Ceramic substrate and manufacturing method thereof

By controlling the solid content of the casting slurry and optimizing the sintering process, the problem of large warpage of ceramic substrates was solved, and high-quality and high-yield ceramic substrate production was achieved.

CN118993712APending Publication Date: 2024-11-22GUANGDONG HUANBO NEW MATERIAL CO LTD +1

Patent Information

Application Number
CN202411036489.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the existing technology, the low solid content of the casting paste during the manufacturing process of ceramic substrates leads to a large warpage of the product, which affects the product quality.

Method used

By controlling the solid content of the cast slurry within the range of 65-70 wt%, and by optimizing the heating rate, cooling rate, and air flow rate during the sintering process, especially the control of the second stage of sintering, the sintering shrinkage rate and deformation are reduced, thereby reducing warpage.

Benefits of technology

It effectively reduces the warpage of ceramic substrates, improves product quality and yield, simplifies the production process, and reduces costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a ceramic substrate and a manufacturing method thereof, and relates to the technical field of ceramic bases.The manufacturing method of the ceramic substrate comprises the following steps that tape casting slurry is prepared, and the solid content of the tape casting slurry is 65-70 wt%; and sequentially carrying out tape casting, lamination and sintering on the tape casting slurry to obtain the ceramic substrate. According to the technical scheme, the density of the tape-casting green body can be improved, and the subsequent sintering shrinkage rate and deformation are effectively reduced, so that the warping degree of a product obtained after sintering is reduced, and the product quality is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of ceramic substrates, and in particular to a ceramic substrate and a manufacturing method thereof. Background Art

[0002] At present, ceramic substrates are widely used in high-power power semiconductor modules, power control circuits, automotive electronics, aerospace and military electronic components, solar panel components, etc. due to their superior heat dissipation performance, current carrying capacity, insulation, thermal expansion coefficient, etc. compared to ordinary glass fiber PCB boards. When making ceramic substrates, the solid content of the cast slurry used is low. After the conventional casting, lamination, and sintering processes, the warpage of the obtained product is large, which affects the quality of the product.

[0003] The above contents are only used to assist in understanding the technical solution of the present invention and do not constitute an admission that the above contents are prior art. Summary of the invention

[0004] The main purpose of the present invention is to provide a ceramic substrate and a manufacturing method thereof, aiming to reduce the warpage of the product and thus improve the product quality.

[0005] To achieve the purpose of the present invention, the present invention provides a method for manufacturing a ceramic substrate, the method comprising the following steps: preparing a tape casting slurry, wherein the solid content of the tape casting slurry is 65-70wt%;

[0006] The casting slurry is sequentially subjected to casting molding, lamination and sintering to obtain the ceramic substrate.

[0007] In one embodiment, the casting slurry includes the following raw materials in parts by mass:

[0008] 40-60 parts of alumina powder, 0.1-1 parts of calcium oxide, 0.1-1 parts of magnesium oxide, 0.1-1 parts of silicon dioxide, 30-45 parts of solvent, 5-10 parts of plasticizer and 7-10 parts of binder.

[0009] In one embodiment, the purity of the aluminum oxide powder is 99-99.999%; and / or the D50 value of the aluminum oxide powder is 0.5-1.0 μm.

[0010] In one embodiment, the solvent includes an ester and an alcohol, and the mass ratio of the ester to the alcohol is (1-3):(7-9), wherein the ester is at least one of ethyl acetate, methyl acetate, propyl acetate, and butyl acetate, and the alcohol is at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol, and isobutanol.

[0011] In one embodiment, the sintering includes a first stage sintering and a second stage sintering. The first stage sintering is a process of heating up first and then keeping warm, and the temperature after heating is 400-1000°C. The second stage sintering is a process of heating up first, keeping warm, and then cooling, and the temperature after heating is 1400-1750°C.

[0012] In one embodiment, the heating rate of the second stage sintering is 0.1-4°C / min, the cooling rate is 0.5-1°C / min, and the holding time is 2-4h.

[0013] In one embodiment, the air flow rate of the second stage sintering is 1-5 L / min.

[0014] In one embodiment, the heating rate of the first stage sintering is 0.1-3°C / min, and the holding time is 4-6h.

[0015] In one embodiment, the laminate is an isostatically pressed laminate, the temperature of the isostatically pressed laminate is 50-80° C., the pressure is 50-100 MPa, and the holding time is 5-20 min.

