the particles with a particle size smaller than it account for 10%. 50 " is the median diameter or median particle size, which indicates the particle size corresponding to when the cumulative particle size distribution percentage of a sample reaches 50%. Its physical meaning is that particles with a particle size larger than it account for 50%, and particles with a particle size smaller than it also account for 50%. "D 90" is the accumulation of a sample, which refers to the particle size value corresponding to when the cumulative distribution percentage from small to large reaches 90% in the particle size distribution. Its physical meaning is that particles with a particle size smaller than it account for 90%. "Primary particle size" refers to the particle size of a single fine grain.
[0042] In the present invention, the conversion rate of fluorine = (in terms of F - The number of moles of rare earth fluoride carbonate is calculated as F - The molar number of fluorosilicic acid mixed acid) × 100%.
[0043] The method of the present invention comprises the following steps: (1) a silicon removal step; (2) a compound precipitation agent step; (3) a continuous co-current precipitation step; and (4) a solid-liquid separation step. The method is described in detail below.
[0044] Silicon removal steps
[0045] The fluorine-silicon mixed waste acid is added dropwise to the ammonia solution, the reaction solution is stirred, and the pH value of the solution is controlled to be 7.2-9.5, preferably 7.5-9.3, and more preferably 7.8-9.0. The reaction solution is subjected to solid-liquid separation to obtain an alkaline fluorine-containing solution and nano-spherical silica. The present invention adopts a reverse hydrolysis method of adding the fluorine-silicon mixed waste acid dropwise to the ammonia solution, and the intermediate product SiF 6 2- Under strong alkaline conditions, condensation reaction is likely to occur, slowing down the hydrolysis rate, and the generated nano-SiO 2 The grains are spherical and the nuclei are uniform.
[0046] In the present invention, the fluorine-silicon mixed waste acid can be selected from waste acid containing fluorine silicic acid or waste acid containing hydrofluoric acid and fluorine silicic acid. Preferably, the fluorine-silicon mixed waste acid is selected from a mixed acid containing hydrofluoric acid and fluorine silicic acid. More preferably, the fluorine-silicon mixed waste acid is selected from a mixed acid containing hydrofluoric acid and fluorine silicic acid with a fluorine-silicon mass ratio of 1:0.08 to 0.20.
[0047] Steps for preparing the precipitant
[0048] The alkaline fluorine-containing solution is compounded with a monobasic alkaline mixed solution to obtain a composite precipitation solution A.
[0049] The monobasic alkaline mixed solution in the present invention can be selected from a mixed solution of carbonate and alkali solution, the carbonate is selected from at least one of ammonium bicarbonate, ammonium carbonate, sodium bicarbonate, sodium carbonate liquid or solid; the alkali solution is selected from at least one of ammonia water or sodium hydroxide liquid. The molar ratio of carbonate to alkali solution can be selected from (5.67-0.82):1, preferably (4.0-1.0):1, and more preferably (2.33-1.50):1. Compared with the traditional single carbonate precipitant, the present invention introduces OH - It can increase the concentration of liquid alkali in the precipitant and improve the reaction efficiency; at the same time, OH - Replacement of part of HCO3 - , reducing CO 2 Emissions due to CO 2 The emission process will take away heat energy and reduce CO 2 Emissions are equivalent to reducing energy consumption, lowering wet processing costs, and achieving the environmental protection significance of energy saving and carbon reduction.
[0050] In the present invention, F - The alkaline fluoride solution and HCO 3 - The molar ratio of the alkaline mixed solution can be selected from (0.267-1):1, preferably (0.355-0.800):1, and more preferably (0.373-0.711):1. Controlling the fluorine quality within this range is beneficial to the stability of fluorine in the back-end roasting process and avoiding the volatilization of fluorine-containing gas.
[0051] Continuous co-current precipitation step
[0052] The composite precipitation solution A and the soluble rare earth salt solution B are continuously added to the continuous precipitation reaction device for reaction. The entire continuous precipitation is divided into four units: an induced nucleation unit, a dielectric growth unit, a control end point unit, and a mature crystal form. Each unit is fed from the bottom of the reaction device and is precisely controlled by different control conditions. In the present invention, the temperature of the entire continuous precipitation process can be selected from room temperature to 80°C, preferably 30 to 78°C, and more preferably 45 to 75°C. Temperature control in this range is conducive to increasing the critical radius of grain nucleation and increasing the generation rate of grains, thereby growing grains. However, the temperature is not easy to be too high, and carbonates are easily decomposed by heat, resulting in excessive molecular kinetic energy in the system, making the crystallization process unstable. The reaction time of each unit can be selected from ≥30min, preferably ≥40min, and more preferably ≥45min.
[0053] The soluble rare earth salt solution of the present invention is an aqueous solution containing a soluble rare earth salt. The soluble rare earth salt is selected from one of rare earth chlorides, rare earth sulfates, rare earth nitrates and rare earth acetates. The rare earth metal in the soluble rare earth salt can be selected from one or more of lanthanum, cerium, praseodymium, neodymium and samarium. Of course, the rare earth metal in the soluble rare earth salt is not limited to these, as long as it can form an aqueous solution.
