Preparation method of beta ''-alumina ceramic based on gel casting
Patent Information
- Application Number
- CN202411267335.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-11
AI Technical Summary
[0003]然而,现有的β"-氧化铝陶瓷在β"含量、生坯加工能力、烧结后体积密度以及力学性能方面均存在一定的缺点
[0023] This application provides a method for preparing β"-alumina ceramics based on gel injection molding, which includes: obtaining β"-alumina ceramic precursor powder with a set β" phase content; The coupling agent is added to the solvent, and then the first ball milling is performed to obtain a premixed liquid; the β"-alumina ceramic precursor powder is and dispersant are added to the premixed liquid, and then the second ball milling is performed to obtain the first slurry; the first slurry is vacuum degassed to obtain the second slurry; and the second slurry is added initiator, and then perform a third ball milling to obtain a third slurry; place the third slurry into a mold for solidification, and then demould, Obtain a blank; and debind and sinter the blank to obtain β"-alumina ceramics. This application rationally designs the process parameters of the preparation method of β"-alumina ceramics, through a multi-stage ball milling process, combined with a dispersant The addition of effectively improves the dispersion and uniformity of ceramic powder in the solvent; vacuum degassing can The bubbles in the slurry are effectively removed, further improving the fluidity of the slurry; by adding an initiator to the slurry and controlling the curing temperature and holding time, the chemical reaction between the monomer and the cross-linking agent can be fully It proceeds to form a stable three-dimensional gel network structure, which helps ensure the uniformity of curing and the strength of the green body. In the debinding and sintering stages, through reasonable process control, impurities and defects in ceramics can be further reduced and the sintering quality improved. Thereby improving the comprehensive performance of β"-alumina ceramics.
Smart Images

Figure CN119038964A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of inorganic non-metallic materials, and in particular to a method for preparing β"-alumina ceramics based on gel injection molding. Background Art
[0002] β" alumina ceramics are used as solid electrolyte materials for sodium-sulfur / nickel batteries due to their excellent sodium ion conductivity. They are the most important core components in solid-state battery systems. They have a crystal structure composed of overlapping aluminum-oxygen blocks and sodium-oxygen layers. Al3+ ions are in the most densely packed form in the gaps of the tetrahedron composed of oxygen ions. These densely packed layers are separated by sparse [NaO] - The Al-O-Al chain is linked together, so Na ions can shuttle between dense layers at high temperatures. When the temperature reaches above 250°C, β" alumina ceramics have an ionic conductivity close to that of aqueous salts, making them the preferred solid electrolyte for many sodium-based batteries (sodium-sulfur batteries and Zebra batteries, etc.).
[0003] However, existing β"-alumina ceramics have certain shortcomings in terms of β" content, green body processing ability, volume density after sintering, and mechanical properties. Therefore, how to improve the comprehensive performance of β"-alumina ceramics is a technical problem that needs to be solved urgently. Summary of the invention
[0004] The present application provides a preparation method of β"-alumina ceramics based on gel injection molding to solve the following technical problem: how to improve the comprehensive performance of β"-alumina ceramics.
[0005] The present application provides a method for preparing β"-alumina ceramics based on gel casting molding, the method comprising:
[0006] Obtaining a β"-alumina ceramic precursor powder having a set β" phase content;
[0007] The monomer and the cross-linking agent are added to the solvent, and then the first ball milling is performed to obtain a premixed solution;
[0008] Adding the β"-alumina ceramic precursor powder and the dispersant to the premixed liquid, and then performing a second ball milling to obtain a first slurry;
[0009] Vacuum degassing the first slurry to obtain a second slurry;
[0010] adding an initiator to the second slurry, and then performing a third ball milling to obtain a third slurry;
[0011] Placing the third slurry into a mold for solidification, and then demolding to obtain a green blank; and
[0012] The green blank is subjected to debinding and sintering to obtain β"-alumina ceramics.
[0013] Optionally, the β" phase content is set to be ≥95%.
[0014] Optionally, the mass concentration of the premix is 10% to 20%, wherein the mass ratio of the monomer to the cross-linking agent is (4 to 6):1, the monomer includes: one or more of methacrylamide, acrylamide and hydroxymethyl acrylamide, and the cross-linking agent includes N,N'-methylenebisacrylamide.