[0016] The present invention also provides a ceramic substrate, which is manufactured by using the manufacturing method of the ceramic substrate as described above.

[0017] The technical solution of the present invention can improve the green density of tape-casting by controlling the solid content of the tape-casting slurry within the range of 65-70wt%, effectively reduce the subsequent sintering shrinkage rate and deformation, thereby reducing the warpage of the product obtained after sintering and improving the product quality. DETAILED DESCRIPTION

[0018] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.

[0019] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.

[0020] In order to solve the technical problem that the solid content of the casting slurry currently used in the production of ceramic substrates is low, resulting in a large warpage of the obtained product, thereby affecting the product quality, the present invention provides a method for producing a ceramic substrate, aiming to reduce the warpage of the product, thereby improving the product quality.

[0021] The method for manufacturing a ceramic substrate provided by the present invention comprises the following steps:

[0022] Prepare a tape casting slurry, wherein the solid content of the tape casting slurry is 65-70wt%;

[0023] The casting slurry is sequentially subjected to casting molding, lamination and sintering to obtain a ceramic substrate.

[0024] The ceramic substrate of the present invention can be an alumina ceramic substrate, and the tape casting slurry used in its production is alumina slurry, and the solid content of the tape casting slurry used is 65-70wt% (such as 65wt%, 66wt%, 67wt%, 68wt%, 69wt%, 70wt% and the interval between any two end points). It should be noted that the solid content of the tape casting slurry refers to the mass percentage of the solid powder content in the total slurry.

[0025] The present invention controls the solid content of the tape casting slurry within the range of 65-70wt%, which can improve the green density of the tape casting, effectively reduce the subsequent sintering shrinkage rate and deformation, thereby reducing the warpage of the product obtained after sintering and improving the product quality.

[0026] In some embodiments of the present invention, the casting slurry includes the following raw materials, measured by mass: 40-60 parts of aluminum oxide powder (such as 40 parts, 45 parts, 50 parts, 55 parts, 60 parts and any interval between the two end points), 0.1-1 part of calcium oxide (such as 0.1 parts, 0.3 parts, 0.5 parts, 0.8 parts, 1 parts and any interval between the two end points), 0.1-1 part of magnesium oxide (such as 0.1 parts, 0.3 parts, 0.5 parts, 0.8 parts, 1 parts and any interval between the two end points) , 0.1-1 parts of silicon dioxide (such as 0.1 parts, 0.3 parts, 0.5 parts, 0.8 parts, 1 parts and the interval between any two endpoints), 30-45 parts of solvent (such as 30 parts, 35 parts, 40 parts, 45 parts and the interval between any two endpoints), 5-10 parts of plasticizer (such as 5 parts, 6 parts, 7 parts, 8 parts, 9 parts, 10 parts and the interval between any two endpoints) and 7-10 parts of binder (such as 7 parts, 8 parts, 9 parts, 10 parts and the interval between any two endpoints). The present invention can obtain a uniformly dispersed casting slurry by reasonably controlling the amount of each raw material of the casting slurry, and it is not easy to have undesirable phenomena such as cracking during the casting molding process. At the same time, the green porcelain tape obtained by the casting molding has high volume density, high strength, toughness and good ductility.

[0027] Optionally, the purity of the alumina powder is 99-99.999%. Selecting high-purity alumina powder is beneficial to improving the dielectric properties, mechanical properties and yield rate of the product.

[0028] Optionally, the D50 value of alumina powder is 0.5-1.0μm (such as 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1.0μm and the interval between any two endpoints). The use of alumina powder with the above submicron particle size can improve the dielectric properties and mechanical properties of the sintered product, and the appearance of the sintered product has no defects such as gray spots and white spots, and the yield rate is high. It should be noted that D50 refers to the particle size corresponding to when the cumulative particle size distribution percentage of a sample reaches 50%. Its physical meaning is that particles with a particle size larger than it account for 50%, and particles with a particle size smaller than it also account for 50%. D50 is also called the median diameter or median particle size, which is the average particle size of alumina powder.

[0029] Optionally, the solvent includes ester and alcohol, and the mass ratio of the ester to the alcohol is (1-3):(7-9), for example, the mass ratio of the two is 1:7, 1:8, 1:9, 2:7, 2:8, 2:9, 3:7, 3:8, 3:9 and an interval value between any two end point values, wherein the ester is at least one of ethyl acetate, methyl acetate, propyl acetate, and butyl acetate, and the alcohol is at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol, and isobutanol.