[0054] The induced nucleation unit is set as a first-stage reaction device, and the composite precipitation solution A and the soluble rare earth salt solution B are added to the first-stage reaction device in parallel to carry out a rare earth fluoride carbonate induced nucleation reaction, and the obtained crystal nucleus slurry automatically overflows to the next-stage reaction device. - +HCO 3 - ) of the composite precipitation solution A and the cation RE 3+The relative molar ratio of the soluble rare earth salt solution B can be selected from (0.23-2.56):1, preferably (0.30-2.25):1, and more preferably (0.33-2.07):1. It should be noted that, since the solubility product of rare earth fluoride is much smaller than that of rare earth carbonate, part of the rare earth carbonate nuclei are replaced by fluorine in the co-current dripping process to induce the formation of fluorocarbonate rare earth nuclei, thereby avoiding the generation of amorphous nuclei of rare earth fluoride. At the same time, the nucleation of particles is regulated by the instantaneous concentration of the co-current dripping of the rare earth salt solution and the composite precipitation solution. Due to the low instantaneous concentration, the probability of ion collision in the crystallization process is reduced, the nucleation growth time is prolonged, thereby promoting the growth of the nucleus, and the lower reaction concentration greatly reduces the pH fluctuation in the reaction process, providing a stable nucleation environment.
[0055] The dielectric growth unit is set as a 2-4 stage reaction device, and the composite precipitation solution A is added to the 2-4 stage reaction device to perform a dielectric growth reaction of the fluorocarbonate rare earth crystal nucleus, and the resulting growth slurry automatically overflows to the next stage reaction device. - +HCO 3 - ) of the composite precipitation solution A accounts for the total cation RE 3+ The molar ratio of the soluble rare earth salt solution B can be selected from (0.44-2.77):1, preferably (0.75-2.70):1, and more preferably (0.93-2.67):1. It should be noted that the ammonium salt or sodium salt reaction system leads to an increase in the Zeta potential of the fluorocarbonate rare earth particles, and the ammonium cations or sodium cations squeeze into the adsorption layer, and the repulsive barrier of the crystal particles is reduced. At the same time, the OH in the system - It is easy to form hydrogen bond bridging effects such as N···H···N and N···H···F with the N atoms in the adsorption layer and the F atoms in the particles, further promoting the nucleation and growth of the grains.
[0056] The control endpoint unit is set as a 5-6 stage reaction device, equipped with an online detection pH meter, a monobasic mixed solution and / or a 1-stage seed slurry is added to the 5-6 stage reaction device to carry out a rare earth complete precipitation reaction, and the obtained complete precipitation slurry automatically overflows to the next stage reaction device. The pH value of the complete precipitation reaction endpoint in the present invention can be selected from 6.2 to 8.0, preferably 6.3 to 7.5, and more preferably 6.4 to 7.2. The use of a monobasic mixed solution to control the reaction endpoint ensures the complete precipitation of rare earth resources, even if it contains trace amounts of rare earth hydroxide, it can be used as a rare earth polishing powder material, and the wastewater does not contain F elements. It should be further explained that adding the 1-stage seed slurry to the 5-stage reaction device can allow the particle crystallization process to be carried out at a lower supersaturation, further ensuring the growth of crystals.
[0057] The ripening crystal unit is set as a 7-stage reaction device, and the overflow slurry of the previous stage undergoes a ripening reaction to obtain a fluorocarbonate rare earth ripening slurry. It should be noted that the agitator type of the ripening crystal unit device is different from that of the previous unit. A rake type, anchor type, and other agitators can be selected, and the shear force generated is moderate, which can evenly disperse the solid particles in the liquid and maintain their suspension state, which is conducive to the ripening and refined growth of the particles.
[0058] Solid-liquid separation step
[0059] The matured slurry is subjected to solid-liquid separation, and the solid-liquid separation process includes: filtering the matured slurry to obtain a filter cake and a filtrate, the filtrate is an ammonium salt aqueous solution or a sodium salt aqueous solution, and the filter cake is a large particle rare earth fluorocarbonate. In the present invention, since the large particle rare earth fluorocarbonate slurry is easy to filter, the filtering method is not particularly limited. For example, a vacuum filter is used to filter to obtain a filter cake and a filtrate. The filter cake is eluted or washed to directly obtain large particles of rare earth fluorocarbonate.
[0060] Example 1
[0061] The method for continuously preparing large-particle rare earth fluoride carbonate and co-producing nano-spherical silicon dioxide by using fluorine-silicon mixed waste acid is as follows:
[0062] (1) Silicon removal with fluorine-silicon mixed waste acid: Under room temperature, fluorine-silicon mixed waste acid (F: 92.24 g / L, Si: 7.81 wt%) was added dropwise to an analytically pure 28% ammonia solution and stirred until the solution pH reached 9.0. The alkaline fluorine-containing solution (F: 75.46 g / L, SiO 2 <0.01g / L), the filter cake is SiO 2 Solid (particle size D 50 =194.6nm, (D 90 -D 10 ) / D 50 =1.3).
