Alumina ceramic substrate as well as preparation method and application thereof
By using spherical alumina powder and an optimized sintering process, the appearance and performance problems of high-purity alumina ceramic substrates are solved, and the dielectric and mechanical properties are improved.
Patent Information
- Application Number
- CN202411033556.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-22
AI Technical Summary
High-purity alumina ceramic substrates have many defects in appearance and poor dielectric and mechanical properties.
Spherical alumina powder is used to replace sheet alumina powder, and optimized alumina powder is prepared by adjusting particle size distribution and adding appropriate solvents, plasticizers and binders, and casting and laminate isostatic sintering processes are used to prepare optimized alumina. Ceramic substrate.
It avoids the poor appearance of the product after sintering, significantly improves the dielectric and mechanical properties, and provides better post-processing performance and stability.
Smart Images

Figure CN118993708A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of alumina ceramic substrates, and in particular to an alumina ceramic substrate and a preparation method and application thereof. Background Art
[0002] Ceramic substrates have the advantages of small size, light weight, high temperature resistance, high electrical insulation performance, low dielectric constant and dielectric loss, large thermal conductivity, good chemical stability, and thermal expansion coefficient similar to that of components. They play an important role in many industries. Alumina ceramic substrates are a type of ceramic substrate. Alumina ceramics are classified by the purity of alumina. Alumina purity of >99% is called corundum porcelain, and alumina purity of about 99%, 95% and 90% is called 99 porcelain, 95 porcelain and 90 porcelain. The higher the purity of the ceramic sheet, the higher the dielectric constant, the lower the dielectric loss, and the better the smoothness of the substrate. Alumina ceramic substrates are widely used in the RF microwave electronics industry as a substrate material. Their high dielectric constant can miniaturize the circuit, and they have good thermal stability, small temperature drift, high substrate strength and chemical stability. Their performance is better than most other oxide materials, and they can be used in various thick film circuits, thin film circuits, hybrid circuits, microwave component modules, etc.
[0003] However, the current high-purity alumina ceramic substrates have many appearance defects and poor dielectric and mechanical properties. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the present invention proposes an alumina ceramic substrate and a preparation method thereof, aiming to solve the problem that the current high-purity alumina ceramic substrate has many appearance defects and poor dielectric and mechanical properties.
[0005] To achieve the above-mentioned purpose, the present invention proposes an alumina ceramic substrate, which comprises, by mass percentage: 40% to 60% alumina powder, wherein the particle size D50 of the alumina powder is 500nm-1000nm, 30% to 45% solvent, 1% to 3% dispersant, 5% to 10% plasticizer, and 2% to 5% binder.
[0006] Optionally, the microscopic morphology of the alumina powder is spherical.
[0007] Optionally, the Span value of the particle size distribution of the alumina powder is 1-1.2.
[0008] Optionally, the powder purity of the spherical alumina powder is not less than 99%.
[0009] Optionally, the solvent comprises a mixture of esters and alcohols, the ester is at least one of ethyl acetate, methyl acetate, propyl acetate, and butyl acetate, and the alcohol is at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol, and isobutanol; and / or the plasticizer comprises dioctyl phthalate and / or polyethylene glycol; and / or the binder comprises polyvinyl butyral; and / or the dispersant comprises triolein.
[0010] To achieve the above object, the present invention provides a method for preparing the above alumina ceramic substrate, comprising the following steps:
[0011] Adding spherical alumina powder to a solvent, adding a dispersant, and performing ball milling and mixing for the first time to obtain an intermediate product, and adding a plasticizer and a binder to the intermediate product, and performing ball milling and mixing for the second time to obtain a slurry;
[0012] Casting the slurry into a tape to obtain a green porcelain tape;
[0013] The green ceramic tape stack is isostatically pressed and then sintered to obtain an alumina ceramic substrate.
[0014] Optionally, the thickness of the green porcelain tape is 30um-60um.
[0015] Optionally, the temperature of the laminate isostatic pressing is 50° C.-80° C., the pressure is 50 MPa-100 MPa, and the holding time is 5 min-20 min.
