Nine cobalt octasulfide (at) zinc sulfide / carbon composite material as well as preparation method and application thereof in sodium ion battery
By preparing a Co9S8 cobalt sulfide@zinc sulfide/carbon composite material, the problems of poor conductivity and volume expansion of Co9S8 were solved, achieving high cycle stability and high capacity at low temperatures for sodium-ion batteries, and providing excellent electrochemical performance.
Patent Information
- Application Number
- CN202411070141.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-22
AI Technical Summary
Existing Co9S8 as a negative electrode material for lithium-ion batteries suffers from poor conductivity and rapid capacity decay and reduced cycle stability due to volume expansion. Furthermore, existing bimetallic sulfides are rarely used in sodium-ion batteries.
An irregular spherical or blocky Co9S8@ZnS/C structure was formed by hydrothermal reaction and annealing using a cobalt octasulfide@zinc sulfide/carbon composite material. The carbon layer encapsulates the nanoparticles, which improves the conductivity and reaction sites, and accelerates ion diffusion through the heterojunction interface.
It significantly improves the cycle stability, lifespan, and battery capacity at low temperatures of sodium-ion batteries, exhibiting high reversible capacity and stable cycle performance, and the materials are inexpensive and readily available.
Smart Images

Figure CN118993160A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of sodium ion battery composite materials, and specifically relates to a nonacobalt octasulfide@zinc sulfide / carbon composite material and a preparation method thereof and application in sodium ion batteries. The prepared bimetallic sulfide Co9S8@ZnS / C is used as a sodium ion battery negative electrode material for manufacturing sodium ion batteries. Background Art
[0002] In today's society, lithium-ion batteries are widely used in portable electronic devices and electric vehicles due to their high specific capacity, portability, recyclability and long service life. At the same time, with the continuous development of society, people's demand for batteries is increasing, and higher requirements are also placed on the specific capacity and cycle life of batteries. Therefore, it is necessary to develop new battery materials.
[0003] Transition metal sulfides have been proven to have high theoretical capacity and good mechanical properties, and are very promising negative electrode materials for lithium-ion batteries. Commonly used ones include cobalt sulfide, nickel sulfide, zinc sulfide, manganese sulfide, iron sulfide, tin sulfide, etc. Among them, Co9S8, as a type of metal sulfide, has also attracted much attention. However, like other metal sulfides, Co9S8 has poor conductivity, and its large volume expansion changes during charging and discharging can easily cause electrode structure collapse, resulting in rapid battery capacity decay and reduced cycle stability. Rechargeable sodium-ion batteries (SIBs) are becoming an important supplement to lithium-ion batteries (LIBs), thanks to their extensive energy storage based on the natural abundance of sodium resources and environmental friendliness.
[0004] Monometallic sulfides have been extensively studied and explored as negative electrode materials for sodium-ion batteries. Bimetallic sulfides have shown extraordinary improvements in electrochemical performance compared to monometallic chalcogenides, but only a very small number of bimetallic sulfides have been studied for use in sodium-ion batteries. Bimetallic sulfide-based sodium-ion battery negative electrode materials have shown good electrochemical performance and should be explored as a promising sodium-ion negative electrode material. Since bimetallic sulfides can be combined with a variety of metals or phases and can be combined in many novel structures, other bimetallic sulfide combinations have been developed and used as high-performance negative electrode materials for SIBs, as well as the exploration of the sodium storage mechanism of the material and the composite modification of the electrode material. Summary of the invention
[0005] The object of the present invention is to provide a cobalt octasulfide @ zinc sulfide / carbon composite material and a preparation method thereof. The prepared Co9S8 @ ZnS / C composite material has an irregular spherical or block structure with a size of 0.4-0.8 μm. The preparation method is simple and the cost is low.
[0006] Another object of the present invention is to provide an application of a nonacobalt octasulfide@zinc sulfide / carbon composite material in a sodium ion battery. The nonacobalt octasulfide@zinc sulfide / carbon composite material is used as an active material to prepare a negative electrode of a sodium ion battery, and then to prepare a sodium ion battery, which greatly improves the cycle stability, service life and battery capacity in a low temperature environment.