[0015] Optionally, the mass of the dispersant accounts for 0.1% to 0.3% of the mass of the β"-alumina ceramic precursor powder, and the dispersant includes one or more of sodium polymethacrylate, sodium hexametaphosphate and sodium polyacrylate.
[0016] Optionally, the mass ratio of the β"-alumina ceramic precursor powder to the premixed liquid is (1-2.3):1, and the solid content of the first slurry is 50%-70%; the ball-to-material ratio of the second ball milling is (3-5):1, and the time of the second ball milling is 10h-15h.
[0017] Optionally, the mass of the initiator accounts for 10% to 12% of the mass of the monomer, and the initiator includes: one or more of ammonium persulfate and sodium persulfate.
[0018] Optionally, the curing temperature is 80° C. to 100° C., and the curing insulation time is 10 h to 15 h.
[0019] Optionally, the temperature of the debinding is 500° C. to 600° C., and the insulation time of the debinding is 1.5 h to 2.5 h.
[0020] Optionally, the sintering temperature is 1600° C. to 1650° C., and the sintering holding time is 20 min to 40 min.
[0021] Optionally, the β"-alumina ceramic meets at least one of the following properties: β" content ≥ 95%, volume density reaches more than 96% of the theoretical volume density, and four-point bending strength ≥ 250MP.
[0022] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0023] The present application provides a preparation method of β"-alumina ceramics based on gel casting, comprising: obtaining a β"-alumina ceramic precursor powder with a set β" phase content; adding a monomer and a cross-linking agent to a solvent, and then performing a first ball milling to obtain a premixed liquid; adding the β"-alumina ceramic precursor powder and a dispersant to the premixed liquid, and then performing a second ball milling to obtain a first slurry; vacuum degassing the first slurry to obtain a second slurry; adding an initiator to the second slurry, and then performing a third ball milling to obtain a third slurry; placing the third slurry in a mold for curing, and then demolding. A green blank is obtained; and the green blank is debinded and sintered to obtain β"-alumina ceramics. The present application rationally designs the process parameters of the preparation method of β"-alumina ceramics, and effectively improves the dispersibility and uniformity of the ceramic powder in the solvent through a multi-stage ball milling process combined with the addition of a dispersant; effectively removes bubbles in the slurry through vacuum degassing, further improving the fluidity of the slurry; and allows the chemical reaction between the monomer and the cross-linking agent to fully proceed by adding an initiator to the slurry and controlling the curing temperature and insulation time, thereby forming a stable three-dimensional gel network structure, which helps to ensure the uniformity of curing and the strength of the blank. In the debinding and sintering stages, reasonable process control can further reduce impurities and defects in the ceramic and improve the sintering quality. Thereby improving the comprehensive performance of β"-alumina ceramics. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0025] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0026] Figure 1 A schematic diagram of a process for preparing β"-alumina ceramics based on gel casting provided in an embodiment of the present application. DETAILED DESCRIPTION
[0027] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0028] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0029] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b and c", can both mean: a, b, c, ab (i.e. a and b), ac, bc or abc, where a, b, c can be single or plural, respectively.
[0030] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0031] The creative ideas of this application are:
[0032] Gel casting is an advanced ceramic molding process. It combines the principle of polymer chemical reaction, mixes ceramic powder, organic monomer, cross-linking agent, initiator and catalyst into slurry, and then injects it into the mold. Through temperature induction, the organic monomer undergoes polymerization reaction to form a three-dimensional network structure of gel, and then the ceramic powder is solidified in situ to form a ceramic body. Gel casting has the advantages of good body uniformity, high strength, direct mechanical processing, no need for expensive equipment in the whole process, and no special requirements for the mold.
[0033] Developing a low-cost, high-β-phase content β-alumina ceramic preparation technology by gel casting is an effective means to improve the comprehensive properties of β-alumina ceramics. However, applying gel casting to the preparation of β-alumina ceramics requires overcoming the following difficulties:
[0034] 1. Slurry preparation and solid content control
[0035] Balance between solid content and performance: The solid content of the slurry is a key factor affecting the performance of the formed green body. A higher solid content helps to improve the density and strength of the green body, but too high a solid content will increase the viscosity of the slurry, making it difficult to flow and inject into the mold, and may also cause performance degradation after sintering, such as coarse grains and reduced strength. Therefore, the solid content of the slurry needs to be precisely controlled to find the best balance between performance and processability.
