Quick-setting type silicon-aluminum phosphate composite cement without high-temperature maintenance and preparation method of quick-setting type silicon-aluminum phosphate composite cement
By introducing calcareous materials and functional control components into silica-alumina phosphate composite cement, and utilizing the heat released by acid-base neutralization reaction to accelerate mineral dissolution and matrix network construction, the problem of slow setting and hardening rate of silica-alumina phosphate composite cement at room temperature is solved, and low-energy and high-strength cement preparation is achieved.
Patent Information
- Application Number
- CN202410902600.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-08
AI Technical Summary
Existing silica-alumina phosphate composite cement has a slow setting and hardening rate at room temperature, resulting in high energy consumption and high cost in its preparation.
Using silica-alumina materials, calcium materials, and phosphate-based activating raw materials, heat is released through acid-base neutralization reactions to accelerate mineral dissolution. Solvents, polymerization accelerators, and early-strength agents are added to synergistically promote the construction of the matrix network and achieve rapid solidification.
Rapid setting and mechanical property development of silica-alumina phosphate composite cement were achieved at room temperature, reducing energy consumption and cost in preparation.
Smart Images

Figure BDA0004930989430000061
Abstract
Description
Technical Field
[0001] The invention belongs to the field of civil engineering materials, and in particular relates to a fast-setting silicoaluminophosphate composite cement that does not require high-temperature curing and a preparation method thereof. Background Art
[0002] Silica-alumina phosphate composite cement is made of silica-alumina materials as raw materials. Under the action of phosphate-based excitation raw materials, it is driven by high temperature to accelerate the depolymerization-polycondensation reaction of minerals in the silica-alumina raw materials to form a three-dimensional network structure matrix. This material has excellent properties such as high mechanical properties, high temperature resistance, acid corrosion resistance, and heavy metal solidification. It has broad potential application prospects in the fields of fire protection and heat insulation, construction, heavy metal solidification, and nuclear waste consolidation.
[0003] However, the reported silicoaluminophosphate composite cement has a very slow setting and hardening rate at room temperature, and often requires high temperature excitation, which leads to problems such as increased carbon emissions, high energy consumption for preparation, and high cost. Therefore, it is of great significance to achieve effective regulation of the setting and hardening of silicoaluminophosphate composite cement at room temperature and reduce its preparation energy consumption and cost for the promotion and application of silicoaluminophosphate composite cement. Summary of the invention
[0004] In view of the above problems, the present invention provides a fast-setting silicoaluminophosphate composite cement that does not require high-temperature curing and a preparation method thereof. The present invention uses silicoaluminomaterials and calcium materials as raw materials, and accelerates the dissolution of minerals in the silicoaluminomaterials through the heat released by the acid-base neutralization reaction between the phosphate-exciting raw materials and the calcium raw materials under the action of phosphate-exciting raw materials. At the same time, under the synergistic effect of the functional regulating components, the construction of the three-dimensional network of the matrix and the development of mechanical properties are accelerated, solving the difficult problems of long setting time and slow strength development of silicoaluminophosphate composite cement under room temperature conditions. The specific contents of the present invention are as follows:
[0005] A fast-setting silicoaluminate phosphate composite cement that does not require high-temperature curing and a preparation method thereof, characterized in that the fast-setting silicoaluminate phosphate composite cement that does not require high-temperature curing comprises a main component and a functional control component. The main components are measured in mass percentage as follows: (1) 50%-70% of silicoaluminate raw materials, (2) 20%-30% of phosphate-based excitation raw materials, and (3) 10%-20% of calcium raw materials, and the sum of the three is 100%. In addition, based on the mass of the silicoaluminate raw materials and the calcium raw materials in the main components being 100%, additional functional control components are added, and the dosage of each functional control component is as follows: (1) 4%-8% of a dissolution agent, (2) 2%-8% of a polymerization accelerator, and (3) 4%-12% of an early strength agent.
