Red spinel transparent ceramic material and preparation method thereof
By doping Cr, Fe, V, Zn, Ca, Mn, Cd, Zr into magnesium aluminum spinel, and performing ball milling, dry press forming, sintering and annealing treatment, the red spinel in the prior art is solved. The problem of difficulty in preparing was that bright red, rose-red, bright, soft and bright red spinel transparent ceramic materials suitable for artificial gemstones were successfully prepared.
Patent Information
- Application Number
- CN202411196715.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-29
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing synthetic red spinels are difficult to achieve bright red, rose-red, bright, soft and bright effects, because Cr ion-doped single crystals are difficult to prepare.
Using a red spinel transparent ceramic material, Cr, Fe, V, Zn, Ca, Mn, Cd, Zr is mixed into magnesium aluminum spinel according to weight ratio, and is formed by ball milling and dry pressing. The red-doped magnesium-aluminum spinel transparent ceramic was prepared by sintering and annealing treatment.
The obtained red-doped magnesium aluminum spinel transparent ceramic material has bright red, rose-red, bright, soft and bright properties, and is suitable for artificial gem materials.
Smart Images

Figure CN118993723A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of transparent ceramic preparation, and in particular relates to a red spinel transparent ceramic material and a preparation method thereof. Background Art
[0002] Although spinel has a variety of colors, red spinel is the most sought after. Compared with ruby, which has similar characteristics, red spinel is relatively rare, and spinel identified as gem-grade is even rarer. In addition, there are no independent mining areas and no mass production, so the price of high-quality spinel has been soaring, especially the "Jedi Knight" that has attracted much attention in recent years. It is bright red and rose red, bright, soft and bright. The gem is transparent. It has fluorescence, and the color is brighter and more vivid under strong light.
[0003] The existing artificial red spinel cannot achieve the above effect because the Cr ion-doped single crystal is difficult to prepare. The present invention intends to solve this problem by using the preparation technology of transparent ceramics. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the existing defects and provide a red spinel transparent ceramic material and a preparation method thereof to solve the problems raised in the above background technology.
[0005] To achieve the above-mentioned purpose, the present invention provides the following technical solutions: a red spinel transparent ceramic material and a preparation method thereof, specifically, mixing Cr, Fe, V, Zn, Ca, Mn, Cd, and Zr into magnesium-aluminum spinel according to a weight ratio.
[0006] A method for preparing a red spinel transparent ceramic material comprises the following steps:
[0007] Step 1. Weighing raw materials: spinel powder and Cr2O3, Fe, V, Zn, Ca, Mn, Cd, Zr;
[0008] Step 2, ball milling: use a ball mill to mix for 2 to 20 hours, the ball mill speed is 200 to 600 rpm, an agate pot or a polyurethane pot is selected, and the grinding balls are selected from alumina balls or zirconium balls. The ball milling medium is composed of a liquid medium and grinding balls, and the liquid medium is deionized water or alcohol;
[0009] Step 3, molding: drying and sieving the mixed slurry obtained in step 2 at 80-120° C. to obtain a powder; using a tablet press to perform dry pressing molding, using an axial unidirectional pressurization method during the dry pressing molding process, the pressure is 2-10 MPa, and the pressure holding time is 1-10 min to form a green blank; cold isostatic pressing molding, the pressure is 100-200 MPa, and the pressure holding time is 1-10 min to form a green blank;
[0010] Step 4: Sintering: Place the formed green blank in a corundum crucible, place the corundum crucible and the sample in an atmosphere furnace, and heat the temperature to 1500-1700°C at a heating rate of 1-10°C / min, and keep the temperature for 1-4 hours;
[0011] Step 5, hot isostatic pressing sintering: the green blank pre-sintered in step 4 is placed in a hot isostatic pressing sintering furnace for sintering at a sintering temperature of 1500-1750° C., a sintering time of 1-20 hours, and a sintering pressure of 20-60 MPa;
[0012] Step 6: Annealing: After hot pressing and sintering, demould and place the sample in a corundum crucible for annealing in an oxidizing environment at a temperature of 800 to 1200° C. for 1 to 10 hours.
[0013] Preferably, the additive in step 1 is one or a mixture of multiple doping elements of Cr, Fe, V, Zn, Ca, Mn, Cd, and Zr.