[0063] (2) Prepare 3M composite precipitation solution (nF - :nHCO 3 - =0.3, nNH 4 HCO 3 :nNH 4 OH=6:4): Under stirring at room temperature, 1.5L of alkaline fluorine-containing solution was mixed with 7.1L of alkaline mixed solution (1.57Kg of ammonium bicarbonate and 995mL of 28wt% ammonia water were dissolved in deionized water and fixed to 7.1L) to form a composite precipitation solution.
[0064] (3) Continuous parallel flow liquid phase precipitation reaction: The reaction temperature of stage 1-7 is controlled at 60°C, and the lanthanum cerium chloride solution ( Figure 2Labeled as "Solution B") (C REO :266.58g / L) and composite precipitation solution ( Figure 2 The composite precipitation solution was fed from the bottom of the first-stage device at a rate of 83 mL / min for the lanthanum chloride cerium solution and 43.7 mL / min for the composite precipitation solution. The reaction slurry was stirred for 1 h and then overflowed to the second-stage reaction. The composite precipitation solution was fed from the bottom of the 2-4-stage device at rates of 43.7 mL / min, 22.0 mL / min, and 22.0 mL / min, respectively. The reaction slurry was stirred and then overflowed to the next-stage reaction. The alkaline mixed solution and the first-stage reaction slurry (in Figure 2 The slurry (marked as "seed crystal") was fed from the bottom of the 5-6 stage device at 20 mL / min, and the reaction was stirred until the pH reached 6.8, and the feeding was stopped. The slurry finally overflowed to the seventh stage; the seventh stage slurry was subjected to a maturation reaction (stirring and aging), and the final matured slurry was obtained after 1 hour.
[0065] (4) Solid-liquid separation: The mature slurry obtained in step (3) is subjected to vacuum filtration to obtain ammonium chloride wastewater and filter cake, and the filter cake is repeatedly washed with water to obtain lanthanum cerium fluorocarbonate (particle size D 50 =50.51μm, (D 90 -D 10 ) / D 50 =1.2, fluorine conversion =99.8%).
[0066] Figure 1 It is the process flow chart of this embodiment; Figure 2 This is a schematic diagram of the continuous parallel flow liquid phase precipitation reaction process in step (3) of this embodiment; Figure 3 (a) SiO prepared in step (1) 2 (a) is an electron microscope image of the solid, and (b) is an electron microscope image of the cerium lanthanum fluorocarbonate prepared in step (4). Figure 3 It can be seen that the SiO prepared by the present invention 2 The morphology is nano-spherical particle agglomerates, while the morphology of lanthanum cerium fluorocarbonate is large particle flake agglomerates.
[0067] Example 2
[0068] The method for continuously preparing large-particle rare earth fluoride carbonate and co-producing nano-spherical silicon dioxide by using fluorine-silicon mixed waste acid is as follows:
[0069] (1) Silicon removal with fluorine-silicon mixed waste acid: Under room temperature, fluorine-silicon mixed waste acid (F: 105.2 g / L, Si: 6.44 wt%) was added dropwise to an analytically pure 28% ammonia solution and stirred until the solution pH reached 8.7. The alkaline fluorine-containing solution (F: 89.42 g / L, SiO 2 <0.01g / L), the filter cake is SiO 2 Solid (particle size D50 =187.2nm, (D 90 -D 10 ) / D 50 =1.3).
[0070] (2) Prepare 3M composite precipitation solution (nF - :nHCO 3 - =0.4, nNaHCO 3 :nNaOH=6:4): Under stirring at room temperature, 1.5L of alkaline fluorine-containing solution was mixed with 6.7L of alkaline mixed solution (1.48Kg of sodium bicarbonate and 0.47Kg of sodium hydroxide) to form a composite precipitation solution.
[0071] (3) Continuous parallel flow liquid phase precipitation reaction: The reaction temperature of stage 1-7 is controlled at 60°C, and the cerium lanthanum chloride solution (C REO : 266.58g / L) and the composite precipitation solution are fed from the bottom of the 1st stage device, the feeding rate of lanthanum chloride cerium solution is 83mL / min, and the feeding rate of the composite precipitation solution is 43.7mL / min. After stirring for 1h, the reaction slurry overflows to the 2nd stage reaction; the composite precipitation solution is fed from the bottom of the 2nd-4th stage device, and the feeding rates are 43.7mL / min, 26.0mL / min, and 17.5mL / min, respectively, and the stirring reaction slurry overflows to the next stage reaction; the alkaline mixed solution and the 1st stage reaction slurry are both fed from the bottom of the 5th-6th stage device at 20mL / min, and the stirring reaction is stopped when the pH is 6.8, and the slurry finally overflows to the seventh stage; the seventh stage slurry is subjected to a slaking reaction, and the final slaking slurry is obtained after 1h.
[0072] (4) Solid-liquid separation: The mature slurry obtained in step (3) is subjected to vacuum filtration to obtain sodium chloride wastewater and filter cake, and the filter cake is repeatedly washed with water to obtain lanthanum cerium fluorocarbonate (particle size D 50 =40.42μm, (D 90 -D 10 ) / D 50 =1.5, fluorine conversion =99.9%).