[0030] Optionally, the dispersant is triolein, which has a good dispersing effect and is conducive to obtaining a uniformly dispersed casting slurry.

[0031] Optionally, the plasticizer is dibutyl phthalate and polyethylene glycol, or a mixture of both; and the binder is polyvinyl butyral.

[0032] In some embodiments of the present invention, the specific operation of preparing the casting slurry is: weigh the various raw materials of the casting slurry according to the mass ratio, then add the alumina powder to the solvent, and then add the dispersant and mix through a ball mill, the mixing time is 20-24h (for example, 20h, 21h, 22h, 23h, 24h and the interval between any two end points), then add the plasticizer and the binder, and continue mixing for 20-24h (for example, 20h, 21h, 22h, 23h, 24h and the interval between any two end points) to obtain the casting slurry, so that a uniformly dispersed casting slurry can be obtained.

[0033] In some embodiments of the present invention, sintering includes a first stage sintering and a second stage sintering, wherein the first stage sintering is a process of heating up first and then keeping warm, and the temperature after heating is 400-1000°C (such as 400°C, 500°C, 600°C, 700°C, 800°C, 900°C, 1000°C and the interval between any two end points), and the second stage sintering is a process of heating up first, keeping warm and then cooling down, and the temperature after heating is 1400-1750°C (such as 1400°C, 1450°C, 1500°C, 1550°C, 1600°C, 1650°C, 1700°C, 1750°C and the interval between any two end points). It should be noted that the second stage sintering is cooled to room temperature.

[0034] In the present invention, the first stage of sintering is degreasing sintering, and the temperature of degreasing sintering is controlled within the range of 400-1000°C, which can make the degreasing more thorough, avoid the gas products generated by the subsequent combustion of residual organic matter to cause internal voids or stratification, which is beneficial to reduce the warpage of the product and improve the product quality. The second stage of calcination is a process of product shrinkage and deformation. The sintering temperature of the second stage of sintering is controlled within the range of 1400-1750°C, which is beneficial to improve the yield rate of the sintered product.

[0035] In some embodiments of the present invention, the heating rate of the first stage sintering is controlled to be 0.1-3°C / min (such as 0.1°C / min, 0.5°C / min, 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min and any interval between the two end points), and the holding time is 4-6h (such as 4h, 5h, 6h and any interval between the two end points). This can make the degreasing more thorough and help improve the product yield.

[0036] In some embodiments of the present invention, the heating rate of the second stage sintering is controlled to be 0.1-4°C / min (for example, 0.1°C / min, 0.5°C / min, 1°C / min, 1.5°C / min, 2°C / min, 2.5°C / min, 3°C / min, 3.5°C / min, 4°C / min and the interval between any two end points), the cooling rate is 0.5-1°C / min (for example, 0.5°C / min, 0.6°C / min, 0.7°C / min, 0.8°C / min, 0.9°C / min, 1°C / min and the interval between any two end points), and the holding time is 2-4h (for example, 2h, 3h, 4h and the interval between any two end points). The present invention strictly controls the heating rate and cooling rate of the second stage sintering, which can effectively reduce the shrinkage and deformation of the product, reduce the warpage of the product, and improve the product yield; if the heating and cooling of the second stage sintering are too fast, it will cause internal stress concentration of the product, and then make the warpage of the obtained product relatively large, affecting the product quality; if the heating and cooling of the second stage sintering are too slow, it is not conducive to the shrinkage and deformation of the product, thereby affecting the product quality.

[0037] In some embodiments of the present invention, the air flow rate of the second stage sintering is controlled to be 1-5L / min (such as 1L / min, 2L / min, 3L / min, 4L / min, 5L / min and the interval between any two end points). The present invention strictly controls the air flow rate of the second stage sintering, effectively reduces the shrinkage and deformation of the product, reduces the warpage of the product, and improves the product yield; if the air flow rate is too large, the airflow will impact the product, thereby causing the warpage of the obtained product to be relatively large, affecting the product quality; if the air flow rate is too small, it is not conducive to the shrinkage and deformation of the product, thereby affecting the product quality.

[0038] It should be noted that air or nitrogen is introduced during both the first-stage sintering and the second-stage sintering.