[0006] The silicoaluminous raw material in the main component is one or two of fly ash, metakaolin and lithium slag. It is further preferred that the sum of the contents of SiO2 and Al2O3 in the chemical composition of the silicoaluminous raw material is greater than 30%.
[0007] The phosphate excitation raw materials in the main components are one or two of amino trimethylene phosphonic acid, disodium hydroxyethylidene diphosphate, and sodium ethylenediaminetetramethylene phosphate.
[0008] The calcium raw material in the main component is one or two of steel slag, slag and quicklime. It is further preferred that the content of CaO in the chemical composition of the calcium raw material is greater than 30%.
[0009] The solubilizing agent in the function regulating component is one or two of ethyl carbamate, niacinamide and polyoxyethylene sorbitan monostearate.
[0010] The polymerization accelerator in the function regulating component is one or two of aluminum tert-butylbenzoate, dibenzylidene sorbitol and phenol ether phosphate potassium salt NP-4PK.
[0011] The early strength agent in the function regulating component is one or two of calcium pantothenate, calcium hypophosphite and calcium metaphosphate.
[0012] The preparation steps of the fast-setting silicoaluminophosphate composite cement that does not require high-temperature curing are as follows:
[0013] ① Raw material grinding: According to the mass percentage, the silicon aluminum raw materials and calcium raw materials in the main components are placed in a ball mill and ground to control the surface area of the obtained powder to 350m 2 / kg-550m 2 / kg.
[0014] ② Mixing: Place the powder obtained in step ① in a mixer, first add phosphate-based stimulating raw materials according to mass percentage and mix and stir for 30 minutes; then, based on the mass of the silicoalumina raw materials and calcium raw materials in the main components being 100%, additional functional regulating components are added in the following order: first add the accelerator and stir for 15 minutes, then add the polymerization accelerator and stir for 15 minutes, and finally add the early strength agent and continue stirring for 30 minutes to obtain a fast-setting silicoalumina phosphate composite cement that does not require high-temperature curing.
[0015] The present invention aims at the problem that the setting and hardening performance and mechanical properties of silicoaluminophosphate composite cement under room temperature conditions develop slowly. Through the introduction of calcium raw materials and the synergistic effect of functional control components, the silicoaluminophosphate composite cement setting and hardening and mechanical properties of silicoaluminophosphate composite cement under room temperature conditions are achieved. The silicoaluminophosphate composite cement prepared by the technology of the present invention does not need high temperature curing, and its final setting time can be adjusted to about 1.0h under room temperature conditions, and the compressive strength can reach 35MPa in 3 days and 60MPa in 28 days. Specifically, its technical characteristics are that under the action of phosphate-based excitation raw materials, the CaO in the introduced calcium raw materials can react with the phosphate-based excitation raw materials to produce a large amount of heat, which is used as a driving force to accelerate the dissolution rate of minerals in the silicoaluminophosphate raw materials; on the other hand, under the action of the functional control component solubilizing agent, the disintegration rate of minerals in the silicoaluminophosphate raw materials can be further accelerated, and the content of oligomeric structural units such as [SiO4] and [AlO4] in the system can be increased, so that more effective components can be released to participate in the reaction, and the reaction rate and the amount of reaction products generated can be increased. At the same time, the polymerization promoter used has a strong binding ability, which can promote the polymerization of oligomer structural units in the system and accelerate the construction of the matrix network. On this basis, based on the salt effect of the early strength agent, it can react chemically with the phosphate-based excitation raw materials, and can participate in the construction of the matrix network of the silicoaluminophosphate composite cement, increase the precipitation rate of the reaction product, accelerate the hydration process of the slurry, and promote the coagulation and hardening of the matrix. Through the synergistic promotion between the above components, the synergistic development of the coagulation and hardening properties and mechanical properties of the silicoaluminophosphate composite cement at room temperature is achieved.