[0016] Optionally, the sintering includes a first stage sintering and a second stage sintering, wherein the sintering temperature in the first stage is increased from room temperature to 400°C to 1000°C, and the heating rate is 0.1°C / min to 0.5°C / min; the sintering temperature in the second stage is increased from room temperature to 1450°C to 1600°C, and the heating rate is 1°C / min to 1.5°C / min.
[0017] In order to achieve the above-mentioned purpose, the present invention further proposes an application of an alumina ceramic substrate, wherein the alumina ceramic substrate is applied to the field of electronic components, the field of optoelectronics or the field of new energy.
[0018] The beneficial effects of the present invention are as follows: the present invention regulates the alumina powder of the alumina ceramic substrate, and adopts spherical alumina powder instead of flaky alumina powder, so as to avoid the situation that the nano-powder is easy to agglomerate and the grain size is too large and the aspect ratio of the grain is too large inside or on the surface of the product after sintering, thereby avoiding the alumina ceramic substrate from having poor appearance such as gray spots and white spots, which is beneficial to post-processing or post-treatment, and can obtain alumina ceramic substrate products with improved dielectric properties and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0020] Figure 1 This is a crystal phase microscope image of the alumina ceramic substrate after sintering according to an embodiment of the present invention, with a magnification of 500 times;
[0021] Figure 2 This is a crystal phase microscope image of the alumina ceramic substrate after sintering in the comparative example of the present invention, with a magnification of 500 times.
[0022] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0023] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0024] Unless otherwise specified, all technical and scientific terms used herein have the common meanings in the art to which the claimed subject matter belongs, and all reagents used are industrial or analytically pure.
[0025] In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application, and are not intended to limit the subject matter described in the claims.
[0026] The "range" disclosed in the present application is defined in the form of a lower limit and an upper limit, and a given range is defined by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundaries of the particular range. The range defined in this way can be inclusive or exclusive of the end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a range. For example, if a range of 60 to 120 and 80 to 110 is listed for a particular parameter, it is understood that a range of 60 to 110 and 80 to 120 is also expected. In addition, if the minimum range values 1 and 2 are listed, and if the maximum range values 3, 4 and 5 are listed, the following ranges can all be expected: 1 to 3, 1 to 4, 1 to 5, 2 to 3, 2 to 4 and 2 to 5. In the present application, unless otherwise specified, the numerical range "a to b" represents an abbreviation of any real number combination between a and b, where a and b are both real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.
[0027] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0028] Unless otherwise specified, all technical features and optional technical features of this application can be combined with each other to form a new technical solution.
[0029] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.
[0030] Ceramic substrates have the advantages of small size, light weight, high temperature resistance, high electrical insulation performance, low dielectric constant and dielectric loss, large thermal conductivity, good chemical stability, and thermal expansion coefficient similar to that of components. They play an important role in many industries. Alumina ceramic substrates are a type of ceramic substrate. Alumina ceramics are classified by the purity of alumina. Alumina purity of >99% is called corundum porcelain, and alumina purity of about 99%, 95%, and 90% is called 99 porcelain, 95 porcelain, and 90 porcelain. The higher the purity of the ceramic sheet, the higher the dielectric constant, the lower the dielectric loss, and the better the smoothness of the substrate. Alumina ceramic substrates are widely used in the RF microwave electronics industry as a substrate material. Their high dielectric constant can miniaturize the circuit, and they have good thermal stability, small temperature drift, high substrate strength and chemical stability. Their performance is better than most other oxide materials, and they can be used in various thick film circuits, thin film circuits, hybrid circuits, microwave component modules, etc.
[0031] However, the currently used high-purity alumina powder with a particle size D50 of 50nm-500nm or 1um-2um is in the form of flakes. The particle size distribution is large (SPAN value is between 1.5-2.5), and the aspect ratio of the grains after sintering is large (aspect ratio 1:3-1:5), which has a certain impact on subsequent processing; nano powders are easy to agglomerate, and after sintering, the grain size inside or on the surface of the product is relatively large (grain size exceeds 50um), so high-purity alumina ceramic substrates are prone to gray spots, white spots and other poor appearances, and the electrical and mechanical properties of local poor locations are low; micron powders are not easy to agglomerate, but the sintering temperature is high, it is difficult to sinter densely, and the dielectric and mechanical properties are low.
