External field polarization defect state bismuth tungstate piezoelectric catalyst and preparation method thereof

By introducing oxygen vacancies defective structures into bismuth tungstate and polarizing under an external electric field, combined with surface defect engineering and external electric field polarization, the problems of low carrier concentration and poor piezoelectric performance of traditional ferroelectric materials are solved, and the problem of low carrier concentration and poor piezoelectric performance of traditional ferroelectric materials is achieved. The high carrier concentration and high voltage electrical performance are taken into account, and the piezoelectric catalytic activity and the efficiency of hydrogen production in decomposition are significantly improved.

CN118993151APending Publication Date: 2024-11-22CHINA JILIANG UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411069574.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-06
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

When traditional ferroelectric materials increase carrier concentration, they are prone to enhance the charge shielding effect, hinder polarization reversal behavior, affect piezoelectric performance, and it is difficult to take into account both high carrier concentration and high voltage electrical coefficient.

Method used

The oxygen vacancies defective structure is introduced into bismuth tungstate by solvent thermal reduction method, and defective bismuth tungstate piezoelectric catalyst containing oxygen vacancies is prepared, and polarized under an external electric field to form polarization with consistent defective dipole orientation. Bismuth tungstate piezoelectric catalyst, a modification method combining surface defect engineering and external electric field polarization.

Benefits of technology

It significantly improves carrier concentration and piezoelectric performance, improves piezoelectric catalytic activity, solves the problem of low carrier concentration and high piezoelectric performance deviation of carrier materials, and realizes efficient piezoelectric catalytic decomposition of water to make hydrogen active.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993151A_ABST
    Figure CN118993151A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of hydrogen production through piezoelectric catalytic decomposition of water, and particularly relates to an external field polarization defect state bismuth tungstate piezoelectric catalyst and a preparation method thereof. The invention provides an external field polarization defect state bismuth tungstate piezoelectric catalyst and a preparation method thereof, and is characterized in that the defect state bismuth tungstate piezoelectric catalyst has a large number of oxygen vacancy defect state structures, and the particle size is 4-20nm; after an external electric field is applied for polarization, the orientations of defect dipoles are consistent, and the piezoelectric amplitude response is greatly improved. Compared with an unmodified bismuth tungstate piezoelectric catalyst, a defect-state structure of the oxygen vacancy-containing bismuth tungstate can form a carrier capture trap, so that compounding of positive and negative charges is reduced, and separation of the positive and negative charges is promoted; out-field polarization enables the orientation of the defect dipoles to be consistent, forward contribution is generated to the piezoelectric property, and the generation and transport efficiency of carriers is further improved. The invention provides a new thought and a new method for designing and developing a high-performance piezoelectric catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of piezoelectric catalysis, and in particular relates to an external field polarized defective bismuth tungstate piezoelectric catalyst and a preparation method thereof. Background Art

[0002] Hydrogen energy is a green energy with high calorific value, zero carbon emission, abundant sources and wide application. At present, industrial hydrogen production mainly relies on fossil energy and industrial by-products, which is not conducive to sustainable development. Clean hydrogen production technologies mainly include water electrolysis hydrogen production technology, photolysis water hydrogen production technology, biomass hydrogen production technology, etc. However, most water electrolysis hydrogen evolution reactions are carried out in strong acid / strong base electrolytes, requiring expensive anion / cation exchange membranes; photolysis water hydrogen production technology has low overall solar energy conversion efficiency due to slow carrier migration kinetics, strict requirements on lighting conditions and solution transmittance, etc.; biomass hydrogen production has low energy density, unstable raw material supply, and strict requirements on light, pH value, temperature, oxygen concentration, etc. Therefore, it is very necessary to develop a green, clean, efficient and stable water decomposition hydrogen production technology.