[0014] Preferably, the optimized doping concentration is: Cr2O3 (0-5%), Fe (0-2%), V (0-2%), Zn (0-2%), Ca (0-2%), Mn (0-2%), Cd (0-2%), and Zr (0-2%).
[0015] Preferably, in step 2, the mass ratio of raw material: ball: liquid medium is 1:5-20:1-20.
[0016] Compared with the prior art, the present invention provides a red spinel transparent ceramic material and a preparation method thereof, which have the following beneficial effects: the present invention provides a preparation method of Cr2O3 (0-5%), Fe (0-2%), V (0-2%), Zn (0-2%), Ca (0-2%), Mn (0-2%), Cd (0-2%), and Zr (0-2%) doped magnesium aluminum spinel transparent ceramics, and the obtained red doped magnesium aluminum spinel transparent ceramics are bright red, rose red, bright, soft and bright, and are very suitable for use as artificial gemstone materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0018] Figure 1 The process flow chart proposed by the present invention. DETAILED DESCRIPTION
[0019] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0020] See also Figure 1 The present invention provides a technical solution: a red spinel transparent ceramic material and a preparation method thereof, specifically, mixing Cr2O3, Fe2O3, V2O5, ZnO, CaO, MnO2, CdO, and ZrO2 into magnesium-aluminum spinel according to a weight ratio.
[0021] A method for preparing a red spinel transparent ceramic material comprises the following steps:
[0022] Step 1. Weighing raw materials: spinel powder and Cr2O3, Fe2O3, V2O5, ZnO, CaO, MnO2, CdO, ZrO2;
[0023] Step 2, ball milling: use a ball mill to mix for 2 to 20 hours, the ball mill speed is 200 to 600 rpm, a nylon tank or a polyurethane tank is used, and the grinding balls are alumina balls or zirconium balls. The ball milling medium is composed of a liquid medium and grinding balls, and the liquid medium is deionized water or alcohol;
[0024] Step 3, molding: drying and sieving the mixed slurry obtained in step 2 at 80-120° C. to obtain a powder; using a tablet press to perform dry pressing molding, using an axial unidirectional pressurization method during the dry pressing molding process, the pressure is 2-10 MPa, and the pressure holding time is 1-10 min to form a green blank; cold isostatic pressing molding, the pressure is 100-200 MPa, and the pressure holding time is 1-10 min to form a green blank;
[0025] Step 4: Sintering: Place the formed green blank in a corundum crucible, place the corundum crucible and the sample in an atmosphere furnace, and heat the temperature to 1500-1700°C at a heating rate of 1-10°C / min, and keep the temperature for 1-4 hours;
[0026] Step 5, hot isostatic pressing sintering: the green blank pre-sintered in step 4 is placed in a hot isostatic pressing sintering furnace for sintering at a sintering temperature of 1500-1750° C., a sintering time of 1-20 hours, and a sintering pressure of 20-60 MPa;
[0027] Step 6: Annealing: After hot pressing and sintering, demould and place the sample in a corundum crucible for annealing in an oxidizing environment at a temperature of 800 to 1200° C. for 1 to 10 hours.
[0028] In the present invention, preferably, the additive in step 1 is one or a mixture of multiple doping elements selected from the group consisting of Cr2O3, Fe2O3, V2O5, ZnO, CaO, MnO2, CdO, and ZrO2.
[0029] In the present invention, the preferred and optimized doping concentrations are: Cr2O3 (0-5%), Fe2O3 (0-2%), V2O5 (0-2%), ZnO (0-2%), CaO (0-2%), MnO2 (0-2%), CdO (0-2%), and ZrO2 (0-2%).
[0030] In the present invention, preferably, in step 2, the mass ratio of raw material: ball: liquid medium is 1:5-20:1-20.
[0031] Embodiment 1
[0032] A red spinel transparent ceramic material and a preparation method thereof, specifically comprising mixing Cr2O3, Fe2O3, V2O5, ZnO, CaO, MnO2, CdO and ZrO2 into magnesium-aluminum spinel according to a weight ratio.