[0032] To solve the above problems, the present invention proposes an alumina ceramic substrate, which comprises, by mass percentage: 40% to 60% alumina powder, wherein the particle size D50 of the alumina powder is 500nm-1000nm, 30% to 45% solvent, 1% to 3% dispersant, 5% to 10% plasticizer, and 2% to 5% binder.
[0033] Alumina powder has different impurity types, contents, and particle sizes, which have different effects on alumina sintering and microstructure.
[0034] In this scheme, the alumina powder of the alumina ceramic substrate is regulated, and spherical alumina powder is used instead of flaky alumina powder to avoid the situation where the nanopowder is easy to agglomerate and the grain size is too large and the grain aspect ratio is too large inside or on the surface of the product after sintering, thereby avoiding the alumina ceramic substrate from having gray spots, white spots and other poor appearances, which is beneficial to post-processing or post-treatment, and can obtain alumina ceramic substrate products with improved dielectric and mechanical properties.
[0035] In some embodiments, the particle size D50 of the aluminum oxide powder is 0.5 um to 1.0 um. Preferably, the particle size D50 of the aluminum oxide powder is 0.5 um to 0.8 um.
[0036] Furthermore, the microscopic morphology of the alumina powder is spherical. Spherical alumina powder has the advantage of changing the microstructure of the material and improving the strength and density of the ceramic. In addition, the spherical alumina powder can maintain the permeability and porosity, significantly improve the sintering performance of the slurry, and thus significantly improve the performance of the ceramic.
[0037] Furthermore, the Span value of the particle size distribution of the alumina powder is 1-1.2.
[0038] In the particle size analysis report, in addition to the typical D10, D50, and D90, there is also the span, which is calculated using the formula (Dv0.9-Dv0.1) / Dv0.5.
[0039] Due to the existence of grading, the wide particle size distribution increases the contact points between particles and reduces the diffusion path, which will increase the initial densification rate of alumina powder. Although the initial densification rate is high, the wide particle size distribution strengthens the growth of grains in the middle of sintering. Since grain growth and green body densification are two competing reactions, the densification rate in the middle of sintering decreases faster than the densification rate of particles of nearly a single size. For the powder system given in this scheme, there is an optimal particle size distribution that makes the green porcelain show the best sinterability.
[0040] In some embodiments, the span value of the particle size distribution of the aluminum oxide powder is any value between 1, 1.1, 1.25, 1.5, 2, etc. The above content is not limited to the listed values, and other values not listed in the numerical range are also applicable.
[0041] Furthermore, the powder purity of the alumina powder is 99% to 99.999%. Within the above purity range, it is beneficial to improve the sintering performance and mechanical properties of the subsequent green porcelain strip sheet, and form a crystalline and plate-like microstructure of alumina porcelain. In some embodiments, the powder purity of the alumina powder is any value between 99%, 99.5%, 99.6%, 99.9%, 99.999%, etc., from 99% to 99.999%.
[0042] Furthermore, the solvent comprises a mixture of esters and alcohols, the ester is at least one of ethyl acetate, methyl acetate, propyl acetate, and butyl acetate, and the alcohol is at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol, and isobutanol; the plasticizer comprises dioctyl phthalate and / or polyethylene glycol; the binder comprises polyvinyl butyral; and the dispersant comprises triolein.
[0043] In this scheme, choosing triolein as the dispersant can prevent the system from agglomeration and ensure that the green tape obtained by casting has the characteristic of uniform density; the plasticizer has good plasticization on the binder and has a slow volatilization rate, which can ensure that the green porcelain tape can be stored in the air for a long time and its flexibility remains unchanged; the rheological properties and drying volatility of the solvent are important factors affecting the viscosity of the slurry and the casting time, which determine the rheological properties of the organic carrier and thus affect the quality of the cast green tape. Reasonable selection of solvents can effectively improve the physical properties of the green tape, such as uniformity and density.