[0003] Piezocatalysis is a technology that utilizes the coupling of piezoelectric effect and catalytic reaction. As an emerging field, its unique advantage lies in breaking the barrier between mechanical energy and chemical energy. Compared with traditional light- and electric-driven catalytic methods, piezocatalysis is not limited by the band gap of materials and can utilize vibration energy that can be found everywhere in life, which reduces the cost of energy conversion while reducing dependence on fossil energy. It has the advantages of being clean, sustainable, and environmentally friendly. However, current research focuses on how to improve the piezoelectric properties of materials to obtain higher piezoelectric catalytic activity. Although traditional ferroelectric materials have high piezoelectric coefficients, their internal intrinsic carrier concentration is low, which is not conducive to the generation of free charges in the piezoelectric process, thereby affecting the piezoelectric catalytic activity. Oxygen vacancy engineering is a common method for regulating the electronic structure and material properties of materials, which can be used to increase the carrier concentration of materials. However, blindly increasing the carrier concentration of materials will enhance their charge screening effect and hinder polarization reversal behavior, thereby adversely affecting the piezoelectric properties of materials. Therefore, how to ensure that oxygen vacancies do not damage the piezoelectric properties of the material while increasing the carrier concentration of the material and promoting the separation and transport of positive and negative charge carriers is a key scientific problem that needs to be urgently solved in the field of piezoelectric catalysis.

[0004] Studies have found that electric field polarization of defects to achieve directional rearrangement is an effective way to improve the piezoelectric properties of materials. Park et al. from the Swiss Federal Institute of Technology [Science, 2022, 375, 653-657] doped Gd into CeO2, a two-dimensional thin film oxide with a central symmetric atomic structure, and introduced oxygen vacancies, inducing a large and sustained piezoelectric effect by breaking the crystal symmetry and applying an external electric field to induce oxygen vacancy rearrangement. Li Guorong et al. from the Shanghai Institute of Ceramics, Chinese Academy of Sciences [Journal of Sichuan University: Natural Science Edition, 2005, 42, 25-28] studied the effect of lattice defects on the piezoelectric properties of sodium bismuth titanate piezoelectric ceramics and found that the lattice defect dipoles composed of oxygen vacancies and A-site vacancies are oriented along the direction of the electric field under the action of an external electric field, and the oriented defect dipoles make a positive contribution to the piezoelectric properties. In addition, the pinning effect of defects can limit the migration of ions, making the material less likely to depolarize after polarization. This helps to improve the polarization properties of the material while ensuring a high carrier concentration, which can be used to effectively separate and migrate carriers and improve catalytic activity.

[0005] Bismuth tungstate (Bi2WO6, abbreviated as BWO) is the simplest oxide in the bismuth layer perovskite family, with a bandgap width (E g ) is about 2.75eV. It is a semiconductor material with indirect bandgap transition. Its special layered perovskite structure is conducive to the transport of carriers. At the same time, BWO has good piezoelectric properties. For example, the piezoelectric constant of BWO ceramics is 15pC N -1 The piezoelectric coefficient of BWO single crystal is about 40pC N -1 Compared with other piezoelectric semiconductors such as ZnO (d 33 =22.5pm·V -1 ) has obvious advantages. However, since high carrier concentration and high piezoelectric coefficient cannot be achieved at the same time, the piezoelectric catalytic performance of BWO is not ideal. The present invention proposes a method for improving the piezoelectric catalytic activity of BWO, which is to first introduce a defective structure into the BWO piezoelectric catalyst by a solvent thermal reduction method to prepare a defective bismuth tungstate (Bi2WO) containing oxygen vacancies. 6-x , abbreviated as BWO-OV) piezoelectric catalyst, and then polarize the obtained BWO-OV piezoelectric catalyst under an external electric field to prepare a polarized BWO-OV (BWO-OV-P) piezoelectric catalyst with consistent defect dipole orientation; on this basis, it is expected that the carrier concentration, piezoelectric properties and piezoelectric catalytic activity of the BWO piezoelectric catalyst can be improved to a large extent through the synergy of oxygen vacancy defect state structure and external electric field polarization. Summary of the invention

[0006] The purpose of the present invention is to modify the BWO piezoelectric catalyst by combining surface defect engineering and external electric field polarization, so as to achieve the consistent orientation of the lattice defect dipoles composed of oxygen vacancies and A-site vacancies, produce a positive contribution to the piezoelectric performance, and prepare a BWO-OV-P piezoelectric catalyst with both high carrier concentration and high piezoelectric performance. The present invention first synthesizes a BWO-OV piezoelectric catalyst containing oxygen vacancies by solvent thermal reduction, and then obtains a BWO-OV-P piezoelectric catalyst with consistent defect dipole orientation by external electric field polarization, thereby achieving the modification of the BWO piezoelectric catalyst and improving the carrier concentration and piezoelectric performance of the material, which largely solves the contradiction between the low carrier concentration of traditional ferroelectric materials and the deviation of the piezoelectric performance of high carrier concentration materials, thereby effectively improving the activity of BWO piezoelectric catalytic water decomposition to produce hydrogen.