[0036] Selection and dosage of dispersants: In order to reduce the viscosity of the slurry and improve fluidity, dispersants are usually added. However, the selection and dosage of dispersants need to be strictly controlled to avoid adverse effects on the surface properties of the ceramic powder and the performance of the green body after molding.
[0037] 2. Gelation process control
[0038] Polymerization reaction rate: The gelation process is a process of temperature-induced polymerization of monomers to form a three-dimensional network structure. The reaction rate needs to be precisely controlled to ensure that the gel has sufficient strength and stability, while avoiding problems caused by too fast or too slow reactions, such as excessive brittleness or insufficient strength of the gel.
[0039] Bubble removal: During the gelation process, the presence of bubbles will seriously affect the quality and performance of the green body. Therefore, effective measures need to be taken to remove the bubbles in the slurry to ensure the density and uniformity of the formed green body.
[0040] 3. Sintering process optimization
[0041] Sintering temperature and time: The sintering temperature and time of β"-alumina ceramics have an important influence on the performance of the finished product. The sintering process parameters need to be optimized to ensure that the ceramic material has excellent mechanical properties and thermal stability.
[0042] Figure 1 A schematic diagram of a process for preparing β"-alumina ceramics based on gel casting provided in an embodiment of the present application.
[0043] See also Figure 1 In order to solve the above technical problems, the present application provides a preparation method of β"-alumina ceramics based on gel casting molding, the method comprising:
[0044] S1, obtaining a β"-alumina ceramic precursor powder having a set β" phase content;
[0045] In some embodiments, the β" phase content is set to be ≥95%.
[0046] A high β" phase content means that the ceramic material will have better properties, such as higher strength, better thermal stability and superior electrical properties. The β" phase content of the β"-alumina ceramic precursor powder is limited to ≥95%, which helps the β" phase content of the β"-alumina ceramic to be ≥95%. Exemplarily, the β" phase content of the β"-alumina ceramic precursor powder can be 95%, 96%, 97%, 98%, 99%, etc.
[0047] S2, adding the monomer and the cross-linking agent into the solvent, and then performing the first ball milling to obtain a premixed solution;
[0048] Monomers and cross-linkers are key components for forming gel networks, and they are dissolved in a solvent to form a homogenous premix. The first ball milling process helps promote the homogenous mixing of these components, laying the foundation for subsequent steps.
[0049] In some embodiments, the mass concentration of the premix is 10% to 20%, wherein the mass ratio of the monomer to the cross-linking agent is (4 to 6):1, the monomer includes: one or more of methacrylamide, acrylamide and hydroxymethyl acrylamide, and the cross-linking agent includes N,N'-methylenebisacrylamide.
[0050] The mass concentration of the premix is an important parameter, which directly affects the uniformity, fluidity and performance of the subsequent slurry. The mass concentration of the premix is limited to 10% to 20%, and the monomer and cross-linking agent can be fully dissolved in the solvent and mixed evenly. Good solubility ensures that they can be evenly distributed throughout the premix, providing a good foundation for subsequent reactions with other components (such as ceramic precursor powders). At the same time, it helps the uniformity of polymerization and cross-linking and the fluidity and stability of the slurry, avoiding uneven local reactions. Exemplarily, the mass concentration of the premix can be 10%, 12%, 14%, 16%, 18%, 20%, etc.
[0051] In the gel casting process, the mass ratio of monomer to cross-linking agent is a crucial parameter, which directly affects the rate of gelation reaction and the formation of three-dimensional gel network structure. By setting the mass ratio of monomer to cross-linking agent in the range of (4-6):1, the curing rate can be controlled within a certain range, so that the reaction is neither too rapid to cause local agglomeration and stress concentration, nor too slow to cause low production efficiency, thereby helping to form a uniform, dense and stable three-dimensional gel network structure and ensure the strength of the green body. Exemplarily, the mass ratio of monomer to the cross-linking agent can be 4:1, 4.5:1, 5:1, 5.5:1, 6:1, etc.