[0044] In some embodiments, the mass ratio of alcohol to ester is (7-9):(1-3).
[0045] In order to solve the above problems, the present invention also provides a method for preparing the above alumina ceramic substrate, comprising the following steps:
[0046] S1: adding spherical alumina powder to a solvent, and then adding a dispersant to perform ball milling and mixing for the first time to obtain an intermediate product, and adding a plasticizer and a binder to the intermediate product to perform ball milling and mixing for the second time to obtain a slurry;
[0047] S2: tape-casting the slurry to obtain a green porcelain tape;
[0048] S3: isostatically pressing and then sintering the green ceramic tape stack to obtain an alumina ceramic substrate.
[0049] In some embodiments, the first ball milling is performed for 20 to 24 hours to obtain an intermediate product, and then dioctyl phthalate and a binder are added to the intermediate product, and the second ball milling is performed for another 20 to 24 hours to obtain slurry 2. The time of the two ball millings can be the same or different, and is not limited in this solution.
[0050] Products made by isostatic pressing have the advantages of uniform structure, high density, small sintering shrinkage, low mold cost, high production efficiency, and can be formed into complex shapes, slender products, large-sized products, and precision-sized products. In some embodiments, laminated isostatic pressing includes laminating the cast green porcelain tape to the required thickness, and then vacuuming the laminated product by isostatic pressing, and then placing the product in an isostatic press to perform isostatic pressing lamination at a certain temperature and pressure.
[0051] Furthermore, the thickness of the green porcelain tape is 30um-60um.
[0052] The thickness of the alumina ceramic green tape affects the insulation properties, hardness and wear resistance, thermal expansion coefficient and light transmittance of the resulting substrate. In this scheme, the alumina ceramic green tape with a thickness within the above range can be obtained by casting according to the application requirements of the substrate.
[0053] Furthermore, the temperature of the laminate isostatic pressing is 50° C.-80° C., the pressure is 50 MPa-100 MPa, and the holding time is 5 min-20 min.
[0054] In some embodiments, the temperature of the isostatic pressing of the laminate is any value between 50°C and 80°C, such as 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, etc.
[0055] In some embodiments, the pressure of the laminate isostatic pressing is any value between 50 MPa and 100 MPa, such as 50 MPa, 60 MPa, 70 MPa, 80 MPa, 90 MPa, and 100 MPa.
[0056] In some embodiments, the holding time of the laminate isostatic pressing is any value between 5 min and 20 min, such as 5 min, 10 min, 15 min, and 20 min.
[0057] Furthermore, the sintering includes a first stage sintering and a second stage sintering, wherein the sintering temperature of the first stage is increased from room temperature to 400°C to 1000°C, and the heating rate is 0.1°C / min to 0.5°C / min; the sintering temperature of the second stage is increased from room temperature to 1450°C to 1600°C, and the heating rate is 1°C / min.
[0058] / min~1.5℃ / min.
[0059] In the tape-casting ceramic substrate technology, the sintering process is closely related to the performance of the final sintered body. The sintering temperature gradient and sintering time both determine the appearance of the final sintered body. When the sintering system does not match, the ceramic substrate is prone to edge warping and fracture, and the ash residue after sintering also greatly affects the dielectric properties of the substrate. Therefore, in this scheme, it is also necessary to set the above sintering process parameters according to the components of the slurry.
[0060] In this scheme, the sintering is a method of first sintering at a low temperature, then heating to a high temperature stage for sintering, and finally cooling to obtain a ceramic body, which can better control the microstructure of the ceramic material and improve its performance.
[0061] In some embodiments, the sintering temperature in the first stage is increased from room temperature to any temperature between 400°C and 1000°C, such as 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C, and 1000°C, and the heating rate is preferably 0.1°C / min to 0.3°C / min.
[0062] In some embodiments, the second stage sintering temperature is increased from room temperature to any temperature between 400°C and 1000°C, such as 1450°C, 1550°C, 1600°C, etc., and the heating rate is preferably 1°C / min to 1.3°C / min.