[0007] The present invention provides an external field polarized defective bismuth tungstate piezoelectric catalyst and a preparation method thereof, which is characterized by being achieved through the following technical solutions:

[0008] (1) First, a defective bismuth tungstate (BWO-OV) piezoelectric catalyst containing oxygen vacancies was synthesized by a solvent thermal reduction method. The specific process is as follows: 0.05-0.07 mol / L sodium tungstate (Na2WO4·2H2O) solution A and bismuth nitrate (Bi(NO3)3·5H2O) solution B were prepared in ethylene glycol, respectively, and then solution A was slowly dripped into solution B according to the molar ratio of W element to Bi element being 1:2, and the solution was placed on a magnetic stirrer and stirred for 1-2 hours at room temperature, and then transferred to a 100 mL stainless steel reactor containing a polytetrafluoroethylene liner, and heated at 160-180°C for 12-20 hours. After the reaction, the precipitate was collected and centrifuged, washed with deionized water or ethanol 2-3 times, and dried at 60°C for 12-24 hours to obtain the BWO-OV piezoelectric catalyst;

[0009] (2) On the premise of obtaining the BWO-OV piezoelectric catalyst, a BWO-OV-P piezoelectric catalyst with uniform defect dipole orientation is obtained by external electric field polarization. The polarization treatment process is specifically as follows: the BWO-OV piezoelectric catalyst powder synthesized in the above step (1) is placed between two copper plates containing needle-tip electrodes, a 3-10 kV corona polarization voltage is applied using a high-voltage DC polarization device, and the voltage is maintained and polarized in air at 25-180° C. for 20-100 min to obtain a BWO-OV-P piezoelectric catalyst with uniform defect dipole orientation.

[0010] Compared with the prior art, the present invention has the following advantages and positive effects:

[0011] The present invention modifies the BWO piezoelectric catalyst by combining surface defect engineering and external electric field polarization to prepare a BWO-OV-P piezoelectric catalyst with high carrier concentration and high piezoelectric performance, which has the advantages of obvious modification effect and low cost. Compared with the modification method of simply improving the carrier concentration of the material, the modification method combining surface defect engineering and external electric field polarization can improve the carrier concentration and piezoelectric performance of the BWO piezoelectric catalyst to a greater extent. This is because on the one hand, the solvent thermal reduction process will produce a large number of defect state structures in the BWO piezoelectric catalyst. These defects can form piezoelectrically induced carrier capture "traps", reduce the recombination of positive and negative charges and promote their separation, and on the other hand, the external electric field polarization can make the lattice defect dipoles composed of oxygen vacancies and A-site vacancies align their orientation, make a positive contribution to the piezoelectric performance, further improve the generation and transport efficiency of piezoelectrically induced carriers, and improve the piezoelectric catalytic activity. At the same time, the pinning effect of defects can limit the migration of ions, making the material less likely to depolarize after polarization, which is beneficial to improving the polarization stability of the material. It is worth noting that the modification method combining surface defect engineering and external electric field polarization proposed in the present invention is also applicable to modifying other piezoelectric materials to simultaneously improve their carrier concentration and piezoelectric properties, thereby ultimately achieving the purpose of significantly improving their piezoelectric catalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] Figure 1 is an X-ray diffraction (XRD) spectrum of the BWO-OV piezoelectric catalyst prepared in Example 1;

[0013] Figure 2 The transmission electron microscope (TEM) image and particle size distribution curve of the BWO-OV piezoelectric catalyst prepared in Example 1;

[0014] Figure 3 Electron paramagnetic resonance (EPR) curves of BWO-OV and BWO piezoelectric catalysts prepared in Example 1;

[0015] Figure 4 Mott-Schottky curves of the BWO-OV and BWO piezoelectric catalysts prepared in Example 1;

[0016] Figure 5 The amplitude response curve of the BWO-OV prepared in Example 1 and the BWO-OV-P piezoelectric catalyst after applying an external electric field to it varies with the bias voltage;

[0017] Figure 6 This is a comparison chart of the piezoelectric catalytic water decomposition and hydrogen production performance of the BWO-OV and BWO piezoelectric catalysts prepared in Example 1 and the BWO-OV-P and BWO-P polarized samples after being polarized by an external electric field. DETAILED DESCRIPTION

[0018] The present invention is not limited to the following specific embodiments. A person skilled in the art can implement the present invention in various other specific embodiments according to the contents disclosed in the present invention, or any simple changes or modifications made to the design structure and ideas of the present invention fall within the protection scope of the present invention. It should be noted that the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict. The present invention is further described in detail below in conjunction with specific embodiments and drawings.