[0073] Example 3
[0074] The method for continuously preparing large-particle rare earth fluoride carbonate and co-producing nano-spherical silicon dioxide by using fluorine-silicon mixed waste acid is as follows:
[0075] (1) Silicon removal with fluorine-silicon mixed waste acid: Under room temperature, fluorine-silicon mixed waste acid (F: 105.2 g / L, Si: 6.44 wt%) was added dropwise to an analytically pure 28% ammonia solution and stirred until the solution pH reached 8.7. The alkaline fluorine-containing solution (F: 89.42 g / L, SiO 2 <0.01g / L), the filter cake is SiO2 Solid (particle size D 50 =192.5nm, (D 90 -D 10 ) / D 50 =1.3).
[0076] (2) Prepare 3M composite precipitation solution (nF - :nHCO 3 - =0.55, nNH 4 HCO 3 :nNH 4 OH=7:3): Under stirring at room temperature, 2L of alkaline fluorine-containing solution was mixed with 6.8L of alkaline mixed solution (1.35Kg of ammonium bicarbonate and 551mL of 28wt% ammonia water were dissolved in deionized water and fixed to 6.8L) to form a composite precipitation solution.
[0077] (3) Continuous parallel flow liquid phase precipitation reaction: The reaction temperature of stage 1-7 is controlled at 60°C, and the praseodymium-neodymium chloride solution (C REO : 271g / L) and the composite precipitation solution are fed from the bottom of the 1st stage device, the feeding rate of the praseodymium-neodymium chloride solution is 25mL / min, and the feeding rate of the composite precipitation solution is 10.8mL / min. The reaction slurry is stirred for 1h20min and overflows to the 2nd stage reaction; the composite precipitation solution is fed from the bottom of the 2nd-4th stage device, and the feeding rates are 10.8mL / min, 8.1mL / min, and 2.7mL / min, respectively, and the reaction slurry is stirred and overflows to the next stage reaction; the alkaline mixed solution and the 1st stage reaction slurry are both fed from the bottom of the 5th-6th stage device at 5mL / min, and the reaction is stirred until the pH is 6.8 and the feeding is stopped, and the slurry finally overflows to the seventh stage; the seventh stage slurry is subjected to a slaking reaction, and the final slaking slurry is obtained after 1h.
[0078] (4) Solid-liquid separation: The mature slurry obtained in step (3) is subjected to vacuum filtration to obtain ammonium chloride wastewater and filter cake, and the filter cake is repeatedly washed with water to obtain praseodymium-neodymium fluorocarbonate (particle size D 50 =28.92μm, (D 90 -D 10 ) / D 50 =1.5, fluorine conversion =99.8%).
[0079] Example 4
[0080] The method for continuously preparing large-particle rare earth fluoride carbonate and co-producing nano-spherical silicon dioxide by using fluorine-silicon mixed waste acid is as follows:
[0081] (1) Silicon removal with fluorine-silicon mixed waste acid: Under room temperature, fluorine-silicon mixed waste acid (F: 113.6 g / L, Si: 7.33 wt%) was added dropwise to an analytically pure 28% ammonia solution and stirred until the solution pH reached 9.0. The alkaline fluorine-containing solution (F: 97.2 g / L, SiO 2 <0.01g / L), the filter cake is SiO 2 Solid (particle size D 50 =187.3nm, (D 90 -D 10 ) / D 50 =1.4).
[0082] (2) Prepare 3M composite precipitation solution (nF - :nHCO 3 - =0.26, nNH 4 HCO 3 :nNH 4 OH=7:3): Under stirring at room temperature, 1L of alkaline fluorine-containing solution was mixed with 7.3L of alkaline mixed solution (1.55Kg of ammonium bicarbonate and 634mL of 28wt% ammonia water were dissolved in deionized water and fixed to 7.3L) to form a composite precipitation solution.
[0083] (3) Continuous parallel flow liquid phase precipitation reaction: The reaction temperature of stage 1-7 is controlled at 65°C, and the samarium chloride solution (C REO : 271g / L) and the composite precipitation solution are fed from the bottom of the 1st stage device, the feeding rate of the samarium chloride solution is 25mL / min, and the feeding rate of the composite precipitation solution is 14.6mL / min. The reaction slurry is stirred for 1h20min and overflows to the 2nd stage reaction; the composite precipitation solution is fed from the bottom of the 2nd-4th stage device, and the feeding rates are 13.0mL / min, 11.4mL / min, and 9.7mL / min, respectively, and the stirring reaction slurry overflows to the next stage reaction; the alkaline mixed solution and the 1st stage reaction slurry are both fed from the bottom of the 5th-6th stage device at 8mL / min, and the stirring reaction is stopped when the pH is 6.8, and the slurry finally overflows to the seventh stage; the seventh stage slurry is subjected to a slaking reaction, and the final slaking slurry is obtained after 1h.
[0084] (4) Solid-liquid separation: The mature slurry obtained in step (3) is subjected to vacuum filtration to obtain ammonium chloride wastewater and filter cake, and the filter cake is repeatedly washed with water to obtain samarium fluorocarbonate (particle size D 50 =22.32μm, (D 90 -D 10 ) / D 50 =1.5, fluorine conversion =99.7%).