[0007] The specific technical solutions of the present invention are as follows:
[0008] A method for preparing a nonacobalt octasulfide@zinc sulfide / carbon composite material comprises the following steps:
[0009] 1) Mixing the CoS nanosphere precursor, the organic ligand and the solvent, and stirring to mix well;
[0010] 2) adding ZnSO4 solution dropwise to the solution in step 1), stirring and reacting to obtain precursor CoS@ZIF-8 nanospheres;
[0011] 3) The precursor CoS@ZIF-8 nanospheres are calcined under a protective atmosphere to obtain a Co9S8@ZnS / C composite material.
[0012] In step 1), the mass ratio of the CoS nanosphere precursor to the organic ligand is 1:6.6-13.2, preferably 1:6.6;
[0013] In step 1), the concentration of the CoS nanosphere precursor in the solvent is 0.001-0.0015 g / mL;
[0014] The preparation method of the CoS nanosphere precursor in step 1) is:
[0015] The cobalt source, NH4F and urea are dispersed in a solvent, and then a sulfur source is added to undergo a hydrothermal reaction to obtain CoS nanospheres.
[0016] In the preparation method of CoS nanospheres, the molar ratio of the cobalt source, the sulfur source, NH4F and urea is 1:4-5.5:1-2:2.5-3; preferably 1:5:1.5:3; the cobalt source is a soluble cobalt source, preferably Co(NO3)2·6H2O or CoSO4·7H2O; the solvent is anhydrous ethanol, and the sulfur source is a soluble sulfur source, preferably thioacetamide; the concentration of the cobalt source in the solvent is 0.01-0.05 mol / L; the hydrothermal reaction is 130-150°C for 10-14h, preferably 140°C for 12h; after the hydrothermal reaction, washing is performed, washing with water 4-6 times, washing with ethanol 1-2 times, centrifuging, and drying at a temperature of 40-80°C for 12-15h;
[0017] In step 1), the prepared CoS nanospheres are relatively smooth spheres with a size of 400±50 nm.
[0018] Preferably, the preparation method of CoS nanospheres is as follows: 0.5 mmol of Co(NO3)2·6H2O, 1.5 mmol of urea, and 0.75 mmol of ammonium fluoride are added to 40 mL of anhydrous ethanol and stirred for 10 min, and then 2.5 mmol of thioacetamide is added and stirred for 10 min, and then a hydrothermal reaction is carried out at 140°C for 12 h, and the product CoS nanospheres are obtained after washing after the reaction is completed.
[0019] In step 1), the organic ligand is 2-methylimidazole;
[0020] In step 1), the solvent is anhydrous methanol;
[0021] In step 1), stirring and mixing means ultrasonic stirring at room temperature for 0.5 h, and then stirring for another 0.5 h;
[0022] In step 2), the volume ratio of the ZnSO4 solution to the volume ratio of the solvent in step 1) is 1:2;
[0023] In step 2), the concentration of the ZnSO4 solution is 0.05-0.1 mol / L, preferably 0.05 mol / L;
[0024] In step 2), the solvent of the ZnSO4 solution is anhydrous methanol, and ZnSO4 is added to anhydrous methanol and stirred for 0.5h to obtain.
[0025] In step 2), the stirring reaction refers to stirring the reaction at room temperature for 4 hours;
[0026] The calcination conditions in step 3) are: calcination at 650°C for 2 hours, preferably, the heating rate is 2°C / min, the temperature is raised to 650°C, and calcination is carried out in a tubular furnace.
[0027] The protective atmosphere in step 4) is nitrogen or argon;
[0028] The present invention provides a nonacobalt octasulfide@zinc sulfide / carbon composite material, which is prepared by the above method. The nonacobalt octasulfide@zinc sulfide / carbon composite material is an irregular spherical or block structure with a size of 0.4-0.8 μm. The core layer is nonacobalt octasulfide with a smooth surface; the shell layer is zinc sulfide with a rough surface.