[0052] S3, adding the β"-alumina ceramic precursor powder and the dispersant to the premixed liquid, and then performing a second ball milling to obtain a first slurry;
[0053] The ceramic precursor powder and dispersant are added to the premixed liquid, and they are fully mixed and evenly dispersed in the solvent through the second ball milling process. The addition of the dispersant helps to reduce the agglomeration between the powder particles and improve the uniformity and fluidity of the slurry.
[0054] In some embodiments, the mass of the dispersant accounts for 0.1% to 0.3% of the mass of the β"-alumina ceramic precursor powder, and the dispersant includes one or more of sodium polymethacrylate, sodium hexametaphosphate and sodium polyacrylate.
[0055] The main function of the dispersant is to adsorb on the surface of the ceramic powder particles, and prevent the agglomeration of particles through electrostatic repulsion or steric hindrance effect, thereby improving the dispersibility of the powder in the solvent. The amount of dispersant added is crucial to ensure the good dispersibility of the β"-alumina ceramic precursor powder in the solvent, as well as the stability and fluidity of the final slurry. Controlling the mass of the dispersant within the range of 0.1% to 0.3% of the mass of the β"-alumina ceramic precursor powder helps to form a stable slurry system and improve the fluidity of the slurry. However, excessive dispersant will aggregate itself or form a micellar structure, which will increase the viscosity of the system. Exemplarily, the mass of the dispersant can account for 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, etc. of the mass of the β"-alumina ceramic precursor powder.
[0056] In some embodiments, the mass ratio of the β"-alumina ceramic precursor powder to the premixed liquid is (1-2.3):1, and the solid content of the first slurry is 50%-70%; the ball-to-material ratio of the second ball milling is (3-5):1, and the time of the second ball milling is 10h-15h.
[0057] The mass ratio of β"-alumina ceramic precursor powder to the premix is a key process parameter, which directly affects the strength of the green body and the density and microstructure of the sintered product. Setting this ratio within the range of (1 to 2.3):1 helps to improve the strength of the green body, improve the sintering density and microstructure after sintering, avoid defect formation, and also helps to improve the controllability and stability of the process. Exemplarily, the mass ratio of β"-alumina ceramic precursor powder to the premix can be 1:1, 1.2:1, 1.5:1, 1.8:1, 2:1, 2.3:1, etc.
[0058] Limiting the solid content of the first slurry to 50% to 70% can reduce shrinkage and deformation after drying, help improve the strength of the green body, and improve the sintering density and microstructure after sintering. Exemplarily, the solid content of the first slurry can be 50%, 55%, 60%, 65%, 70%, etc.
[0059] The ball-to-material ratio of the second ball milling is limited to (3-5):1, and the second ball milling time is 10h-15h, which can improve the grinding efficiency and help the uniformity of the slurry. Exemplarily, the ball-to-material ratio of the second ball milling is 3:1, 3.5:1, 4:1, 4.5:1, 5:1, etc., and the second ball milling time can be 10h, 11h, 12h, 13h, 14h, 15h, etc.
[0060] S4, vacuum degassing the first slurry to obtain a second slurry;
[0061] The slurry may contain bubbles, which may cause defects inside the green body during the molding process. Therefore, it is necessary to remove the bubbles through a vacuum degassing process to obtain a second slurry without bubbles.
[0062] S5, adding an initiator to the second slurry, and then performing a third ball milling to obtain a third slurry;
[0063] The addition of initiator is the key step to start the gelation reaction. The third ball milling process makes the initiator evenly dispersed in the slurry, preparing for the subsequent curing process.
[0064] In some embodiments, the mass of the initiator accounts for 10% to 12% of the mass of the monomer, and the initiator includes: one or more of ammonium persulfate and sodium persulfate.
[0065] The mass of the initiator is limited to 10% to 12% of the mass of the monomer, which can effectively initiate the polymerization reaction and regulate the reaction rate so as to leave sufficient time for subsequent injection molding. For example, the mass of the initiator accounts for 10%, 10.5%, 11%, 11.5%, 12% of the mass of the monomer, etc.
[0066] S6, placing the third slurry into a mold for solidification, and then demolding to obtain a green blank; and
[0067] The slurry containing the initiator is injected into the mold, and the monomer is polymerized by controlling the temperature and time to form a gel with a three-dimensional network structure, thereby solidifying the ceramic powder in situ to form a green blank. After the solidification is completed, the demoulding operation is performed to obtain a complete green blank.