[0063] In some embodiments, the first stage sintering is kept at the highest temperature for 4 hours to 6 hours; the second stage sintering is kept at the highest temperature for 2 hours to 4 hours.
[0064] In order to solve the above problems, the present invention also proposes an application of the above alumina ceramic substrate, wherein the alumina ceramic substrate is applied in the field of electronic components, optoelectronics or new energy.
[0065] In some embodiments, the electronic components field includes power electronics, electronic packaging, hybrid microelectronics and multi-chip modules.
[0066] In some embodiments, the optoelectronic field includes fields such as optical fiber communication, optoelectronic device manufacturing, and solar cell manufacturing: In optical fiber communication, the alumina ceramic substrate of this scheme can be used as the base of the optical fiber connector to fix and protect the optical fiber, and provide good mechanical support and thermal conductivity to ensure the transmission quality of the optical fiber. In optoelectronic device manufacturing, the alumina ceramic substrate of this scheme is used to manufacture the packaging and support structure of optoelectronic devices, such as photodiodes, photoelectric sensors, etc., and can provide good mechanical stability and electrothermal performance. In solar cell manufacturing, the ceramic substrate of this scheme is used for the support and packaging of the battery to provide stable mechanical and electrical properties.
[0067] In some embodiments, the new energy field includes new energy vehicles, supercapacitors and other fields.
[0068] Example 1
[0069] (1) Ingredients: Weigh 1000 g of flaky alumina powder (particle size D50: 0.6 μm, powder purity: 99.98%, span value: 1.1), 800 g of solvent (560 g of ethyl acetate, 240 g of ethanol), 20 g of triolein, 100 g of dibutyl phthalate, and 80 g of polyvinyl butyral;
[0070] (2) Alumina powder was added to the solvent, and then a dispersant was added and mixed by a ball mill for 24 hours to obtain slurry 1. DOP and a binder were then added to slurry 1 and mixed for another 24 hours to obtain slurry 2;
[0071] (3) Casting the ground slurry 2 into a 60 μm thick green porcelain tape;
[0072] (4) First stage sintering: sintering temperature 500 °C, heating rate 0.2 °C / min, holding time 4 h;
[0073] (5) Second stage sintering: sintering temperature is 1530°C, heating rate is 1°C / min, holding time is 4h, and cooling is performed to obtain an alumina ceramic substrate.
[0074] Example 2
[0075] The preparation method is the same as that of Example 1, except that the microscopic morphology of the aluminum oxide powder is flaky, the particle size D50 is 0.8 um, and the Span value is 1.1.
[0076] Example 3
[0077] The preparation method is the same as that of Example 1, except that the microscopic morphology of the alumina powder is spherical, the particle size D50 is 0.6 um, and the Span value is 1.1.
[0078] Comparative Example 1
[0079] The preparation method is the same as that of Example 1, except that the microscopic morphology of the aluminum oxide powder is flaky, the particle size D50 is 0.2 um, and the Span value is 1.1.
[0080] Comparative Example 2
[0081] The preparation method is the same as that of Example 1, except that the microscopic morphology of the aluminum oxide powder is flaky, the particle size D50 is 1.5 um, and the Span value is 1.1.
[0082] Comparative Example 3
[0083] The preparation method is the same as that of Example 1, except that the microscopic morphology of the aluminum oxide powder is flaky, the particle size D50 is 0.6 um, and the Span value is 1.5.
[0084] Furthermore, the sintered products of Example 3 and Comparative Example 1 were observed using a crystal phase microscope. Figure 1 and attached Figure 2 In addition, the mechanical, electrical properties and appearance of Examples 1-3 and Comparative Examples 1-3 were tested. The mechanical properties were tested by a mechanical universal machine to obtain their bending strength, and the dielectric constant was obtained by a resonant cavity method. The results are summarized in the following table:
[0085] Table 1. Performance test results
[0086]
[0087] From the above embodiments and comparative examples, it can be seen that the powder particle size of comparative example 1 is smaller than the minimum value in the range of this application, and the obtained alumina ceramic substrate has a crystal defect of 70.5μm; the powder particle size of comparative example 2 is larger than the maximum value of this application, resulting in a smaller dielectric constant and poor bending strength; in comparative example 3, the powder Span value is larger, and the obtained alumina ceramic substrate has appearance defects.