[0033] A method for preparing a red spinel transparent ceramic material comprises the following steps:
[0034] Step 1. Weighing raw materials: spinel powder and Cr2O3, Fe2O3, V2O5, ZnO, CaO, MnO2, CdO, ZrO2;
[0035] Step 2, ball milling: use a ball mill to mix for 2 to 20 hours, the ball mill speed is 200 to 600 rpm, a nylon tank or a polyurethane tank is used, and the grinding balls are alumina balls or zirconium balls. The ball milling medium is composed of a liquid medium and grinding balls, and the liquid medium is deionized water or alcohol;
[0036] Step 3, molding: drying and sieving the mixed slurry obtained in step 2 at 80-120° C. to obtain a powder; using a tablet press to perform dry pressing molding, using an axial unidirectional pressurization method during the dry pressing molding process, the pressure is 2-10 MPa, and the pressure holding time is 1-10 min to form a green blank; cold isostatic pressing molding, the pressure is 100-200 MPa, and the pressure holding time is 1-10 min to form a green blank;
[0037] Step 4: Sintering: Place the formed green blank in a corundum crucible, place the corundum crucible and the sample in an atmosphere furnace, and heat the temperature to 1500-1700°C at a heating rate of 1-10°C / min, and keep the temperature for 1-4 hours;
[0038] Step 5, hot isostatic pressing sintering: the green blank pre-sintered in step 4 is placed in a hot isostatic pressing sintering furnace for sintering at a sintering temperature of 1500-1750° C., a sintering time of 1-20 hours, and a sintering pressure of 20-60 MPa;
[0039] Step 6: Annealing: After hot pressing and sintering, demould and place the sample in a corundum crucible for annealing in an oxidizing environment at a temperature of 800 to 1200° C. for 1 to 10 hours.
[0040] In the present invention, preferably, the additive in step 1 is one or a mixture of multiple doping elements selected from the group consisting of Cr2O3, Fe2O3, V2O5, ZnO, CaO, MnO2, CdO, and ZrO2.
[0041] In the present invention, preferably, the optimized doping concentration is: Cr2O3 (1%), Fe (1%), V (1%), Zn (1%), Ca (1%), Mn (1%), Cd (1%), and Zr (1%).
[0042] In the present invention, preferably, in step 2, the mass ratio of raw material: ball: liquid medium is 1:5-20:1-20.
[0043] Embodiment 2
[0044] A red spinel transparent ceramic material and a preparation method thereof, specifically comprising mixing Cr2O3, Fe2O3, V2O5, ZnO, CaO, MnO2, CdO and ZrO2 into magnesium-aluminum spinel according to a weight ratio.
[0045] A method for preparing a red spinel transparent ceramic material comprises the following steps:
[0046] Step 1. Weighing raw materials: spinel powder and Cr2O3, Fe2O3, V2O5, ZnO, CaO, MnO2, CdO, ZrO2
[0047] Step 2, ball milling: use a ball mill to mix for 2 to 20 hours, the ball mill speed is 200 to 600 rpm, a nylon tank or a polyurethane tank is used, and the grinding balls are alumina balls or zirconium balls. The ball milling medium is composed of a liquid medium and grinding balls, and the liquid medium is deionized water or alcohol;
[0048] Step 3, molding: drying and sieving the mixed slurry obtained in step 2 at 80-120° C. to obtain a powder; using a tablet press to perform dry pressing molding, using an axial unidirectional pressurization method during the dry pressing molding process, the pressure is 2-10 MPa, and the pressure holding time is 1-10 min to form a green blank; cold isostatic pressing molding, the pressure is 100-200 MPa, and the pressure holding time is 1-10 min to form a green blank;
[0049] Step 4: Sintering: Place the formed green blank in a corundum crucible, place the corundum crucible and the sample in an atmosphere furnace, and heat the temperature to 1500-1700°C at a heating rate of 1-10°C / min, and keep the temperature for 1-4 hours;
[0050] Step 5, hot isostatic pressing sintering: the green blank pre-sintered in step 4 is placed in a hot isostatic pressing sintering furnace for sintering at a sintering temperature of 1500-1750° C., a sintering time of 1-20 hours, and a sintering pressure of 20-60 MPa;
[0051] Step 6: Annealing: After hot pressing and sintering, demould and place the sample in a corundum crucible for annealing in an oxidizing environment at a temperature of 800 to 1200° C. for 1 to 10 hours.
[0052] In the present invention, preferably, the additive in step 1 is Cr2O3, Fe2O3, V2O5, ZnO, CaO, MnO2, CdO, ZrO2
[0053] A mixture of one or more doping elements.