[0068] In some embodiments, the curing temperature is 80° C. to 100° C., and the curing insulation time is 10 h to 15 h.
[0069] The curing temperature and holding time are key factors to ensure that the chemical reaction between the monomer and the crosslinker is fully carried out and a stable three-dimensional gel network structure is formed. The curing temperature is limited to 80°C to 100°C, the curing holding time is 10h to 15h, and the chemical reaction rate between the monomer and the crosslinker is moderate. Too low a temperature will result in a slow reaction rate and a longer time to complete the curing; while too high a temperature may cause unnecessary side reactions and affect the structure and performance of the gel network. At the same time, it can ensure that the monomers and crosslinkers in the entire slurry system can fully react to form a uniform gel network. In addition, by controlling the curing temperature and holding time, the gel network can be gradually shrunk and densified during the formation process, thereby reducing the risk of stress concentration. Exemplarily, the curing temperature can be 80°C, 85°C, 90°C, 95°C, 100°C, etc., and the curing holding time can be 10h, 11h, 12h, 13h, 14h, 15h, etc.
[0070] Ensure that the chemical reaction between the monomer and the cross-linker is sufficient to ensure uniform curing.
[0071] S7, debinding and sintering the green blank to obtain β"-alumina ceramic.
[0072] The green body contains a certain amount of organic matter (such as monomers, cross-linking agents, dispersants, etc.), which needs to be removed through the debinding process before sintering. After debinding, sintering is carried out to form a dense bond between the ceramic particles, and obtain β"-alumina ceramics with excellent performance.
[0073] In some embodiments, the debinding temperature is 500° C. to 600° C., and the debinding holding time is 1.5 h to 2.5 h.
[0074] The temperature of debinding is limited to 500℃~600℃, and the holding time of debinding is 1.5h~2.5h, which can effectively and completely remove organic matter and avoid discharge at high temperature, which will cause pores on the ceramic surface and affect the ceramic performance. For example, the temperature of debinding can be 500℃, 520℃, 540℃, 560℃, 580℃, 600℃, etc., and the holding time of debinding can be 1.5h, 1.7h, 1.9h, 2.0h, 2.2h, 2.4h, 2.5h, etc.
[0075] In some embodiments, the sintering temperature is 1600° C. to 1650° C., and the sintering holding time is 20 min to 40 min.
[0076] The sintering temperature is limited to 1600°C to 1650°C, and the sintering holding time is 20min to 40min, which helps to achieve the best density of the ceramic and uniform microstructure. Too low temperature leads to low density of the ceramic, and too high temperature leads to abnormal growth of ceramic grains. Exemplarily, the sintering temperature can be 1600°C, 1610°C, 1620°C, 1630°C, 1640°C, 1650°C, etc., and the sintering holding time can be 20min, 22min, 25min, 30min, 35min, 40min, etc.
[0077] In some embodiments, the β"-alumina ceramic meets at least one of the following properties: β" content ≥ 95%, volume density reaches more than 96% of the theoretical volume density, and four-point bending strength ≥ 250MP.
[0078] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.
[0079] Example 1
[0080] This embodiment provides a method for preparing β"-alumina ceramics based on gel casting, comprising the following steps:
[0081] S11, preparing a β"-alumina ceramic precursor powder having a β" phase content of 98% by a solid phase synthesis method;
[0082] S21, adding 4 parts of methacrylamide (C4H7NO) and 1 part of N'-methylenebisacrylamide (linear molecular formula: CH2=CHCONH)2CH2) to 28.5 parts of water, and then performing a first ball milling for 15 minutes to obtain a uniformly mixed premixed solution;
[0083] S31, adding 30 parts of β"-alumina ceramic precursor powder and 0.003 parts of sodium polyacrylate dispersant (CAS No.: 9003-04-7) to the premixed liquid, and then performing a second ball milling with a ball-to-material ratio of 3:1 and a grinding time of 12 hours to obtain a first slurry;
[0084] S41, vacuum degassing the first slurry to obtain a second slurry;
[0085] S51, adding 0.4 parts of initiator ammonium persulfate ((NH4)2S2O8) to the second slurry, and then performing a third ball milling for 15 minutes to obtain a third slurry;
[0086] S61, placing the third slurry into a mold, placing it in a 90° C. oven for 12 hours to solidify, and then demolding to obtain a green blank, the green blank strength of which reaches 15 MPa; and
[0087] S71, debinding the green blank at 500°C for 2 hours, and sintering at 1600°C for 2 hours to obtain β"-alumina ceramic. The β" content of the β"-alumina ceramic is ≥95%, and the sintered volume density is 3.216 g / cm 3 , reaching 98.95% of the theoretical volume density, and the four-point bending strength is 286MPa.