[0019] Embodiment 1:

[0020] (1) First, a defective bismuth tungstate (BWO-OV) piezoelectric catalyst containing oxygen vacancies was synthesized by a solvent thermal reduction method. The specific process is as follows: 0.528 g of sodium tungstate (Na2WO4·2H2O, 1.6 mmol) was dissolved in 24 mL of ethylene glycol solution and stirred for 30 min to form a transparent solution A; 1.552 g of bismuth nitrate (Bi(NO3)3·5H2O, 3.2 mmol) was dissolved in 56 mL of ethylene glycol solution and stirred for 30 min to form a transparent solution B; solution A was slowly dripped into solution B, placed on a magnetic stirrer and stirred for 2 h at room temperature, and then transferred to a 100 mL stainless steel reactor containing a polytetrafluoroethylene liner, heated at 160°C for 20 h, and after the reaction, the precipitate was collected and centrifuged, washed with ethanol three times, and dried at 60°C for 12 h to obtain BWO-OV powder. For comparison, the oxygen vacancy-free bismuth tungstate (BWO) piezoelectric catalyst is obtained by heat treating the above-obtained BWO-OV with oxygen. The specific process is as follows: 1 g of the BWO-OV sample is weighed and placed in a crucible, which is placed in a muffle furnace with an air-rich atmosphere, and annealed at 400°C for 4 hours to obtain BWO powder.

[0021] (2) On the premise of obtaining the above-mentioned BWO-OV piezoelectric catalyst, a polarized BWO-OV (abbreviated as: BWO-OV-P) piezoelectric catalyst with consistent defect dipole orientation is obtained by external electric field polarization. The specific polarization treatment process is as follows: take 1g of BWO-OV sample, place these powder samples between two copper plates with a diameter of 4cm containing needle-tip electrodes, add alcohol to flatten and solidify on the copper plates, and then dry naturally at room temperature; then use a high-voltage DC polarization device to maintain pressure polarization for 40 minutes at a temperature of 25°C and a corona polarization voltage of 10kV to obtain a BWO-OV-P piezoelectric catalyst with consistent defect dipole orientation. Similarly, as a comparison, under the same conditions, the BWO piezoelectric catalyst is polarized by external electric field polarization to obtain a polarized BWO (BWO-P) piezoelectric catalyst.

[0022] The piezoelectric catalytic performance of the above-mentioned oxygen vacancy bismuth tungstate (BWO-OV) and oxygen vacancy-free bismuth tungstate (BWO) piezoelectric catalysts and their external electric field polarized bismuth tungstate samples (BWO-OV-P, BWO-P) prepared by the present invention is tested by using a laboratory-made ultrasonic water decomposition hydrogen production system to test their piezoelectric catalytic water decomposition hydrogen production performance. The specific process and steps are as follows: 13.5 mL of deionized water, 1.5 mL of methanol as a sacrificial agent, and 20 mg of piezoelectric catalyst powder are added to a 36 mL quartz glass bottle, and after ultrasonic dispersion is uniformly dispersed, the quartz glass bottle is continuously heated to 40 °C. The air was expelled by filling with argon for 10 minutes, and then the system was sealed with an airtight soft stopper and an aluminum cap. After that, vibration was applied to it with an ultrasonic machine with a power of 100 W and a frequency of 45 kHz as a vibration source. Ultrasonic treatment was carried out for 2 hours under light-proof conditions. During this period, the system temperature was kept at 25°C by changing the cooling water. After the reaction was completed, a gas injection needle was inserted through the airtight soft stopper to extract 1 mL of gas from the reactor, which was injected into a gas chromatograph and the hydrogen content was detected by a thermal conductivity detector (TCD). The actual hydrogen volume was converted from the known standard curve, and then its piezoelectric catalytic hydrogen production rate was calculated.