[0039] In some embodiments of the present invention, tape casting specifically includes: tape casting the tape slurry into a green porcelain tape having a thickness ranging from 30 to 60 μm (eg, 30 μm, 40 μm, 50 μm, 60 μm and any interval between two end points).

[0040] In some embodiments of the present invention, the lamination is isostatic lamination, and the specific operation is: laminating the raw porcelain tape to the required thickness, and vacuumizing the lamination by isostatic pressing, and after vacuumizing, placing the laminated raw porcelain tape into an isostatic press for isostatic lamination, the temperature of the isostatic lamination is 50-80°C (such as 50°C, 60°C, 70°C, 80°C and the interval between any two end points), the pressure is 50-100MPa (such as 50MPa, 60MPa, 70MPa, 80MPa, 90MPa, 100MPa and the interval between any two end points), and the holding time is 5-20min (such as 5min, 10min, 15min, 20min and the interval between any two end points). The above-mentioned isostatic lamination operation is conducive to reducing the warpage of the product and improving the yield rate of the product.

[0041] Furthermore, in some embodiments of the present invention, the method for manufacturing a ceramic substrate also includes operations such as powder coating, debinding, correction and leveling, and size sorting, wherein the powder coating operation and the debinding operation are performed before the sintering operation, and the correction and leveling and size sorting operations are performed after the sintering operation. The operations of powder coating, debinding, correction and leveling, and size sorting are all conventional operations, and their specific operations can be referred to the existing technology, and will not be described one by one here.

[0042] The present invention also provides a ceramic substrate manufactured by the above-mentioned method for manufacturing a ceramic substrate. Due to the use of the method for manufacturing a ceramic substrate of the above-mentioned embodiment, the ceramic substrate provided by the present invention has a lower warpage and a higher product yield.

[0043] The method for manufacturing the ceramic substrate of the present invention is described in detail below through specific embodiments.

[0044] Example 1

[0045] (1) Preparation of tape casting slurry: The solid content of the tape casting slurry is 65wt%. First, weigh 1841.14g of high-purity nano-alumina powder (D50 value is 0.6um, powder purity is 99.98%), 5g of magnesium oxide, 3g of calcium oxide, 8g of silicon dioxide, 800g of solvent (including 560g of ethyl acetate and 240g of ethanol), 20g of dispersant (triolein), 100g of plasticizer (dibutyl phthalate), and 80g of binder (polyvinyl butyral); then add the alumina powder to the solvent, add the dispersant, and mix them in a ball mill for 24h, then add the plasticizer and binder, and continue mixing for 24h to obtain the tape casting slurry.

[0046] (2) Casting: The casting slurry obtained in step (1) is cast into a 60 μm thick green porcelain tape.

[0047] (3) Isostatic pressing and lamination: The green ceramic tape obtained in step (2) is laminated and the laminated layer is evacuated by isostatic pressing. After evacuation, the laminated green ceramic tape is placed in an isostatic press and isostatically laminated at a temperature of 60° C. and a pressure of 80 MPa for 10 min.

[0048] (4) First stage sintering: first increase the temperature to 500 °C at a heating rate of 0.2 °C / min, and then keep it at this temperature for 2 h.

[0049] (5) Second stage sintering: first, heat the sample to 1600 °C at a heating rate of 1 °C / min, then keep the temperature for 4 h, and then cool the sample to room temperature at a cooling rate of 1 °C / min. During the sintering process, the air flow rate was maintained at 5 L / min.

[0050] Example 2

[0051] The only difference between this embodiment and embodiment 1 is that the solid content of the casting slurry in step (1) is 70wt%, wherein the amount of high-purity nano-alumina powder is 2317.33g, and the amounts of other raw materials and other operations are the same as those in embodiment 1.

[0052] Example 3

[0053] The only difference between this embodiment and embodiment 2 is that the air intake flow rate in step (5) is 1 L / min, and the amount of raw materials and other operations are the same as those in embodiment 2.

[0054] Example 4

[0055] The only difference between this embodiment and embodiment 2 is that the heating rate in step (5) is 0.5°C / min, and the amount of raw materials and other operations are the same as those in embodiment 2.

[0056] Example 5

[0057] The only difference between this embodiment and embodiment 2 is that the cooling rate in step (5) is 0.5°C / min, and the amount of raw materials and other operations are the same as those in embodiment 2.