[0029] Another object of the present invention is to provide an application of a nonacobalt octasulfide@zinc sulfide / carbon composite material in a sodium ion battery. The nonacobalt octasulfide@zinc sulfide / carbon composite material is used as an active material to prepare a negative electrode of a sodium ion battery, and then to prepare a sodium ion battery.
[0030] Specifically, the nonacobalt octasulfide@zinc sulfide / carbon composite material is an active material, which is evenly mixed with conductive carbon black and PVDF in a ratio of 8:1:1 or 7:2:1, and then evenly dispersed in N-methylpyrrolidone (NMP) by magnetic stirring for 6-8 hours, and the evenly mixed slurry is coated on a copper foil by a coater, and placed in a vacuum drying oven at 60-80°C, and after drying for 12-24 hours, it is pressed by a tablet press, and then cut into a small circular electrode sheet by a sheet cutter; the prepared electrode sheet is assembled into a button battery in a glove box filled with high-purity argon and the water oxygen value is ≤0.01ppm; the electrolyte is NaPF6+DEGDME, the purity of the sodium sheet is Na≥99.99%, the thickness is 0.5mm, and it is cut to the size of the electrode sheet after rolling.
[0031] The specific method of assembling the battery is: add 1 drop of electrolyte on the positive electrode shell of the battery and place the electrode sheet, then add 1 drop of electrolyte and place the glass fiber, add 3 drops of electrolyte on the glass fiber and place the sodium sheet as the counter electrode, then put in two pieces of foam nickel, then add 4 drops of electrolyte, cover the negative electrode shell, press and seal the battery with a hydraulic press, and leave it for 6-12 hours.
[0032] Transition metal sulfides are considered to be excellent negative electrode materials for SIBs due to their high theoretical specific capacity and low manufacturing cost. However, the poor rate performance and durability of transition metal sulfides always lead to low conductivity during the conversion reaction. The present invention improves the conductivity of bimetallic sulfides by calcining the carbon layer obtained by in-situ growth of ZIF-8 on the outer layer of the precursor CoS. The nonacobalt octasulfide@zinc sulfide / carbon composite material provided by the present invention has good cycle stability and high rate performance.
[0033] The present invention improves the electrochemical performance of monometallic Co9S8 and monometallic ZnS by in-situ growth and combining bimetallic sulfides. The polycrystalline surface structure formed between different metal sulfides provides more active sites, improves electron transmission, and the composite material exhibits excellent electrochemical performance. The unique heterojunction of this composite material can accelerate the transmission of electron ions, ensure sufficient electrochemical reaction under low temperature conditions, and maintain capacity and stability. Therefore, the hybrid battery composed of two metal sulfides has great potential in reliable sodium ion batteries with long cycle life.
[0034] Sulfide heterojunction materials have excellent low-temperature cycle performance as negative electrode materials for sodium-ion batteries mainly due to the following reasons:
[0035] Fast ion conductivity: Sulfide heterojunction materials generally have high ionic conductivity, that is, sodium ions can be transported quickly within their structure, which helps to achieve high battery performance in low temperature environments.
[0036] Lower polarization effect: Sulfide heterojunction materials may exhibit lower electrode polarization effect at low temperatures, which means that the stable performance of the battery can be more effectively maintained during the battery charging and discharging process and the cycle life can be improved.
[0037] Excellent structural stability: Sulfide heterojunction materials may have good structural stability and are not prone to structural changes or delamination in low-temperature environments, which helps maintain the performance stability of the battery.
[0038] High specific capacity and cycle stability: Sulfide heterojunction materials generally have higher specific capacity, can store more sodium ions, and can maintain good stability during multiple cycles of charge and discharge.
[0039] Electrochemical reaction kinetics: Sulfide heterojunction materials may have excellent electrochemical reaction kinetics, which can rapidly carry out battery charge and discharge reactions in low temperature environments, thereby improving battery efficiency and cycle performance.
[0040] In general, the excellent low-temperature cycle performance of sulfide heterojunction materials as negative electrode materials for sodium-ion batteries is due to the combined effects of their fast ion conductivity, low polarization effect, structural stability, high specific capacity, electrochemical reaction kinetics, etc. These characteristics make sulfide heterojunction materials a potential choice of excellent negative electrode materials, which can achieve efficient and stable sodium-ion battery performance under low temperature conditions.