[0085] Example 5
[0086] The method for continuously preparing large-particle rare earth fluoride carbonate and co-producing nano-spherical silicon dioxide by using fluorine-silicon mixed waste acid is as follows:
[0087] (1) Silicon removal with fluorine-silicon mixed waste acid: Under room temperature, fluorine-silicon mixed waste acid (F: 128.0 g / L, Si: 7.26 wt%) was added dropwise to an analytically pure 28% ammonia solution and stirred until the solution pH reached 8.7. The alkaline fluorine-containing solution (F: 101.3 g / L, SiO 2 <0.01g / L), the filter cake is SiO 2 Solid (particle size D 50 =164.8nm, (D 90 -D 10 ) / D 50 =1.3).
[0088] (2) Prepare 3.5M composite precipitation solution (nF - :nHCO 3 - =0.85, nNH 4 HCO 3 :nNH 4 OH=7:3): Under stirring at room temperature, 2L of alkaline fluorine-containing solution was mixed with 4.6L of alkaline mixed solution (1.62Kg of ammonium bicarbonate and 659.4mL of 28wt% ammonia water were dissolved in deionized water and fixed to 4.6L) to form a composite precipitation solution.
[0089] (3) Continuous parallel flow liquid phase precipitation reaction: The reaction temperature of stage 1-7 is controlled at 70°C, and the lanthanum cerium nitrate solution (C REO : 283.5g / L) and the composite precipitation solution are fed from the bottom of the 1st stage device, the feeding rate of lanthanum cerium nitrate solution is 20.8mL / min, and the feeding rate of the composite precipitation solution is 8.0mL / min. After stirring for 2h, the reaction slurry overflows to the 2nd stage reaction; the composite precipitation solution is fed from the bottom of the 2nd-4th stage device, and the feeding rates are 8.0mL / min, 8.0mL / min, and 6.0mL / min, respectively, and the stirring reaction slurry overflows to the next stage reaction; the alkaline mixed solution and the 1st stage reaction slurry are both fed from the bottom of the 5th-6th stage device at 5mL / min, and the reaction is stirred until the pH is 6.8 and the feeding is stopped. The slurry finally overflows to the seventh stage; the seventh stage slurry is subjected to a slaking reaction, and the final slaking slurry is obtained after 2h.
[0090] (4) Solid-liquid separation: The mature slurry obtained in step (3) is subjected to vacuum filtration to obtain ammonium nitrate wastewater and filter cake, and the filter cake is repeatedly washed with water to obtain lanthanum cerium fluorocarbonate (particle size D 50 =27.31μm, (D 90 -D 10 ) / D 50=1.5, fluorine conversion =99.8%).
[0091] Example 6
[0092] The method for continuously preparing large-particle rare earth fluoride carbonate and co-producing nano-spherical silicon dioxide by using fluorine-silicon mixed waste acid is as follows:
[0093] (1) Silicon removal with fluorine-silicon mixed waste acid: Under room temperature, fluorine-silicon mixed waste acid (F: 128.0 g / L, Si: 7.26 wt%) was added dropwise to an analytically pure 28% ammonia solution and stirred until the solution pH reached 8.7. The alkaline fluorine-containing solution (F: 101.3 g / L, SiO 2 <0.01g / L), the filter cake is SiO 2 Solid (particle size D 50 =178.3nm, (D 90 -D 10 ) / D 50 =1.5).
[0094] (2) Prepare 3M composite precipitation solution (nF - :nHCO 3 - =0.6, nNH 4 HCO 3 :nNH 4 OH=7:3): Under stirring at room temperature, 1L of alkaline fluorine-containing solution was mixed with 3.7L of alkaline mixed solution (0.702Kg of ammonium bicarbonate and 286mL of 28wt% ammonia water were dissolved in deionized water and fixed to 3.7L) to form a composite precipitation solution.
[0095] (3) Continuous parallel flow liquid phase precipitation reaction: The reaction temperature of stage 1-7 is controlled at 70°C, and the cerium sulfate solution (C REO : 28.2g / L) and the composite precipitation solution are fed from the bottom of the 1st stage device, the feeding rate of the cerium sulfate solution is 100mL / min, and the feeding rate of the composite precipitation solution is 6.55mL / min. The reaction slurry is stirred for 40min and overflows to the 2nd stage reaction; the composite precipitation solution is fed from the bottom of the 2nd-4th stage device, and the feeding rates are 4.4mL / min, 3.3mL / min, and 2.2mL / min, respectively, and the stirring reaction slurry overflows to the next stage reaction; the alkaline mixed solution and the 1st stage reaction slurry are both fed from the bottom of the 5th-6th stage device at 3mL / min, and the stirring reaction is stopped when the pH is 6.8, and the slurry finally overflows to the seventh stage; the seventh stage slurry is subjected to a slaking reaction, and the final slaking slurry is obtained after 1h.
[0096] (4) Solid-liquid separation: The mature slurry obtained in step (3) is subjected to vacuum filtration to obtain ammonium sulfate wastewater and filter cake, and the filter cake is repeatedly washed with water to obtain cerium fluorocarbonate (particle size D50 =33.12μm, (D 90 -D 10 ) / D 50 =1.4, fluorine conversion =99.8%).