[0058] Comparative Example 1

[0059] The only difference between this comparative example and Example 1 is that the solid content of the casting slurry in step (1) is 50wt%, wherein the amount of high-purity nano-alumina powder is 984g, and the amounts of other raw materials and other operations are the same as those in Example 1.

[0060] Comparative Example 2

[0061] The only difference between this comparative example and Example 1 is that the solid content of the casting slurry in step (1) is 60wt%, of which the amount of high-purity nano alumina powder is 1484g, and the amounts of other raw materials and other operations are the same as in Example 1.

[0062] Comparative Example 3

[0063] The only difference between this comparative example and Example 3 is that the air intake flow rate in step (5) is 20 L / min, and the amount of raw materials and other operations are the same as those in Example 3.

[0064] Comparative Example 4

[0065] The only difference between this comparative example and Example 3 is that the air intake flow rate in step (5) is 50 L / min, and the amount of raw materials and other operations are the same as those in Example 3.

[0066] Comparative Example 5

[0067] The only difference between this comparative example and Example 4 is that the heating rate in step (5) is 4.5°C / min, and the amount of raw materials and other operations are the same as those in Example 4.

[0068] Comparative Example 6

[0069] The only difference between this comparative example and Example 4 is that the heating rate in step (5) is 5°C / min, and the amount of raw materials and other operations are the same as those in Example 4.

[0070] Comparative Example 7

[0071] The only difference between this comparative example and Example 5 is that the cooling rate in step (5) is 2°C / min, and the amount of raw materials and other operations are the same as those in Example 5.

[0072] Comparative Example 8

[0073] The only difference between this comparative example and Example 5 is that the cooling rate in step (5) is 3°C / min, and the amount of raw materials and other operations are the same as those in Example 5.

[0074] The warpage of the sintered products obtained in Examples 1-5 and Comparative Examples 1-8 was measured, and the results are shown in Table 1. It should be noted that the warpage was measured using a common measurement method, and based on the square structure of the substrate, the present invention uses the ratio of warpage < side length × 0.2% to characterize the warpage of the product.

[0075] Table 1 Warpage measurement results of sintered products obtained in Examples 1-5 and Comparative Examples 1-8

[0076] Warpage < side length × 0.2% of the proportion, % Example 1 100 Example 2 100 Example 3 100 Example 4 100 Example 5 100 Comparative Example 1 70 Comparative Example 2 88 Comparative Example 3 85 Comparative Example 4 55 Comparative Example 5 83 Comparative Example 6 48 Comparative Example 7 78 Comparative Example 8 55

[0077] It can be seen from the measurement results in Table 1 that when manufacturing a ceramic substrate, the present invention reasonably controls the solid content of the casting slurry (65-70wt%), improves the green density of the casting molding, effectively reduces the subsequent sintering shrinkage rate and deformation, and optimizes the air intake flow rate (1-5L / min), heating rate (0.1-4℃ / min) and cooling rate (0.5-1℃ / min) of the second stage sintering process to further reduce the product shrinkage rate and deformation, and can effectively reduce the warpage of the product, so that the warpage of the product after sintering The proportion of the side length × 0.2% reaches 100%, and the product sintering yield is high; and, there is no need for secondary re-firing, the production process is relatively simple, and the production cost is relatively low.

[0078] By comparing Example 1, Example 2, Comparative Example 1 and Comparative Example 2, it can be seen that the only difference is the solid content of the tape casting slurry, and the operations are the same. When the solid content of the tape casting slurry is lower than 65wt%, the warpage of the sintered product is relatively large. This is because the lower solid content of the tape casting slurry will lead to a lower green density of the tape casting, and then the subsequent sintering shrinkage and deformation are relatively large, and the warpage of the sintered product is relatively large. In addition, as the solid content of the tape casting slurry decreases, the warpage of the sintered product increases.

[0079] By comparing Example 3, Comparative Example 3 and Comparative Example 4, it can be seen that the only difference is the different air flow rate of the second stage sintering, and the raw materials and operations are the same. When the air flow rate of the second stage sintering is greater than 5L / min, the warpage of the sintered product is relatively large. This is because the air flow rate is relatively large during the second stage sintering, and the airflow will impact the product, resulting in a relatively large warpage of the product. In addition, as the air flow rate of the second stage sintering increases, the warpage of the sintered product increases.