[0041] In the final 650°C high-temperature calcination process of the present invention, the precursor CoS is reduced by the outer layer of carbon, the valence changes, and the lattice fringes also change. The Co ions in CoS are divalent, while those in Co9S8 are lower than divalent. S sublimates at high temperature and combines with free Zn ion metal salts to generate ZnS, which adheres to the surface of the precursor and forms ZnS lattice fringes. Because the precursor is spherical, the free Zn ions still maintain a spherical structure after adhering to the surface to form MOF, and the carbon shell formed by carbonization is also spherical, mainly because the internal Co9S8 after calcination supports the spherical structure. The formed carbon layer is very thin, so the size of the final product is almost the same as the size of the precursor CoS.
[0042] Compared with the prior art, the present invention has the advantage of preparing a nonacobalt octasulfide@zinc sulfide / carbon composite material through a simple hydrothermal reaction and annealing process, in which bimetallic sulfide Co9S8@ZnS nanoparticles are encapsulated in a carbon layer. The heterogeneous interface between Co9S8 and ZnS crystals can induce an internal electric field to accelerate ion diffusion kinetics, improve electrical conductivity and provide abundant reaction sites for sodium energy storage. In addition, the carbon matrix shortens the path of electrons / ions and alleviates the strain of volume change. Benefiting from these advantages, the prepared Co9S8@ZnS / C composite material has a high conductivity at 1A g -1After 400 cycles at the same current density, the current density was 458.2 mAh g -1 The high reversible capacity, high specific capacity, stable cycle performance and robust rate performance show that Co9S8@ZnS / C is an excellent and promising SIB negative electrode material. In addition, the zinc source, cobalt source and sulfur source in the present invention are inexpensive and easy to obtain; after carbon coating, the cycle stability of the battery is greatly improved, the service life is increased, and the capacity is increased and stable. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 This is a SEM image of the CoS nanosphere material of the precursor precipitation product of Example 1;
[0044] Figure 2 This is a SEM image of the CoS@ZIF-8 nanosphere material, a precursor precipitation product prepared in Example 1;
[0045] Figure 3 This is a SEM image of the cobalt octasulfide@zinc sulfide / carbon composite material Co9S8@ZnS / C prepared in Example 1;
[0046] Figure 4 TEM image of the nonacobalt octasulfide@zinc sulfide / carbon composite material Co9S8@ZnS / C prepared in Example 1;
[0047] Figure 5 This is the XRD pattern of the cobalt octasulfide@zinc sulfide / carbon composite material Co9S8@ZnS / C prepared in Example 1;
[0048] Figure 6 This is the XRD pattern of the nanosphere material of the precursor CoS precipitation product of Example 1;
[0049] Figure 7 TEM image of the cobalt octasulfide@zinc sulfide / carbon composite material Co9S8@ZnS / C prepared in Example 2;
[0050] Figure 8 The cobalt octasulfide@zinc sulfide / carbon composite material Co9S8@ZnS / C prepared in Example 1 was used as a negative electrode material for sodium ion batteries at 0.1A g -1 Cyclic stability test diagram under current density;
[0051] Fig. 9 The constant current charge-discharge curve of the cobalt octasulfide@zinc sulfide / carbon composite material Co9S8@ZnS / C prepared in Example 1 as the negative electrode material of the sodium ion battery;
[0052] Fig.10 This is a rate diagram of the nonacobalt octasulfide@zinc sulfide / carbon composite material Co9S8@ZnS / C prepared in Example 1 as a negative electrode material for a sodium ion battery;
[0053] Fig.11 The cobalt octasulfide@zinc sulfide / carbon composite material Co9S8@ZnS / C prepared in Example 1 was used as a negative electrode material for sodium ion batteries at 1A g -1 Cyclic stability test diagram under current density;