[0088] Example 2
[0089] This embodiment provides a method for preparing β"-alumina ceramics based on gel casting, comprising the following steps:
[0090] S11, preparing a β"-alumina ceramic precursor powder having a β" phase content of 98% by a solid phase synthesis method;
[0091] S21, adding 10 parts of methacrylamide (C4H7NO) and 2 parts of N'-methylenebisacrylamide (linear molecular formula: CH2=CHCONH)2CH2) to 108 parts of water, and then performing a first ball milling for 15 minutes to obtain a uniformly mixed premixed solution;
[0092] S31, adding 160 parts of β"-alumina ceramic precursor powder and 0.32 parts of sodium polyacrylate dispersant (CAS No.: 9003-04-7) to the premixed liquid, and then performing a second ball milling with a ball-to-material ratio of 3:1 and a grinding time of 12 hours to obtain a first slurry;
[0093] S41, vacuum degassing the first slurry to obtain a second slurry;
[0094] S51, adding 1.1 parts of initiator ammonium persulfate ((NH4)2S2O8) to the second slurry, and then performing a third ball milling for 15 minutes to obtain a third slurry;
[0095] S61, placing the third slurry into a mold, placing it in a 90° C. oven for 12 hours to solidify, and then demolding to obtain a green blank, the green blank strength of which reaches 15 MPa; and
[0096] S71, debinding the green blank at 500°C for 2 hours, and sintering it at 1600°C for 2 hours to obtain β"-alumina ceramics. The β" content of β"-alumina ceramics is ≥95%, and the sintered volume density of the ceramics is 3.184 g / cm 3 , reaching 97.97% of the theoretical volume density, and the four-point bending strength is 268MPa.
[0097] Example 3
[0098] This embodiment provides a method for preparing β"-alumina ceramics based on gel casting, comprising the following steps:
[0099] S11, preparing a β"-alumina ceramic precursor powder having a β" phase content of 98% by a solid phase synthesis method;
[0100] S21, add 12 parts of methacrylamide (C4H7NO), 2 parts of N'-methylenebisacrylamide (linear molecular formula: CH2=CHCONH)2CH2) to 80 parts of water, and then perform the first ball milling for 15 minutes to obtain a uniformly mixed premixed solution; wherein,
[0101] S31, adding 135 parts of β"-alumina ceramic precursor powder and 0.4 parts of sodium polyacrylate dispersant (CAS No.: 9003-04-7) to the premixed solution, and then performing a second ball milling with a ball-to-material ratio of 5:1 and a grinding time of 12 hours to obtain a first slurry;
[0102] S41, vacuum degassing the first slurry to obtain a second slurry;
[0103] S51, adding 1.44 parts of initiator ammonium persulfate ((NH4)2S2O8) to the second slurry, and then performing a third ball milling for 15 minutes to obtain a third slurry;
[0104] S61, placing the third slurry into a mold, placing it in an oven at 80° C. for 12 hours for curing, and then demolding to obtain a green blank, the green blank strength of which reaches 23 MPa; and
[0105] S71, debinding the green blank at 500°C for 2 hours, and sintering at 1620°C for 2 hours to obtain β"-alumina ceramic. The β" content of the β"-alumina ceramic is ≥95%, and the sintered bulk density is 3.208 g / cm 3 , reaching 98.71% of the theoretical volume density, and the four-point bending strength is 274MPa.