[0016] The beneficial effects of the present invention are as follows: the fast-setting silicoaluminophosphate composite cement and its preparation method provided by the present invention, which do not require high-temperature curing, avoid the high-temperature excitation link in the existing preparation process of silicoaluminophosphate composite cement, and achieve low-energy consumption and low-cost preparation of silicoaluminophosphate composite cement. At the same time, the realization of the coordinated development goals of the setting and hardening properties and mechanical properties of silicoaluminophosphate composite cement under room temperature conditions enriches the application scenarios of silicoaluminophosphate composite cement. DETAILED DESCRIPTION
[0017] In order to further reflect the effects brought by the present invention, the technical effects of the present invention are further explained in combination with specific examples. The silicon-aluminum raw materials, phosphate-based excitation raw materials and calcium raw materials in the main components of the listed examples are represented by fly ash, disodium hydroxyethylidene diphosphate and steel slag, respectively, wherein the sum of the contents of SiO2 and Al2O3 in the fly ash used is 35.7% to 50.4%, and the content of CaO in the steel slag used is 40.3% to 55.6%. Based on the mass of the silicon-aluminum raw materials and calcium raw materials in the main components as 100%, the additional functional regulating components are represented by polyoxyethylene sorbitan monostearate, phenol ether phosphate potassium salt NP-4PK and calcium pantothenate. The specific details and technical effects of each case are described as follows.
[0018] Example 1
[0019] Weigh each raw material in the main component by mass percentage, wherein the functional control component is calculated based on the mass of the silicon-aluminum raw material and the calcium raw material in the main component as 100%, and is additionally added as follows:
[0020] Main components: fly ash 50%, disodium hydroxyethylidene diphosphate 30%, steel slag 20%, the sum of the three is 100%. The sum of the contents of SiO2 and Al2O3 in the fly ash used in this embodiment is 50.4%, and the content of CaO in the steel slag used is 55.6%.
[0021] Functional regulating components (calculated by the mass percentage of the main components of fly ash, alumina-silica raw material, and steel slag, additionally added): 8% polyoxyethylene sorbitan monostearate, 8% phenol ether phosphate potassium salt NP-4PK, 12% calcium pantothenate.
[0022] ① Raw material grinding: accurately weigh 5kg of fly ash and steel slag according to the mass percentage of the main components and grind them in a ball mill to control the surface area of the obtained powder to 350m 2 / kg-400m 2 / kg.
[0023] ② Mixing: Place the powder obtained in step ① in a mixer, first add the phosphate-based activating raw material disodium hydroxyethylidene diphosphate according to mass percentage, and mix and stir for 30 minutes; then, based on the mass of the silicoalumina raw material fly ash and the calcium raw material steel slag in the main components being 100%, additional functional regulating components are added, and the order of addition is: first add the promoter polyoxyethylene sorbitan monostearate and stir for 15 minutes, then add the polymerization accelerator phenol ether phosphate potassium salt NP-4PK and stir for 15 minutes, and finally add the early strength agent calcium pantothenate and continue stirring for 30 minutes to obtain the fast-setting silicoalumina phosphate composite cement that does not require high-temperature curing.
[0024] Example 2
[0025] Weigh each raw material in the main component by mass percentage, wherein the functional control component is calculated based on the mass of the silicon-aluminum raw material and the calcium raw material in the main component as 100%, and is additionally added as follows:
[0026] Main components: fly ash 60%, disodium hydroxyethylidene diphosphate 26%, steel slag 14%, the sum of the three is 100%. The sum of the contents of SiO2 and Al2O3 in the fly ash used in this embodiment is 45.8%, and the content of CaO in the steel slag used is 47.2%.
[0027] Functional regulating components (calculated by the mass percentage of the main components of fly ash, alumina-silica raw material, and steel slag, added additionally): polyoxyethylene sorbitan monostearate 7%, phenol ether phosphate potassium salt NP-4PK 6%, and calcium pantothenate 8%.
[0028] ① Raw material grinding: 5 kg of fly ash and steel slag are weighed accurately according to the mass percentage of the main components and placed in a ball mill for grinding, so that the surface area of the obtained powder is controlled within 400 m 2 / kg-450m 2 / kg.