[0097] Example 7
[0098] The method for continuously preparing large-particle rare earth fluoride carbonate and co-producing nano-spherical silicon dioxide by using fluorine-silicon mixed waste acid is as follows:
[0099] (1) Silicon removal with fluorine-silicon mixed waste acid: Under room temperature, fluorine-silicon mixed waste acid (F: 128.0 g / L, Si: 7.26 wt%) was added dropwise to an analytically pure 28% ammonia solution and stirred until the solution pH reached 8.7. The alkaline fluorine-containing solution (F: 101.3 g / L, SiO 2 <0.01g / L), the filter cake is SiO 2 Solid (particle size D 50 =176.8nm, (D 90 -D 10 ) / D 50 =1.5).
[0100] (2) Prepare 2.5M composite precipitation solution (nF - :nHCO 3 - =0.5, nNH 4 HCO 3 :nNH 4 OH=7:3): Under stirring at room temperature, 1L of alkaline fluorine-containing solution was mixed with 5.4L of alkaline mixed solution (0.842Kg of ammonium bicarbonate and 344mL of 28wt% ammonia water were dissolved in deionized water and fixed to 5.4L) to form a composite precipitation solution.
[0101] (3) Continuous parallel flow liquid phase precipitation reaction: The reaction temperature of stage 1-7 is controlled at 70°C, and the lanthanum acetate solution (C REO : 294g / L) and the composite precipitation solution are fed from the bottom of the 1st stage device, the feeding rate of lanthanum acetate solution is 20mL / min, and the feeding rate of the composite precipitation solution is 21.6mL / min. The reaction slurry is stirred for 1h40min and overflows to the 2nd stage reaction; the composite precipitation solution is fed from the bottom of the 2nd-4th stage device, and the feeding rates are 11.5mL / min, 5.8mL / min, and 4.3mL / min, respectively, and the stirring reaction slurry overflows to the next stage reaction; the alkaline mixed solution and the 1st stage reaction slurry are both fed from the bottom of the 5th-6th stage device at 10mL / min, and the stirring reaction is stopped when the pH is 6.8, and the slurry finally overflows to the seventh stage; the seventh stage slurry is subjected to a slaking reaction, and the final slaking slurry is obtained after 1h.
[0102] (4) Solid-liquid separation: The mature slurry obtained in step (3) is subjected to vacuum filtration to obtain ammonium acetate wastewater and filter cake, and the filter cake is repeatedly washed with water to obtain lanthanum fluorocarbonate (particle size D 50 =35.78μm, (D 90 -D 10 ) / D 50 =1.5, fluorine conversion =99.8%).
[0103] Example 8
[0104] The method for continuously preparing large-particle rare earth fluoride carbonate and co-producing nano-spherical silicon dioxide by using fluorine-silicon mixed waste acid is as follows:
[0105] (1) Silicon removal with fluorine-silicon mixed waste acid: At room temperature, 30 wt% fluorosilicic acid was added dropwise to an analytically pure 28% ammonia solution and stirred until the solution pH reached 9.2. The alkaline fluorine-containing solution (F: 231.5 g / L, SiO 2 <0.01g / L), the filter cake is SiO 2 Solid (particle size D 50 =150.3nm, (D 90 -D 10 ) / D 50 =1.3).
[0106] (2) Prepare 3M composite precipitation solution (nF - :nHCO 3 - =1, nNH 4 HCO 3 :nNH 4 OH=7:3): Under stirring at room temperature, 1L of alkaline fluorine-containing solution was mixed with 7.1L of alkaline mixed solution (0.963Kg of ammonium bicarbonate and 393mL of 28wt% ammonia water were dissolved in deionized water and fixed to 7.1L) to form a composite precipitation solution.
[0107] (3) Continuous parallel flow liquid phase precipitation reaction: The reaction temperature of stage 1-7 is controlled at 65°C, and the cerium chloride solution (C REO: 285.6g / L) and the composite precipitation solution are fed from the bottom of the 1st stage device, the feeding rate of the cerium chloride solution is 25mL / min, the feeding rate of the composite precipitation solution is 13.8mL / min, and the reaction slurry is stirred for 1h40min and overflows to the 2nd stage reaction; the composite precipitation solution is fed from the bottom of the 2nd-4th stage device, and the feeding rates are 13.8mL / min, 6.9mL / min, and 6.9mL / min, respectively, and the stirring reaction slurry overflows to the next stage reaction; the alkaline mixed solution and the 1st stage reaction slurry are both fed from the bottom of the 5th-6th stage device at 8mL / min, and the stirring reaction is stopped when the pH is 6.8, and the slurry finally overflows to the seventh stage; the seventh stage slurry is subjected to a slaking reaction, and the final slaking slurry is obtained after 1h.
[0108] (4) Solid-liquid separation: The mature slurry obtained in step (3) is subjected to vacuum filtration to obtain ammonium chloride wastewater and filter cake, and the filter cake is repeatedly washed with water to obtain cerium fluorocarbonate (particle size D 50 =29.32μm, (D 90 -D 10 ) / D 50 =1.5, fluorine conversion =99.8%).