[0054] Fig.12 The cobalt octasulfide@zinc sulfide / carbon composite material Co9S8@ZnS / C prepared in Example 1 was used as a negative electrode material for sodium ion batteries at 0.2A g -1 Cyclic stability test diagram under current density;
[0055] Fig.13 The cobalt octasulfide@zinc sulfide / carbon composite material Co9S8@ZnS / C prepared in Example 1 was used as a negative electrode material for sodium ion batteries at 1A g -1 Cyclic stability test diagram at current density and high temperature of 50°C;
[0056] Fig.14 The cobalt octasulfide@zinc sulfide / carbon composite material Co9S8@ZnS / C prepared in Example 1 was used as a negative electrode material for sodium ion batteries at 1A g -1 Cyclic stability test diagram at current density and low temperature -10℃;
[0057] Fig.15 This is a rate diagram of the nonacobalt octasulfide@zinc sulfide / carbon composite material Co9S8@ZnS / C prepared in Example 1 as a negative electrode material for sodium ion batteries at a low temperature of -10°C;
[0058] Fig.16 This is the SEM image of the precursor precipitation product CoS@ZIF-8 nanosphere material prepared in Comparative Example 1;
[0059] Fig.17 This is the SEM image of the precursor precipitation product CoS@ZIF-8 nanosphere material prepared in Comparative Example 2;
[0060] Fig.18 This is a SEM image of the cobalt octasulfide@zinc sulfide / carbon composite material Co9S8@ZnS / C prepared in Comparative Example 2;
[0061] Fig.19 The cobalt octasulfide@zinc sulfide / carbon composite material Co9S8@ZnS / C prepared in comparative example 2 was used as the negative electrode material for sodium ion batteries at 1A g -1 Cyclic stability test diagram at current density and low temperature of -10℃. DETAILED DESCRIPTION
[0062] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0063] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.
[0064] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.
[0065] Example 1
[0066] A method for preparing a nonacobalt octasulfide@zinc sulfide / carbon composite material comprises the following steps:
[0067] 1) Preparation of precursor: Weigh 0.146g Co(NO3)2·6H2O, 0.09g urea and 0.02775g NH4F respectively and put them into a 100mL beaker, add 40mL anhydrous ethanol, stir magnetically for 10min to dissolve, add 0.1878g thioacetamide, stir magnetically for 10min, transfer to a 50mL polytetrafluoroethylene reactor, put into an oven at 140℃ for reaction for 12h. Cool naturally to room temperature, wash with deionized water by centrifugation 4 times, wash with ethanol twice, vacuum dry at 60℃ for 12h, and collect the precursor CoS precipitate. Its SEM picture is as follows Figure 1 As shown in the figure, it can be seen that it is a nanosphere with a size of about 400nm.
[0068] 2) Preparation of CoS@ZIF-8:
[0069] Weigh 0.1g CoS precursor and 0.66g 2-methylimidazole and add them to 100mL anhydrous methanol, ultrasonicate for 0.5h, stir at room temperature for 0.5h; then add 50mL 0.05M zinc sulfate anhydrous methanol solution dropwise into the mixed solution, stir at room temperature for 4h, wash with deionized water for 4 times, wash with ethanol twice, vacuum dry at 60℃ for 12h, and collect the precursor CoS@ZIF-8 precipitate. Its SEM picture is as follows Figure 2 As shown in the figure, it can be seen that it is a nanosphere with a size of about 400nm.
[0070] 3) Preparation of Co9S8@ZnS / C:
[0071] The dried intermediate product CoS@ZIF-8 was placed on a porcelain boat and calcined in a nitrogen flow atmosphere at a temperature of 650°C, a calcination time of 2h, and a heating rate of 2°C / min. Finally, the product Co9S8@ZnS / C was obtained, and its SEM image is shown in the figure. Figure 3 As shown in the figure, it can be seen that it is an irregular spherical structure. Figure 4 shown.
[0072] The XRD pattern of the Co9S8@ZnS / C composite material obtained in this example is as follows Figure 5 As shown, it is proved that the obtained product is Co9S8@ZnS / C. The XRD pattern of the CoS precursor material obtained in this example is as follows Figure 6 shown.
[0073] Example 2
[0074] A method for preparing a nonacobalt octasulfide@zinc sulfide / carbon composite material comprises the following steps:
[0075] 1) Preparation of precursor: same as in Example 1.