[0029] ② Mixing: Place the powder obtained in step ① in a mixer, first add the phosphate-based activating raw material disodium hydroxyethylidene diphosphate according to mass percentage, and mix and stir for 30 minutes; then, based on the mass of the silicoalumina raw material fly ash and the calcium raw material steel slag in the main components being 100%, additional functional regulating components are added, and the order of addition is: first add the promoter polyoxyethylene sorbitan monostearate and stir for 15 minutes, then add the polymerization accelerator phenol ether phosphate potassium salt NP-4PK and stir for 15 minutes, and finally add the early strength agent calcium pantothenate and continue stirring for 30 minutes to obtain the fast-setting silicoalumina phosphate composite cement that does not require high-temperature curing.
[0030] Example 3
[0031] Weigh each raw material in the main component by mass percentage, wherein the functional control component is calculated based on the mass of the silicon-aluminum raw material and the calcium raw material in the main component as 100%, and is additionally added as follows:
[0032] Main components: fly ash 65%, disodium hydroxyethylidene diphosphate 23%, steel slag 12%, the sum of the three is 100%. The sum of the contents of SiO2 and Al2O3 in the fly ash used in this embodiment is 38.4%, and the content of CaO in the steel slag used is 44.6%.
[0033] Functional regulating components (calculated by the mass percentage of the main components of fly ash, alumina-silica raw material, and steel slag, additionally added): polyoxyethylene sorbitan monostearate 6%, phenol ether phosphate potassium salt NP-4PK 4%, and calcium pantothenate 6%.
[0034] ① Raw material grinding: accurately weigh 5kg of fly ash and steel slag according to the mass percentage of the main components and grind them in a ball mill to control the surface area of the obtained powder to 450m 2 / kg-500m 2 / kg.
[0035] ② Mixing: Place the powder obtained in step ① in a mixer, first add the phosphate-based activating raw material disodium hydroxyethylidene diphosphate according to mass percentage, and mix and stir for 30 minutes; then, based on the mass of the silicoalumina raw material fly ash and the calcium raw material steel slag in the main components being 100%, additional functional regulating components are added, and the order of addition is: first add the promoter polyoxyethylene sorbitan monostearate and stir for 15 minutes, then add the polymerization accelerator phenol ether phosphate potassium salt NP-4PK and stir for 15 minutes, and finally add the early strength agent calcium pantothenate and continue stirring for 30 minutes to obtain the fast-setting silicoalumina phosphate composite cement that does not require high-temperature curing.
[0036] Example 4
[0037] Weigh each raw material in the main component by mass percentage, wherein the functional control component is calculated based on the mass of the silicon-aluminum raw material and the calcium raw material in the main component as 100%, and is additionally added as follows:
[0038] Main components: fly ash 70%, disodium hydroxyethylidene diphosphate 20%, steel slag 10%, the sum of the three is 100%. The sum of the contents of SiO2 and Al2O3 in the fly ash used in this embodiment is 35.7%, and the content of CaO in the steel slag used is 40.3%.
[0039] Functional regulating components (calculated by the mass percentage of the main components of fly ash, alumina-silica raw material, and steel slag, additionally added): polyoxyethylene sorbitan monostearate 4%, phenol ether phosphate potassium salt NP-4PK 2%, and calcium pantothenate 4%.
[0040] ① Raw material grinding: 5 kg of fly ash and steel slag are weighed accurately according to the mass percentage of the main components and placed in a ball mill for grinding, so that the surface area of the obtained powder is controlled within 500 m 2 / kg-550m 2 / kg.
[0041] ② Mixing: Place the powder obtained in step ① in a mixer, first add the phosphate-based activating raw material disodium hydroxyethylidene diphosphate according to mass percentage, and mix and stir for 30 minutes; then, based on the mass of the silicoalumina raw material fly ash and the calcium raw material steel slag in the main components being 100%, additional functional regulating components are added, and the order of addition is: first add the promoter polyoxyethylene sorbitan monostearate and stir for 15 minutes, then add the polymerization accelerator phenol ether phosphate potassium salt NP-4PK and stir for 15 minutes, and finally add the early strength agent calcium pantothenate and continue stirring for 30 minutes to obtain the fast-setting silicoalumina phosphate composite cement that does not require high-temperature curing.