[0109] Example 9
[0110] The types and concentrations of the raw materials are the same as those in Example 1, and the steps of step (1) removing silicon from the fluorine-silicon mixed waste acid, step (2) preparing the 3M composite precipitation solution, and step (4) solid-liquid separation are the same. The difference is step (3). In this embodiment, step (3) is: continuous parallel flow liquid phase precipitation reaction: the reaction temperature of the 1-7 stages is controlled at 60°C, and the cerium chloride solution (C REO :266.58g / L) and composite precipitation solution are fed from the bottom of the first-stage device, the feeding rate of lanthanum chloride cerium solution is 83mL / min, the feeding rate of composite precipitation solution is 43.7mL / min, and the reaction slurry overflows to the second-stage reaction after stirring for 1h; the composite precipitation solution is fed from the bottom of the 2-4-stage device, and the feeding rates are 43.7mL / min, 22.0mL / min, and 22.0mL / min, respectively, and the stirring reaction slurry overflows to the next-stage reaction; the alkaline mixed solution is fed from the bottom of the 5-6-stage device at 20mL / min, and the stirring reaction is stopped until the pH is 6.8, and the slurry finally overflows to the seventh stage; the seventh-stage slurry is subjected to a slaking reaction (standing and aging), and the final slaking slurry is obtained after 1h. That is, in this embodiment, the first-stage reaction slurry is not added to the 5-6-stage device of step (3).
[0111] In this embodiment, the particle size D of the cerium lanthanum fluorocarbonate obtained in step (4) is 50 =14.61μm, (D 90 -D 10 ) / D 50 =1.3, fluorine conversion =99.7%).
[0112] By comparing the results of Example 9 with those of Example 1, it can be seen that the continuous precipitation reaction supplemented with seed slurry to induce precipitation can promote the further growth of the fluorocarbonate rare earth particles.
[0113] Comparative Example 1
[0114] The types and concentrations of the raw materials are the same as those in Example 1, and the steps of (1) removing silicon from the fluorine-silicon mixed waste acid, (2) preparing the 3M composite precipitation solution, and (4) solid-liquid separation are the same, except that step (3) adopts a single-tank precipitation reaction: the reaction temperature is controlled at 60°C, 1.2L of lanthanum cerium chloride solution (C REO : 266.58g / L) and 1.9L composite precipitation solution were added dropwise from the upper part of the reaction tank to the bottom liquid containing 1L deionized water, and the stirring reaction was started. The feeding rate of lanthanum cerium chloride solution was 10mL / min, and the feeding rate of composite precipitation solution was 15.8mL / min. After the feeding was completed, an alkaline mixed solution was added to adjust the pH of the reaction slurry to 6.8, and aged for 1h to obtain the final slurry.
[0115] In this comparative example, the particle size D of the cerium lanthanum fluorocarbonate obtained in step (4) is 50 =4.827μm, (D 90 -D 10 ) / D 50 =2.86, fluorine conversion rate =99.6%.
[0116] Comparative Example 2
[0117] The types and concentrations of the raw materials are the same as those in Example 1, and the steps of (1) removing silicon from the fluorine-silicon mixed waste acid, (2) preparing the 3M composite precipitation solution, and (4) solid-liquid separation are the same, except that step (3) uses a single-pot seed crystal to induce the precipitation reaction: the reaction temperature is controlled at 60°C, 1.2L of lanthanum cerium chloride solution (C REO : 266.58g / L) and 1.9L composite precipitation solution were dripped from the upper part of the reaction tank into the bottom liquid, the bottom liquid was composed of 1L deionized water and 71g lanthanum cerium fluorocarbonate seed crystals, and the stirring reaction was started. The feeding rate of lanthanum cerium chloride solution was 10mL / min, and the feeding rate of composite precipitation solution was 15.8mL / min. After the feeding was completed, an alkaline mixed solution was added to adjust the pH of the reaction slurry to 6.8, and aged for 1h to obtain the final slurry.
[0118] In this comparative example, the particle size D of the cerium lanthanum fluorocarbonate obtained in step (4) is 50 =7.259μm, (D 90 -D 10 ) / D 50 =1.9, fluorine conversion =99.7%).
[0119] By comparing the results of Comparative Example 1 and Example 1, it can be seen that the continuous precipitation reaction solves the problem of small particle size of rare earth fluorocarbonate particles in the single-pot precipitation reaction.
[0120] By comparing the results of Comparative Example 2 and Example 1, it can be seen that the continuous precipitation reaction solves the problem of small particle size of rare earth fluorocarbonate particles in the single-pot seed-induced precipitation reaction.
[0121] The above description is only a preferred specific implementation manner of the present invention, and the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, and they should be covered by the protection scope of the present invention.