[0076] 2) Preparation of CoS@ZIF-8:
[0077] 0.1 g of CoS precursor and 1.32 g of 2-methylimidazole were weighed and added to 100 mL of anhydrous methanol solution. The mixture was ultrasonicated for 0.5 h and stirred at room temperature for 0.5 h. Then, 50 mL of 0.1 M zinc sulfate anhydrous methanol solution was slowly added. The mixture was stirred at room temperature for 4 h, washed by centrifugation with deionized water 4 times, washed with ethanol twice, and dried in vacuo at 60 °C for 12 h. The precursor CoS@ZIF-8 precipitate was collected.
[0078] 3) Preparation of Co9S8@ZnS / C:
[0079] The dried intermediate product CoS@ZIF-8 was placed on a porcelain boat and calcined in a nitrogen flow atmosphere at a temperature of 650°C for 2 h at a heating rate of 2°C / min. The final product Co9S8@ZnS / C was obtained. The TEM image is shown in Figure 2. Figure 7 shown.
[0080] Example 3
[0081] Example 1 The product of nonacobalt octasulfide@zinc sulfide / carbon composite material is used as a negative electrode material for a sodium ion battery to prepare a sodium battery, specifically:
[0082] The nonacobalt octasulfide@zinc sulfide / carbon composite material is an active material. After being uniformly mixed with conductive carbon black and PVDF in a ratio of 7:2:1, it is evenly dispersed in NMP by magnetic stirring for 8 hours. The evenly mixed slurry is coated on a copper foil by a coater, placed in a vacuum drying oven at 70°C, and pressed into a sheet by a tablet press after drying for 24 hours. It is then cut into a small circular electrode sheet by a sheet cutter; the prepared electrode sheet is assembled into a button battery in a glove box filled with high-purity argon and with a water and oxygen value of ≤0.01ppm; the electrolyte is NaPF6+DEGDME, the purity of the sodium sheet is Na≥99.99%, the thickness is 0.5mm, and it is cut to the size of the electrode sheet after rolling.
[0083] The specific method of assembling the battery is: add 1 drop of electrolyte on the positive electrode shell of the battery and place the electrode sheet, then add 1 drop of electrolyte and place the glass fiber, add 3 drops of electrolyte on the glass fiber and place the sodium sheet as the counter electrode, then put in two pieces of foam nickel, then add 4 drops of electrolyte, cover the negative electrode shell, press and seal the battery with a hydraulic press, and leave it for 12 hours.
[0084] Specific test process: After assembling the sodium ion half-cell, set the process steps on the Xinwei tester, first discharge to 0.2V with constant current, then charge to 3V with constant current, and repeat this cycle for a certain number of times. The active material load of the electrode sheet is about 1.2mgcm -2 .
[0085] Figure 8 The current density is 0.1A g -1 The first cycle is constant current discharge, and then constant current charging. At a lower current density, the battery can be stably cycled for more than 100 times, and the charge and discharge coulomb efficiency is close to 100% (room temperature 25°C).
[0086] Fig. 9 The current density is 0.1A g -1 The first cycle is constant current discharge, then constant current charging, and a representative cycle charge and discharge curve is selected. The figure shows the voltage platform corresponding to the electrochemical reaction. That is, at what voltage does the main capacity contribution occur (room temperature 25℃)
[0087] Fig.10 This is a rate cycle diagram at different current densities at room temperature (25°C). The first cycle is a constant current discharge, followed by a constant current charge. Ten cycles are performed at each current density. The data is from a small current density of 0.1A g -1 Gradually increase to 10A g -1 , and this was done twice in succession, reflecting the advantage of the electrode material that it can be charged quickly.
[0088] Fig.11 The current density is 1A g-1 In the first cycle, constant current discharge is performed, and then constant current charging is performed. After 400 consecutive discharge and charging cycles, the battery still maintains a relatively high capacity, which shows that it still has the advantage of long cycle life under fast charging (room temperature 25°C).
[0089] Fig.12 The current density is 0.2A g -1 The first cycle was performed with constant current discharge and then constant current charging, which verified that after increasing the current density a little, stable cycling was possible, and the charge and discharge coulomb efficiency was close to 100% (room temperature 25°C).