[0106] Comparative Example 1
[0107] This comparative example provides a method for preparing β"-alumina ceramics based on gel casting molding, comprising the following steps:
[0108] S11, preparing a β"-alumina ceramic precursor powder having a β" phase content of 98% by a solid phase synthesis method;
[0109] S21, adding 12 parts of methacrylamide (C4H7NO) and 6 parts of N'-methylenebisacrylamide (linear molecular formula: CH2=CHCONH)2CH2) to 60 parts of water, and then performing a first ball milling for 15 minutes to obtain a uniformly mixed premixed solution;
[0110] S31, adding 135 parts of β"-alumina ceramic precursor powder and 0.3 parts of sodium polyacrylate dispersant (CAS No.: 9003-04-7) to the premixed solution, and then performing a second ball milling with a ball-to-material ratio of 5:1 and a grinding time of 12 hours to obtain a first slurry;
[0111] S41, vacuum degassing the first slurry to obtain a second slurry;
[0112] S51, adding 1.44 parts of initiator ammonium persulfate ((NH4)2S2O8) to the second slurry, and then performing a third ball milling for 15 minutes to obtain a third slurry;
[0113] S61, placing the third slurry into a mold, placing it in an oven at 80° C. for 12 hours to solidify, and then demolding to obtain a green blank, the green blank strength of which is less than 5 MPa; and
[0114] S71, debinding the green blank at 500°C for 2 hours, and sintering at 1620°C for 2 hours to obtain β"-alumina ceramic. The β" content of the β"-alumina ceramic is ≥95%, and the sintered bulk density is 2.922 g / cm 3 , only reaching 89.9% of the theoretical volume density, and the four-point bending strength is 64MPa.
[0115] Comparative Example 2
[0116] This comparative example provides a method for preparing β"-alumina ceramics based on gel casting molding, comprising the following steps:
[0117] S11, preparing a β"-alumina ceramic precursor powder having a β" phase content of 98% by a solid phase synthesis method;
[0118] S21, adding 10 parts of methacrylamide (C4H7NO) and 2 parts of N'-methylenebisacrylamide (linear molecular formula: CH2=CHCONH)2CH2) to 108 parts of water, and then performing a first ball milling for 15 minutes to obtain a uniformly mixed premixed solution;
[0119] S31, adding 160 parts of β"-alumina ceramic precursor powder and 0.48 parts of sodium polyacrylate dispersant (CAS No.: 9003-04-7) to the premixed liquid, and then performing a second ball milling with a ball-to-material ratio of 3:1 and a grinding time of 12 hours to obtain a first slurry;
[0120] S41, vacuum degassing the first slurry to obtain a second slurry;
[0121] S51, adding 1.1 parts of initiator ammonium persulfate ((NH4)2S2O8) to the second slurry, and then performing a third ball milling for 15 minutes to obtain a third slurry;
[0122] S61, placing the third slurry into a mold, placing it in a 90° C. oven for 12 hours to solidify, and then demolding to obtain a green blank, the green blank strength of which reaches 16 MPa; and
[0123] S71, debinding the green body at 500°C for 2 hours, and sintering at 1550°C for 2 hours to obtain β"-alumina ceramics. The β" content of β"-alumina ceramics is ≥95%, and the sintered volume density of the ceramics is 3.014 g / cm 3 , only reaching 92.7% of the theoretical volume density, and the four-point bending strength is 124MPa.
[0124] Comparative Example 3
[0125] This comparative example provides a method for preparing β"-alumina ceramics based on gel casting molding, comprising the following steps:
[0126] S11, preparing a β"-alumina ceramic precursor powder having a β" phase content of 98% by a solid phase synthesis method;
[0127] S21, adding 10 parts of methacrylamide (C4H7NO) and 2 parts of N'-methylenebisacrylamide (linear molecular formula: CH2=CHCONH)2CH2) to 108 parts of water, and then performing a first ball milling for 15 minutes to obtain a uniformly mixed premixed solution;
[0128] S31, adding 80 parts of β"-alumina ceramic precursor powder and 0.1 parts of sodium polyacrylate dispersant (CAS No.: 9003-04-7) to the premixed liquid, and then performing a second ball milling with a ball-to-material ratio of 3:1 and a grinding time of 12 hours to obtain a first slurry;
[0129] S41, vacuum degassing the first slurry to obtain a second slurry;
[0130] S51, adding 1.1 parts of initiator ammonium persulfate ((NH4)2S2O8) to the second slurry, and then performing a third ball milling for 15 minutes to obtain a third slurry;
[0131] S61, placing the third slurry into a mold, placing it in a 90° C. oven for 12 hours to solidify, and then demolding to obtain a green blank, the green blank strength of which reaches 10 MPa; and
[0132] S71, debinding the green blank at 500°C for 2 hours, and sintering it at 1550°C for 2 hours to obtain β"-alumina ceramics. The β" content of β"-alumina ceramics is ≥95%, and the sintered volume density of the ceramics is 2.936 g / cm 3 , only reaching 90.3% of the theoretical volume density, and the four-point bending strength is 92MPa.