[0023] Figure 1 This is the X-ray diffraction (XRD) spectrum of the BWO-OV piezoelectric catalyst prepared in Example 1. As can be seen from the figure, the main diffraction peaks of the sample completely correspond to the orthorhombic bismuth tungstate standard card (JCPDS no.79-2381, space group Pca21, point group mm2), indicating that the main components of the sample are all orthorhombic bismuth tungstate, without other impurities.

[0024] Figure 2 The transmission electron microscope (TEM) image and particle size distribution curve of the BWO-OV piezoelectric catalyst prepared in Example 1. As can be seen from the figure, the BWO-OV sample is in a granular form with a size between 4 and 20 nm and good dispersion.

[0025] Figure 3 The electron paramagnetic resonance (EPR) curves of the bismuth tungstate containing oxygen vacancies (BWO-OV) and the bismuth tungstate without oxygen vacancies (BWO) piezoelectric catalysts prepared in Example 1 are shown in FIG. Figure 3It can be seen that the sample BWO-OV produces a typical Lorentz characteristic absorption peak curve near the magnetic field g = 2.003. The appearance of this absorption characteristic peak is closely related to the number of unpaired electrons of oxygen atoms in the material, confirming the existence of oxygen vacancy defect state structure in BWO-OV; while the oxygen vacancy-free bismuth tungstate (BWO) sample after oxygen heat treatment has no obvious EPR signal, indicating that the BWO-OV sample synthesized by the solvent thermal reduction method has been treated with oxygen-rich high temperature, and the oxygen vacancies in it have been repaired. The EPR results confirm that the solvent thermal reduction synthesis process can produce a large number of oxygen vacancy defect state structures during the formation of bismuth tungstate, and this defect state structure can be repaired in an oxygen-rich atmosphere.

[0026] Figure 4 The Mott-Schottky curves of the piezoelectric catalysts of bismuth tungstate with oxygen vacancies (BWO-OV) and bismuth tungstate without oxygen vacancies (BWO) prepared in Example 1. The carrier concentration (N d ) can be determined by the following formula:

[0027]

[0028] Where e0, ε0, ε represent the charge unit (1.6×10 19 C), vacuum dielectric constant (8.85×10 14 Fm -1 ) and the dielectric constant of the material. Generally speaking, the smaller the slope of the Mott-Schottky curve, the higher the carrier concentration (N d ) is larger. The carrier concentration (N d ) values ​​are 2.90×10 20 cm -3 and 1.97×10 20 cm -3 . In metal oxides, oxygen vacancies are usually positively charged because when an oxygen atom in the crystal lattice leaves, it takes away two electrons that originally belonged to other atoms, forming a positively charged defect. This positively charged defect can attract electrons and increase the electron concentration of the material, thereby increasing the carrier concentration. At the same time, oxygen vacancies introduce additional defect energy levels in the band structure, which can serve as centers for carrier generation or recombination. Under appropriate conditions, these energy levels can act as "traps" for electrons or holes, thereby increasing the carrier concentration of the material.

[0029] Figure 5 The amplitude response curve of the oxygen vacancy bismuth tungstate (BWO-OV) piezoelectric catalyst prepared in Example 1 before and after external electric field polarization is shown as a function of bias voltage. Figure 5It can be seen that the amplitude of the piezoelectric catalyst of the polarized sample (BWO-OV-P) has been greatly improved in response to the bias voltage, and its amplitude value is 10.5 times that of the piezoelectric catalyst of the unpolarized sample (BWO-OV). This is because the external electric field polarization can make the lattice defect dipoles composed of oxygen vacancies and A-site vacancies in BWO-OV align in orientation, which makes a positive contribution to the piezoelectric performance. In addition, the pinning effect of the defects can limit the migration of ions, making it difficult for the material to depolarize after polarization, which is beneficial to improving the polarization stability of the material. It can be seen that the modification method combining oxygen vacancy defects and external field polarization can simultaneously improve the carrier concentration and piezoelectric properties of the material, and to a large extent solves the contradiction between the low carrier concentration of traditional ferroelectric materials and the deviation of piezoelectric properties of high carrier concentration materials, thereby effectively reducing the piezoelectric-induced positive-negative charge recombination and promoting their separation and transport, thereby improving the piezoelectric catalytic activity.