[0054] In the present invention, preferably, the optimized doping concentration is: Cr2O3 (2%), Fe (2%), V (2%), Zn (2%), Ca (2%), Mn (2%), Cd (2%), and Zr (2%).
[0055] In the present invention, preferably, in step 2, the mass ratio of raw material: ball: liquid medium is 1:5-20:1-20.
[0056] (reference group)
[0057] A method for preparing a red spinel transparent ceramic material comprises the following steps:
[0058] Step 1. Weighing raw materials: 100 g spinel powder, 0.2856 g Cr2O3 powder and sintering aid;
[0059] Step 2: ball milling: put the powder weighed in step (1) into a nylon ball mill, add 72 g of zirconium balls and 36 g of anhydrous ethanol, and then grind for 3 h to obtain a slurry;
[0060] Step 3, dry pressing: After ball milling, the slurry is dried at 100°C, and dry pressed by a tablet press. A pressure of 8MPa is applied to the axial direction, and the pressure is maintained for 8 minutes to form a φ24mm disc to obtain a green embryo;
[0061] Step 4, sintering: put the product of step (3) into a corundum crucible and put it into an atmosphere furnace, raise the temperature to 1650°C at a heating rate of 4°C / min, and keep it at that temperature for 3h;
[0062] Step 5, hot isostatic pressing sintering: the sintered product is placed in a hot isostatic pressing sintering furnace for sintering, firstly heating up to 1750°C at a heating rate of 17°C / min, then keeping the temperature for 6 hours, and the sintering pressure is 200Mpa;
[0063] Step 6: Annealing: After hot isostatic pressing, place the sample in a corundum crucible for annealing in an oxidizing environment at a temperature of 1000°C for 8 hours.
[0064] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A red spinel transparent ceramic material and a preparation method thereof, characterized in that: Specifically, Cr, Fe, V, Zn, Ca, Mn, Cd, and Zr are mixed into magnesium-aluminum spinel according to weight proportions.
2. The method for preparing a red spinel transparent ceramic material according to claim 1, characterized in that: The following steps are involved: Step 1. Weighing raw materials: spinel powder and Cr2O3, Fe, V, Zn, Ca, Mn, Cd, Zr; Step 2, ball milling: using a ball mill for mixing for 2 to 20 hours, the ball mill speed is 200 to 600 rpm, an agate tank or a polyurethane tank is selected, and the grinding balls are agate balls or zirconium balls. The ball milling medium is composed of a liquid medium and grinding balls, and the liquid medium is deionized water or alcohol; Step 3, molding: drying and sieving the mixed slurry obtained in step 2 at 80-120° C. to obtain a powder; using a tablet press to perform dry pressing molding, using an axial unidirectional pressurization method during the dry pressing molding process, the pressure is 2-10 MPa, and the pressure holding time is 1-10 min to form a green blank; cold isostatic pressing molding, the pressure is 100-200 MPa, and the pressure holding time is 1-10 min to form a green blank; Step 4: Sintering: Place the formed green blank in a corundum crucible, place the corundum crucible and the sample in an atmosphere furnace, and heat the temperature to 1500-1700°C at a heating rate of 1-10°C / min, and keep the temperature for 1-4h; Step 5, hot isostatic pressing sintering: the green blank pre-sintered in step 4 is placed in a hot isostatic pressing sintering furnace for sintering at a sintering temperature of 1500-1750° C., a sintering time of 1-20 hours, and a sintering pressure of 100-200 MPa; Step 6: Annealing: After hot pressing and sintering, demould and place the sample in a corundum crucible for annealing in an oxidizing environment at a temperature of 800 to 1200° C. for 1 to 10 hours.
3. The method for preparing a red spinel transparent ceramic material according to claim 2, characterized in that: In the step 1, the additive is one or a mixture of multiple doping elements of Cr, Fe, V, Zn, Ca, Mn, Cd, and Zr.
4. The method for preparing a red spinel transparent ceramic material according to claim 3, characterized in that: The optimized doping concentrations are: Cr2O3 (0-5%), Fe (0-2%), V (0-2%), Zn (0-2%), Ca (0-2%), Mn (0-2%), Cd (0-2%), and Zr (0-2%).
5. The method for preparing a red spinel transparent ceramic material according to claim 2, characterized in that: In the step 2, the mass ratio of raw material: ball: liquid medium is 1:5-20:1-20.