[0042] Comparative Example 1
[0043] In this comparative example, no dissolution promoter polyoxyethylene sorbitan monostearate was added, and the rest was the same as in Example 1.
[0044] Comparative Example 2
[0045] In this comparative example, no polymerization accelerator phenol ether phosphate potassium salt NP-4PK was added, and the rest was the same as in Example 2.
[0046] Comparative Example 3
[0047] In this comparative example, no early strength agent calcium pantothenate is added, and the rest is the same as in Example 3.
[0048] Comparative Example 4
[0049] In this comparative example, no function regulating component is added, and the rest is the same as in Example 1.
[0050] Comparative Example 5
[0051] In this comparative example, the calcium raw material steel slag is completely replaced by the silicon-alumina raw material fly ash, and the rest is the same as Example 1.
[0052] Comparative Example 6
[0053] In this comparative example, the calcium raw material steel slag is completely replaced by the silicon-aluminum raw material fly ash, and no function regulating component is added. The rest is the same as Example 1.
[0054] The above embodiments and comparative examples were tested for setting time according to GB / T1346-2019 "Test Method for Standard Consistency, Setting Time and Stability of Cement"; and the compressive strength of each embodiment and comparative example was tested for 3 days and 28 days according to GB / T 17671-2021 "Test Method for Strength of Cement Mortar (ISO Method)". The test results of each embodiment and comparative example are shown in Table 1.
[0055] Table 1 Setting time and compressive strength of fast-setting silicon-aluminum phosphate composite cement without high temperature curing
[0056]
[0057] It can be seen from Table 1 that in Comparative Example 6, since no calcium raw material and functional regulating component were added, the prepared silicoaluminophosphate composite cement solidified and hardened very slowly, the final setting time was as long as 48.4 hours, and its 3-day and 28-day compressive strengths were both low. In comparison, the present invention significantly shortened the setting time and greatly improved the strength of the silicoaluminophosphate composite cement in Examples 1-4 by introducing calcium raw materials and under the synergistic effect of functional regulating components, achieving the coordinated development of the setting and hardening properties and mechanical properties of the silicoaluminophosphate composite cement at room temperature.
[0058] Compared with Example 1, due to the lack of a solvent in the functional regulating component, Comparative Example 1 reduces the disintegration rate of minerals in the silicoaluminate raw material, resulting in a decrease in the content of oligomeric structural units such as the effective ingredients [SiO4] and [AlO4] participating in the reaction in the system, thereby reducing the reaction rate and the amount of reaction products generated, causing the matrix coagulation time to be slightly extended and the strength to be significantly reduced.
[0059] Compared with Example 2, due to the lack of polymerization promoter in the function regulating component, the polymerization degree of the oligomer structural units in the matrix in Comparative Example 2 is reduced, resulting in prolonged coagulation time of the matrix and significantly reduced strength.
[0060] Compared with Example 3, due to the absence of the early strength agent in the functional regulation component, the precipitation rate of the reaction product and the hydration process of the slurry were reduced in Comparative Example 3, which resulted in a prolonged setting time of the matrix and reduced strength.
[0061] Compared with Example 1, Comparative Example 4 reduces the disintegration rate and reaction rate of the silicoaluminate mineral and the precipitation rate and generation amount of the product due to the lack of the functional regulating components of the solvent, polymerization accelerator and early strength agent, resulting in a significant extension of the setting time of the matrix and a significant reduction in strength.
[0062] Compared with Example 1, in Comparative Example 5, due to the lack of calcium raw materials, the heat released during the reaction is greatly reduced, thereby significantly reducing the dissolution rate of minerals in the silicon-aluminum raw materials. Even under the action of the functional regulating components, the coagulation, hardening and strength development of the matrix are still very slow.