[0030] Figure 6 The piezoelectric catalytic water decomposition hydrogen production performance comparison chart of the oxygen vacancy bismuth tungstate (BWO-OV) and oxygen vacancy-free bismuth tungstate (BWO) piezoelectric catalysts and their polarized samples (BWO-OV-P, BWO-P) prepared in Example 1. From the test results, it can be seen that the rates of water decomposition hydrogen production by BWO-OV, BWO-OV-P, BWO and BWO-P are 65.36, 93.48, 32.18 and 38.56 μmol g –1 h –1 . Obviously, the piezoelectric catalytic activity of the oxygen vacancy-free bismuth tungstate (BWO-P) sample after external electric field polarization is significantly enhanced compared with the unpolarized sample (BWO) (the average hydrogen production rate is increased by 19.8%). This is because after external field polarization, the electric dipoles inside the BWO material are arranged in an orderly manner, and the polarization performance of the material is improved, which is conducive to the separation and transport of carriers, thereby improving the catalytic efficiency. Compared with the unpolarized oxygen vacancy-containing bismuth tungstate (BWO-OV) sample, the piezoelectric catalytic activity of the BWO-OV-P polarized sample is more significantly improved (the average hydrogen production rate is increased by 30.1%). This is because in addition to the orderly arrangement of the electric dipoles inside the BWO-OV material itself, which can contribute to the polarization performance, the lattice defect dipoles composed of oxygen vacancies and A-site vacancies are oriented along the direction of the electric field under the action of the external electric field. The oriented defect dipoles make an additional positive contribution to the piezoelectric performance, further improving the polarization performance of the sample, which is used to effectively separate and migrate carriers, thereby improving the catalytic activity to a greater extent.

Claims

1. An external field polarized defective bismuth tungstate piezoelectric catalyst, characterized in that: The defective bismuth tungstate piezoelectric catalyst has a large number of oxygen vacancy defect structures, and its particle size is between 4 and 20 nm; after applying an external electric field for polarization, its defect dipoles are oriented in the same direction, and the piezoelectric amplitude response is greatly improved.

2. A method for preparing an external field polarized defective bismuth tungstate piezoelectric catalyst, characterized in that This is achieved through the following technical solutions: (1) First, a defective bismuth tungstate (Bi2WO) containing oxygen vacancies was prepared by solvent thermal reduction. 6-x , abbreviated as BWO-OV) piezoelectric catalyst, the specific process is: prepare 0.05-0.07 mol / L sodium tungstate solution A and bismuth nitrate solution B in ethylene glycol, then slowly drip solution A into solution B according to the molar ratio of W element to Bi element of 1:2, mix and stir for 1-2h, then place in a stainless steel reactor containing polytetrafluoroethylene liner to maintain a certain high temperature condition for heating reaction for a period of time, collect the precipitate after the reaction to obtain BWO-OV piezoelectric catalyst; (2) Weigh 1 to 5 g of the BWO-OV piezoelectric catalyst powder prepared in the above step (1) and place it in a high-voltage DC polarization device to obtain a polarized BWO-OV (BWO-OV-P) piezoelectric catalyst with consistent defect dipole orientation by applying an external electric field.

3. The method for preparing an external field polarized defective bismuth tungstate piezoelectric catalyst according to claim 2, characterized in that: In the step (1), the heating temperature is 160-180° C. and the reaction time is 12-20 hours.

4. The method for preparing an external field polarized defective bismuth tungstate piezoelectric catalyst according to claim 2, characterized in that: The specific steps of the external electric field polarization process in step (2) are as follows: (1) BWO-OV piezoelectric catalyst powder was placed between two copper plates containing needle-tip electrodes in a high-voltage DC polarization device; (2) Turn on the high voltage DC power supply to apply a corona polarization voltage of 3 to 10 kV, and polarize at a temperature of 25 to 180° C. in air for 20 to 100 minutes; (3) After the voltage-maintaining polarization is completed, the high-voltage DC power supply is turned off to prepare the BWO-OV-P piezoelectric catalyst after external field polarization.

Citation Information

Cited By

  • Synthesis of three-heterojunction type piezoelectric hydrogen evolution catalyst and efficient piezoelectric catalytic hydrogen production method of three-heterojunction type piezoelectric hydrogen evolution catalyst

    CN121381044A