[0090] Fig.13 The current density is 1A g -1 In the first cycle, constant current discharge is performed first, and then constant current charging is performed. At a higher current density and a higher ambient temperature (50°C), the battery can be stably cycled for more than 160 times, and the capacity remains high, and the charge and discharge coulomb efficiency is close to 100%.
[0091] Fig.14 The current density is 1A g -1 The first cycle is constant current discharge, and then constant current charging. At a higher current density and lower ambient temperature (-10°C), the battery can be stably cycled for more than 220 times, and the capacity remains high, and the charge and discharge coulomb efficiency is close to 100%, reflecting the excellent low-temperature battery performance.
[0092] Fig.15 This is a rate cycle diagram at different current densities under low ambient temperature (-10°C). The first cycle is constant current discharge, then constant current charging, and 10 cycles are performed at each current density. The data is from the minimum current density of 0.1A g -1 Gradually increase to 5A g -1 , and it was done three times in a row, which shows that the electrode material can be charged quickly at low temperature. It also shows the practical application potential of the battery, especially in northern cities.
[0093] The difference between Example 1 and Example 2 is:
[0094] The amount of in-situ grown ZIF-8 on the outer layer of the precursor CoS increases, and the carbon layer becomes thicker after calcination. When the film is pulled on the electrode sheet, the mass per unit volume becomes lighter and the carbon content increases, resulting in a decrease in the cycle specific capacity.
[0095] Comparative Example 1
[0096] A method for preparing a nonacobalt octasulfide@zinc sulfide / carbon composite material comprises the following steps:
[0097] 1) Preparation of precursor: same as in Example 1.
[0098] 2) Preparation of CoS@ZIF-8:
[0099] Weigh 0.1g CoS precursor and 0.66g 2-methylimidazole and add them to 100mL ultrapure water solution, ultrasonicate for 0.5h, stir at room temperature for 0.5h, then slowly add 50mL 0.05M zinc sulfate aqueous solution, stir at room temperature for 4h, wash with deionized water by centrifugation 4 times, wash with ethanol twice, vacuum dry at 60℃ for 12h, and collect the precursor CoS@ZIF-8 precipitate. Fig.16 As shown, it is obvious that when ultrapure water is used as the solvent, metal ions and organic ligands can hardly fuse under the same conditions.
[0100] Comparative Example 2
[0101] A method for preparing a nonacobalt octasulfide@zinc sulfide / carbon composite material comprises the following steps:
[0102] 1) Preparation of precursor: same as in Example 1.
[0103] 2) Preparation of CoS@ZIF-8:
[0104] Weigh 0.1g CoS precursor and 0.66g 2-methylimidazole and add them to 100mL anhydrous ethanol solution, ultrasonicate for 0.5h, stir at room temperature for 0.5h, then slowly add 50mL 0.05M zinc sulfate ethanol solution, stir at room temperature for 4h, wash with deionized water for 4 times, wash with ethanol twice, vacuum dry at 60℃ for 12h, and collect the precursor CoS@ZIF-8 precipitate. Fig.17 As shown, when anhydrous ethanol is used as the solvent, under the same conditions, the metal source and the organic ligand can be dissolved, providing a uniform environment for the reaction and forming a uniform ZIF structure.
[0105] 3) Preparation of Co9S8@ZnS / C:
[0106] The dried intermediate product CoS@ZIF-8 was placed on a porcelain boat and calcined in a nitrogen flow atmosphere at a temperature of 650°C for 2 h at a heating rate of 2°C / min to obtain the final product Co9S8@ZnS / C. The SEM image is shown in Figure 2. Fig.18 shown.
[0107] The performance test of comparative example 2 is as follows Fig.19 As shown in the figure, the low-temperature -10°C cycle capacity is lower than that of Example 1, and the initial capacity decay is obvious. This is because the degree of binding between metal ions and organic ligands using anhydrous ethanol as a solvent is not as good as that using anhydrous methanol as a solvent. This will lead to an unstable heterogeneous structure between the two metal sulfide materials, thereby affecting the transmission of ions during the charge and discharge process.