Claims
1. A method for continuously preparing large-particle rare earth fluoride carbonate and co-producing nano-spherical silicon dioxide using fluorine-silicon mixed waste acid, characterized in that: The following steps are involved: (1) Removal of silicon from fluorine-silicon mixed waste acid: Mixing the fluorine-silicon mixed waste acid with ammonia water to obtain an alkaline fluorine-containing solution and nano-spherical silica; (2) Compounding the precipitant: compounding the alkaline fluorine-containing solution obtained in step (1) with a monobasic alkaline mixed solution to obtain a composite precipitation solution A; (3) Continuous co-current precipitation: the composite precipitation solution A obtained in step (2) is subjected to a continuous precipitation reaction with the soluble rare earth salt solution B; (4) solid-liquid separation: filtering the mature slurry obtained from the reaction in step (3) to obtain the large particles of rare earth fluorocarbonate; The particle size D of the large particle fluorocarbonate rare earth 50 ≥28μm, particle size range is (D 90 -D 10 ) / D 50 ≤1.5; the primary particle size D of the nano-spherical silica 50 ≤300nm, particle size range is (D 90 -D 10 ) / D 50 ≤1.5; In step (3), the continuous precipitation reaction includes inducing nucleation, dielectric growth, controlling the endpoint and aging crystallization process in sequence.
2. The method according to claim 1, characterized in that In step (1), the fluorine-silicon mixed waste acid is selected from waste acid containing fluorine silicic acid or waste acid containing hydrofluoric acid and fluorine silicic acid, the content of fluorine element in the fluorine-silicon mixed waste acid is 90-250 g / L, and the content of silicon element is 0.5-10 wt %; the pH value of the alkaline fluorine-containing solution obtained by stirring and mixing the fluorine-silicon mixed waste acid with ammonia water is controlled to be 7.2-9.
5.
3. The method according to claim 1, characterized in that In step (2), the monobasic alkaline mixed solution is selected from a mixed solution of carbonate and alkali solution, the carbonate is selected from at least one of ammonium bicarbonate, ammonium carbonate, sodium bicarbonate, sodium carbonate liquid or solid; the alkali solution is selected from at least one of ammonia water or sodium hydroxide solution; - Alkaline fluoride solution and HCO3 - The molar ratio of the monobasic alkaline mixed solution is (0.267~1):
1.
4. The method according to claim 1, characterized in that: In step (3), the soluble rare earth salt solution is selected from one of rare earth chlorides, rare earth sulfates, rare earth nitrates and rare earth acetates, and the temperature of the entire continuous precipitation reaction process is 25 to 80°C.
5. The method according to claim 1, characterized in that In step (3), the continuous precipitation reaction is carried out in a continuous precipitation reaction device, and the composite precipitation solution A and the soluble rare earth salt solution B are continuously added to the continuous precipitation reaction device. The continuous precipitation reaction device is divided into four units, namely, an induced nucleation unit, a dielectric growth unit, an endpoint control unit and a aging crystal form, which respectively carry out the induced nucleation, dielectric growth, endpoint control and aging crystallization processes. The feeding method of each unit is to feed from the bottom of the reaction device, and the reaction time of each unit is ≥30min.
6. The method according to claim 5, characterized in that The induced nucleation unit is set as a first-stage reaction device, and the composite precipitation solution A and the soluble rare earth salt solution B are added to the first-stage reaction device in parallel to carry out a rare earth fluorocarbonate induced nucleation reaction, and the obtained first-stage seed slurry automatically overflows to the next-stage reaction device; The dielectric growth unit is set as a 2-4 stage reaction device, the composite precipitation solution A is added into the 2-4 stage reaction device to carry out dielectric growth reaction of rare earth fluoride carbonate crystal nuclei, and the grown slurry automatically overflows to the next stage reaction device; The control endpoint unit is set as a 5-6 stage reaction device, equipped with an online detection pH meter, a monobasic alkaline mixed solution and / or a 1-stage seed slurry is added to the 5-6 stage reaction device to perform a rare earth complete precipitation reaction, and the obtained complete precipitation slurry automatically overflows to the next stage reaction device; The ripening crystal unit is configured as a 7-stage reaction device, and the overflow slurry of the previous stage undergoes a ripening reaction to obtain rare earth fluorocarbonate ripening slurry.
7. The method according to claim 6, characterized in that In the first-stage reaction device, anions (F - +HCO3 - ) of the composite precipitation solution A and the cation RE 3+ The relative molar ratio of the soluble rare earth salt solution B is (0.23-2.56):1; in the 2-4 stage reaction device, the total amount of anions (F - +HCO3 - ) of the composite precipitation solution A and the total cation RE 3+ The molar ratio of the soluble rare earth salt solution B is (0.44~2.77):
1.
8. The method according to claim 6, characterized in that The endpoint of the complete precipitation reaction is controlled at a pH value of 6.2 to 8.
0.
9. Large-particle rare earth fluorocarbonate and nano-spherical silicon dioxide prepared according to the method according to any one of claims 1 to 8.
Citation Information
Patent Citations
A kind of preparation method of superfine fluorine-containing cerium-based polishing powder
CN104387988B
A method for preparing rare earth fluoride polishing powder and rare earth fluoride polishing liquid
CN110885637B
A system and method for preparing rare earth polishing powder
CN112724839B
Technological method for preparing white carbon black from potassium feldspar
CN103539130A
Preparation method of rare earth polishing powder
CN104017500A