[0063] In summary, it can be seen that the combined use of calcium raw materials and functional control components is an effective means to achieve the coordinated development of the setting and hardening properties and mechanical properties of silicoaluminophosphate composite cement at room temperature. The absence of any component will have an adverse effect on the performance of silicoaluminophosphate composite cement.
[0064] The above embodiments are only used to explain the present invention and do not constitute a limitation on the scope of the claims. Other alternative means that can be thought of by those skilled in the art based on the contents of the present specification should be within the protection scope of the claims of the present invention.
Claims
1. A fast-setting silicoaluminophosphate composite cement that does not require high-temperature curing, characterized in that: The fast-setting silicoaluminate phosphate composite cement that does not require high-temperature curing includes a main component and a functional control component; wherein the main components are measured in mass percentage as follows: (1) 50%-70% of silicoaluminate raw materials, (2) 20%-30% of phosphate-based stimulating raw materials, and (3) 10%-20% of calcium raw materials, and the sum of the three is 100%; in addition, based on the mass of the silicoaluminate raw materials and the calcium raw materials in the main components being 100%, additional functional control components are added, and the dosage of each functional control component is as follows: (1) 4%-8% of a dissolution agent, (2) 2%-8% of a polymerization accelerator, and (3) 4%-12% of an early strength agent.
2. The fast-setting silicoaluminophosphate composite cement that does not require high-temperature curing according to claim 1, characterized in that: The silicoaluminous raw materials in the main components are one or two of fly ash, metakaolin, and lithium slag, and the sum of the mass percentages of SiO2 and Al2O3 in the chemical composition of the silicoaluminous raw materials is greater than 30%; the phosphate excitation raw materials in the main components are one or two of aminotri(methylene)phosphoric acid, disodium hydroxyethylidene diphosphate, and sodium ethylenediaminetetramethylene phosphate; the calcium raw materials in the main components are one or two of steel slag, slag, and quicklime, and the mass percentage of CaO in the chemical composition of the calcium raw materials is greater than 30%.
3. According to claim 1, a fast-setting silicoaluminophosphate composite cement that does not require high-temperature curing, its technical feature is that the dissolution promoter in the functional regulation component is one or two of ethyl formate, niacinamide and polyoxyethylene sorbitan monostearate; the polymerization accelerator in the functional regulation component is one or two of aluminum tert-butyl benzoate, dibenzylidene sorbitol and phenol ether phosphate potassium salt NP-4PK; the early strength agent in the functional regulation component is one or two of calcium pantothenate, calcium hypophosphite and calcium metaphosphate.
4. A method for preparing a fast-setting silicoaluminophosphate composite cement that does not require high temperature curing as described in any one of claims 1 to 3, characterized in that Here are the steps: ① Raw material grinding: According to the mass percentage, the silicon aluminum raw materials and calcium raw materials in the main components are placed in a ball mill and ground to control the surface area of the obtained powder to 350m 2 / kg-550m 2 / kg; ② Mixing: Place the powder obtained in step ① in a mixer, first add phosphate-based stimulating raw materials according to mass percentage and mix and stir for 30 minutes; then, based on the mass of the silicoalumina raw materials and the calcium raw materials in the main components being 100%, additional functional regulating components are added in the following order: first add the accelerator and stir for 15 minutes, then add the polymerization accelerator and stir for 15 minutes, and finally add the early strength agent and continue stirring for 30 minutes to obtain the fast-setting silicoalumina phosphate composite cement that does not require high-temperature curing.
Citation Information
Patent Citations
Modified reinforced geopolymer gelling material and preparation method thereof
CN107746212A
Modifier for improving setting and hardening performance and carbonization resistance of ardealite-based cementing material
CN115093150A
Cement-free residue soil curing agent as well as preparation method and application thereof
CN115231892A
Low-temperature early-strength coagulant for magnesite cementing material as well as preparation method and use method of low-temperature early-strength coagulant
CN116514449A
Quick-setting alkali-activated low-calcium silicon-aluminum composite cement without high-temperature maintenance and preparation method of quick-setting alkali-activated low-calcium silicon-aluminum composite cement
CN117247239A