[0108] The Co9S8 material mixed with the ZnS material provided by the present invention provides more active sites during the charge and discharge process. The Co9S8@ZnS / C composite material and its polycrystalline surface structure and increased conductivity after carbon wrapping can greatly improve the cycle stability, service life and battery capacity. The excellent structural design enables it to withstand long cycles of large currents, reduce the loss of active substances during the charge and discharge process, buffer the volume change during the charge and discharge process, and reduce the shedding of active material materials during the cycle, thereby improving the electrochemical performance of the negative electrode material. Among them, ZnS / C has better conductivity, which is conducive to sodium / de-sodiumization during the reaction process. Therefore, it is expected to accelerate the reaction kinetics by constructing a Co9S8@ZnS polycrystalline surface structure. The multi-component synergistic effect of the present invention promotes the rapid transfer of charge, thereby producing excellent low-temperature rate performance and low-temperature cycle performance. The interface effect of the bimetallic sulfide can introduce an internal electric field to improve the reaction kinetics, while providing abundant electrochemical reaction sites, thereby improving its reversible capacity and cycle stability.
[0109] The present invention develops anode materials with unique structures through a practical and direct SIB method. Electrode materials with micro / nano structures are promising candidate materials. Mixed metal sulfides increase the conductivity of redox reaction sites, thereby improving the electrochemical performance of the electrode. The use of bimetallic sulfide material form and effective design of the material's microstructure can effectively reduce the volume expansion phenomenon of the material and prevent the material's structural pulverization, thereby preventing the structural collapse of the electrode material.
[0110] In addition, composite with conductive carbon species can effectively reduce the negative impact of poor conductivity. Carbon-based composites with reasonable structure can improve electronic conductivity and buffer internal stress, which is beneficial to the electrochemical performance of SIBs. Therefore, nanostructured Co9S8 mixed with ZnS to form nanospheres and combined with nitrogen-doped carbon layers is an effective strategy to achieve high-performance SIBs.
[0111] The description of the above embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the protection scope of the present invention.
Claims
1. A method for preparing a nonacobalt octasulfide@zinc sulfide / carbon composite material, characterized in that: The preparation method comprises the following steps: 1) Mixing the CoS nanosphere precursor, the organic ligand and the solvent, and stirring to mix well; 2) adding ZnSO4 solution dropwise to the solution in step 1), stirring and reacting to obtain precursor CoS@ZIF-8 nanospheres; 3) The precursor CoS@ZIF-8 nanospheres are calcined under a protective atmosphere to obtain a Co9S8@ZnS / C composite material.
2. The preparation method according to claim 1, characterized in that: In step 1), the mass ratio of the CoS nanosphere precursor to the organic ligand is 1:6.6-13.
2.
3. The preparation method according to claim 1 or 2, characterized in that: The preparation method of the CoS nanosphere precursor in step 1) is: The cobalt source, NH4F and urea are dispersed in a solvent, and then a sulfur source is added to undergo a hydrothermal reaction to obtain CoS nanospheres.
4. The preparation method according to claim 1 or 2, characterized in that: In step 1), the organic ligand is 2-methylimidazole.
5. The preparation method according to claim 1 or 2, characterized in that: In step 1), the solvent is anhydrous methanol.
6. The preparation method according to claim 1, characterized in that: In step 2), the volume ratio of the ZnSO4 solution to the solvent in step 1) is 1:
2.
7. The preparation method according to claim 1 or 6, characterized in that: In step 2), the concentration of the ZnSO4 solution is 0.05-0.1 mol / L; the solvent of the ZnSO4 solution is anhydrous methanol.
8. The preparation method according to claim 1, characterized in that: The calcination conditions in step 3) are: calcination at 650° C. for 2 hours.
9. A nonacobalt octasulfide@zinc sulfide / carbon composite material prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The nonacobalt octasulfide@zinc sulfide / carbon composite material is an irregular spherical or block structure with a size of 0.4-0.8 μm.
10. Use of the nonacobalt octasulfide@zinc sulfide / carbon composite material according to claim 9 in a sodium ion battery.