[0088] The above data results confirm that the alumina powder of the alumina ceramic substrate is regulated and spherical alumina powder is used instead of flake alumina powder to avoid the situation where the nanopowder is easy to agglomerate and the grain size is too large and the grain aspect ratio is too large inside or on the surface of the product after sintering. In addition, the alumina ceramic substrate is prevented from having gray spots, white spots and other poor appearances, which is beneficial for post-processing or post-treatment, and can obtain alumina ceramic substrate products with improved dielectric and mechanical properties.
[0089] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and modifications. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. An alumina ceramic substrate, characterized in that: In terms of mass percentage, it includes: Alumina powder 40% to 60%, the particle size D50 of the alumina powder is 500nm to 1000nm, Solvent 30%~45%, Dispersant 1%~3%, Plasticizer 5%~10%, Binder 2%~5%.
2. The alumina ceramic substrate according to claim 1, characterized in that: The microscopic morphology of the aluminum oxide powder is spherical.
3. The alumina ceramic substrate according to claim 1, characterized in that: The Span value of the particle size distribution of the alumina powder is 1-1.
2.
4. The alumina ceramic substrate according to claim 1, characterized in that: The powder purity of the aluminum oxide powder is not less than 99%.
5. The alumina ceramic substrate according to claim 1, characterized in that: The solvent comprises a mixture of an ester and an alcohol, wherein the ester is at least one of ethyl acetate, methyl acetate, propyl acetate, and butyl acetate, and the alcohol is at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol, and isobutanol; and / or, the plasticizer comprises dioctyl phthalate and / or polyethylene glycol; and / or, the binder comprises polyvinyl butyral; And / or, the dispersant comprises triolein.
6. A method for preparing an alumina ceramic substrate as claimed in any one of claims 1 to 5, characterized in that: The following steps are involved: Adding spherical alumina powder to a solvent, adding a dispersant, and performing ball milling and mixing for the first time to obtain an intermediate product, and adding a plasticizer and a binder to the intermediate product, and performing ball milling and mixing for the second time to obtain a slurry; Casting the slurry into a tape to obtain a green porcelain tape; The green ceramic tape stack is isostatically pressed and then sintered to obtain an alumina ceramic substrate.
7. The method for preparing an alumina ceramic substrate according to claim 6, characterized in that: The thickness of the green porcelain tape is 30um-60um.
8. The method for preparing an alumina ceramic substrate according to claim 6, characterized in that: The temperature of the laminate isostatic pressing is 50° C.-80° C., the pressure is 50 MPa-100 MPa, and the holding time is 5 min-20 min.
9. The method for preparing an alumina ceramic substrate according to claim 6, characterized in that: The sintering includes a first stage sintering and a second stage sintering, Wherein, the first stage sintering temperature is increased from room temperature to 400°C to 1000°C, and the heating rate is 0.1°C / min to 0.5°C / min; The second stage sintering temperature is increased from room temperature to 1450°C to 1600°C, and the heating rate is 1°C / min to 1.5°C / min.
10. Use of the alumina ceramic substrate as claimed in any one of claims 1 to 5, characterized in that: The alumina ceramic substrate is used in the field of electronic components, optoelectronics or new energy.
Citation Information
Patent Citations
Spherical alumina and preparation method and application thereof
CN111470522A
High-purity ultrathin high-strength aluminum oxide ceramic substrate as well as preparation method and application thereof
CN114538900A
Alumina for tape cast, alumina composition, alumina green sheet, alumina sintered plate and its production
JP1995089759A
Alumina sintered body and process for producing the same
KR1020000012006A
Alumina materials for low temperature co-sintering with refractory metallization
US4769294A
Cited By
Large-size, high-smoothness and high-strength aluminum oxide ceramic substrate and preparation method thereof
CN119285337A
High-thermal-conductivity aluminum oxide ceramic substrate for quick-response IGBT module and preparation method thereof