[0080] By comparing Example 4, Comparative Example 5 and Comparative Example 6, it can be seen that the only difference is the heating rate of the second stage sintering. The raw materials and operations are the same. When the heating rate of the second stage sintering is greater than 4°C / min, the warpage of the sintered product is relatively large. This is because the heating rate of the second stage sintering is relatively fast, which will cause internal stress concentration in the product, thereby making the warpage of the product relatively large. In addition, as the heating rate of the second stage sintering increases, the warpage of the sintered product increases.

[0081] By comparing Example 5, Comparative Example 7 and Comparative Example 8, it can be seen that the only difference is the heating rate of the second stage sintering. The raw materials and operations are the same. When the cooling rate of the second stage sintering is greater than 1°C / min, the warpage of the sintered product is relatively large. This is because the cooling temperature of the second stage sintering is relatively fast, which will cause internal stress concentration in the product, thereby making the warpage of the product relatively large. In addition, as the cooling rate of the second stage sintering increases, the warpage of the sintered product increases.

[0082] It should be noted that, in this article, the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or system including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or system. In the absence of further restrictions, an element defined by the sentence "comprises a ..." does not exclude the existence of other identical elements in the process, method, article or system including the element.

[0083] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent articles or equivalent process changes made using the contents of the present invention specification, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A method for manufacturing a ceramic substrate, characterized in that: The production method comprises the following steps: Prepare a tape casting slurry, wherein the solid content of the tape casting slurry is 65-70wt%; The casting slurry is sequentially subjected to casting molding, lamination and sintering to obtain the ceramic substrate.

2. The method for manufacturing a ceramic substrate according to claim 1, wherein: The tape casting slurry includes the following raw materials in parts by mass: 40-60 parts of alumina powder, 0.1-1 parts of calcium oxide, 0.1-1 parts of magnesium oxide, 0.1-1 parts of silicon dioxide, 30-45 parts of solvent, 5-10 parts of plasticizer and 7-10 parts of binder.

3. The method for manufacturing a ceramic substrate according to claim 2, wherein: The purity of the aluminum oxide powder is 99-99.999%; and / or, The D50 value of the aluminum oxide powder is 0.5-1.0 μm.

4. The method for manufacturing a ceramic substrate according to claim 2, wherein: The solvent includes an ester and an alcohol, and the mass ratio of the ester to the alcohol is (1-3):(7-9), wherein the ester is at least one of ethyl acetate, methyl acetate, propyl acetate, and butyl acetate, and the alcohol is at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol, and isobutanol.

5. The method for manufacturing a ceramic substrate according to any one of claims 1 to 4, characterized in that: The sintering includes a first stage sintering and a second stage sintering. The first stage sintering is a process of heating up first and then keeping the temperature, and the temperature after heating is 400-1000°C. The second stage sintering is a process of heating up first, keeping the temperature, and then cooling down, and the temperature after heating is 1400-1750°C.

6. The method for manufacturing a ceramic substrate according to claim 5, characterized in that: The heating rate of the second stage sintering is 0.1-4°C / min, the cooling rate is 0.5-1°C / min, and the holding time is 2-4h.

7. The method for manufacturing a ceramic substrate according to claim 5, characterized in that: The air flow rate of the second stage sintering is 1-5 L / min.

8. The method for manufacturing a ceramic substrate according to claim 5, characterized in that: The heating rate of the first stage sintering is 0.1-3°C / min, and the holding time is 4-6h.

9. The method for manufacturing a ceramic substrate according to any one of claims 1 to 4, characterized in that: The laminate is an isostatically pressed laminate, the temperature of the isostatically pressed laminate is 50-80° C., the pressure is 50-100 MPa, and the pressure holding time is 5-20 min.

10. A ceramic substrate, characterized in that: The ceramic substrate is manufactured by the method for manufacturing a ceramic substrate according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Alumina ceramic slurry as well as preparation method and application thereof

    CN114292091A

  • High-purity ultrathin high-strength aluminum oxide ceramic substrate as well as preparation method and application thereof

    CN114538900A

  • Glue discharging method of electronic ceramic green body

    CN115259864A

  • Thermal shock resistant ceramic substrate and preparation method thereof

    CN115925399A

  • Method for manufacturing low temperature fired ceramics

    US4726921A

Cited By

  • Method for manufacturing laminated chip inductor element from low-temperature co-fired ferrite raw material belt

    CN119626753A

  • Low-warpage laminated sheet ceramic and anti-warpage preparation method of laminated sheet ceramic

    CN119874335A