[0133] In addition, one or more technical solutions in the embodiments of the present invention have at least the following technical effects or advantages:
[0134] In the embodiment of the present invention, the process parameters of the preparation method of β"-alumina ceramics are reasonably designed, which helps to improve the dispersibility and uniformity, improve the fluidity of the slurry, optimize the curing process, and improve the sintering quality, thereby improving the comprehensive performance of the β"-alumina ceramics.
[0135] In the embodiments of the present invention, the prepared β"-alumina ceramic has a high β" content, strong green body processing capability, high bulk density after sintering, and excellent mechanical properties.
[0136] In the embodiment of the present invention, the β" content of the β"-alumina ceramic is ≥95%, the volume density reaches more than 96% of the theoretical volume density, and the four-point bending strength is ≥250MP.
[0137] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A method for preparing β"-alumina ceramics based on gel casting, characterized in that: The method comprises: Obtaining a β"-alumina ceramic precursor powder having a set β" phase content; The monomer and the cross-linking agent are added to the solvent, and then the first ball milling is performed to obtain a premixed solution; Adding the β"-alumina ceramic precursor powder and the dispersant to the premixed liquid, and then performing a second ball milling to obtain a first slurry; Vacuum degassing the first slurry to obtain a second slurry; adding an initiator to the second slurry, and then performing a third ball milling to obtain a third slurry; Placing the third slurry into a mold for solidification, and then demolding to obtain a green blank; and The green blank is subjected to debinding and sintering to obtain β"-alumina ceramics.
2. The method according to claim 1, characterized in that The β" phase content is set to be ≥95%.
3. The method according to claim 1, characterized in that The mass concentration of the premix is 10% to 20%, wherein the mass ratio of the monomer to the crosslinking agent is (4 to 6):1, the monomer includes one or more of methacrylamide, acrylamide and hydroxymethyl acrylamide, and the crosslinking agent includes N,N'-methylenebisacrylamide.
4. The method according to claim 1, characterized in that: The mass of the dispersant accounts for 0.1% to 0.3% of the mass of the β"-alumina ceramic precursor powder, and the dispersant includes one or more of sodium polymethacrylate, sodium hexametaphosphate and sodium polyacrylate.
5. The method according to claim 1, characterized in that The mass ratio of the β"-alumina ceramic precursor powder to the premixed liquid is (1-2.3):1, and the solid content of the first slurry is 50%-70%; the ball-to-material ratio of the second ball milling is (3-5):1, and the time of the second ball milling is 10h-15h.
6. The method according to claim 1, characterized in that The mass of the initiator accounts for 10% to 12% of the mass of the monomer, and the initiator includes: one or more of ammonium persulfate and sodium persulfate.
7. The method according to claim 1, characterized in that The curing temperature is 80° C. to 100° C., and the curing heat preservation time is 10 h to 15 h.
8. The method according to claim 1, characterized in that The debinding temperature is 500° C. to 600° C., and the debinding heat preservation time is 1.5 h to 2.5 h.
9. The method according to claim 1, characterized in that: The sintering temperature is 1600° C. to 1650° C., and the sintering heat preservation time is 20 min to 40 min.
10. The method according to claim 1, characterized in that The β"-alumina ceramic meets at least one of the following properties: β" content ≥ 95%, volume density reaches more than 96% of theoretical volume density, and four-point bending strength ≥ 250MP.
Citation Information
Patent Citations
Preparation method of complex-shaped aluminum oxide ceramic
CN111533540A
Method for rapidly preparing aluminum oxide ceramic chip and prepared aluminum oxide ceramic chip
CN115368116A
Cited By
Gel injection molding method for ceramic electrolyte of solid sodium salt battery for energy storage
CN121872758A
Gelcasting-based method for preparing β"-aluminum oxide ceramic
WO2026056883A1