Preparation method of material with silicon removal and fluorine removal functions
By calcining coal-to-oil residue with alumina at high temperature and polymerizing reaction, copolymers with active groups are generated, which solves the problem of poor effect of traditional silicon removal and fluorine removal methods and achieves various pollutions in steel wastewater Efficient removal of substances, especially significant reductions in solubility of silicon and fluorine.
Patent Information
- Application Number
- CN202411132877.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-22
AI Technical Summary
The traditional silicon removal method has poor effect on difficult industrial wastewater treatment, and there are problems such as restriction of use conditions or colloidal pollution, making it difficult to effectively remove pollutants such as soluble silicon, fluoride ions and COD in steel wastewater.
By calcining the coal-to-oil residue with alumina at high temperature and mixing it in a pore-forming agent, followed by polymerization under the action of hydroxyethyl methacrylate and acrylic monomer, a copolymer with active groups is achieved. Removal of silicon and fluorine in wastewater.
The resulting materials have high strength, many pore structures and rich reactive groups. They can effectively remove soluble silicon, fluoride ions and COD in wastewater, significantly reduce the pollutant content of wastewater, and are suitable for the treatment of high-concentration silicon fluorine wastewater.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of wastewater treatment, and in particular relates to a method for preparing a material having the functions of removing silicon and fluorine. Background Art
[0002] In view of the current pressure of water shortage, industrial wastewater treatment technology faces unprecedented challenges. Traditional wastewater treatment methods have been unable to meet the treatment needs of high-difficulty wastewater. Therefore, "zero discharge" technology has emerged, aiming to achieve a closed-loop cycle of industrial wastewater treatment, reduce pollution to the environment, and improve the utilization efficiency of water resources. The concentrated brine in the zero-discharge process of steel wastewater contains a variety of pollutants such as soluble silicon, fluoride ions, COD and hardness. Among them, the inorganic salt components are complex and difficult to degrade, and it is a wastewater that is difficult to treat. At present, the commonly used methods for silicon removal and fluorine removal include membrane silicon removal, ion exchange method and coagulation method, but various silicon removal and fluorine removal methods have certain restrictions or defects in use conditions. For example, membrane silicon removal has high requirements for water quality, ion exchange method cannot remove colloidal silicon, etc. The agents used in the coagulation method will cause high water hardness or produce colloidal pollution. Summary of the invention
[0003] The primary purpose of the present invention is to provide a method for preparing a material with both silicon removal and fluorine removal functions, so as to effectively remove various pollutants contained in wastewater, such as soluble silicon, fluoride ions, COD and hardness.
[0004] To this end, the present invention provides the following technical solutions.
[0005] One aspect of the present invention provides a method for preparing a material having both silicon and fluorine removal functions, the method comprising the following steps:
[0006] The coal-to-liquid residue is mixed and crushed, and then calcined at 800 to 1200° C. for 4 to 10 hours under the protection of an inert gas to obtain a first product;
[0007] The obtained first product is immersed in acid and stirred at 40-60° C. and 200-400 rpm for 1-3 hours to obtain a second product;
[0008] The obtained second product and alumina are mixed evenly in a mass ratio of 1:0.1-0.5 and then immersed in a hydroxyethyl methacrylate / pore-forming agent blend, and then acrylic acid monomer and initiator are added and stirred at 30-100° C. for 4-8 hours, and then the obtained product is filtered, washed and dried to obtain the final product.
[0009] In a preferred embodiment of the present invention, the acid is an inorganic acid or an organic acid; the inorganic acid is selected from at least one of hydrochloric acid, nitric acid, carbonic acid, phosphoric acid, and boric acid, and the organic acid is selected from at least one of acetic acid, oxalic acid, malic acid, citric acid, and tartaric acid.
[0010] In a preferred embodiment of the present invention, the mass fraction of the acid is 10-30 wt %.
[0011] In a preferred embodiment of the present invention, the aluminum oxide is obtained by calcining aluminum hydroxide trihydrate, and the calcination conditions are: temperature 800-1200° C., time 2-4 hours.
[0012] In a preferred embodiment of the present invention, the hydroxyethyl methacrylate / pore former mixed liquid is prepared by mixing hydroxyethyl methacrylate, pore former and water in a volume mass ratio of 1 mL: 0.3-0.5 g: 5-15 mL.
[0013] In a preferred embodiment of the present invention, the pore former is selected from at least one of NaHCO3, K2CO3, K2C2O4, (NH4)2CO3, NH4HCO3 or CH3COONH4.
[0014] In a preferred embodiment of the present invention, the acrylic acid monomer is acrylic acid and / or methacrylic acid.
[0015] In a preferred embodiment of the present invention, the amount of the acrylic acid monomer added is 1 to 3 times the mass of hydroxyethyl methacrylate.
[0016] In a preferred embodiment of the present invention, the initiator is selected from any one of benzoyl peroxide, lauroyl peroxide, azobisisobutyronitrile, ammonium persulfate, potassium persulfate, and sodium persulfate.
[0017] In a preferred embodiment of the present invention, the added amount of the initiator is 0.1-0.6% of the mass of hydroxyethyl methacrylate.
[0018] By means of the above technical scheme, the present invention has at least the following advantages: the present invention generates an active coal-to-oil residue / alumina mixture with a large number of closed pores and vents by combining coal-to-oil residue and alumina under the action of a pore-forming agent, and at the same time, uses hydroxyethyl methacrylate and acrylic acid as monomers to undergo a polymerization reaction under the action of an initiator to generate a copolymer with active groups, and the copolymer generated by the polymerization reaction can also achieve the coating of the coal-to-oil residue / alumina mixture, so that the obtained product not only has a variety of porous structures, but also gives the product surface a variety of active groups, thereby achieving the simultaneous removal of silicon and fluorine in wastewater. The material of the present invention has a specific structure, high strength, and good comprehensive performance.
[0019] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the preferred embodiments of the present invention are described in detail as follows. DETAILED DESCRIPTION
[0020] In order to make the technical means, creative features, objectives and effects of the present invention easy to understand, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0021] Unless otherwise specified, the percentage content involved in the present invention refers to mass percentage for solid-liquid mixing and solid-solid mixing, and refers to volume percentage for liquid-liquid mixing.
[0022] Unless otherwise specified, the percentage concentrations referred to in the present invention all refer to the final concentration, which refers to the percentage of the added component in the system after the addition of the component.
[0023] The temperature parameters in the present invention, if not specifically limited, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows the temperature to fluctuate within the precision range controlled by the instrument.
[0024] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0025] Unless otherwise specified, the materials and reagents used in the following examples can be obtained from commercial sources.
[0026] Embodiment 1:
[0027] A method for preparing a material having both silicon removal and fluorine removal functions, the method comprising the following steps:
[0028] The coal-to-liquid residue was mixed and crushed, and then calcined at 1000° C. for 7 h under argon gas protection to obtain the first product. The first product was immersed in a 20 wt % acetic acid solution and stirred at 50° C. and 300 rpm for 2 h to obtain the second product.
[0029] Aluminum hydroxide trihydrate was calcined at 1000°C for 3h to obtain aluminum oxide. The obtained second product and aluminum oxide were mixed evenly in a mass ratio of 1:0.3 and then immersed in a hydroxyethyl methacrylate / NH4HCO3 mixed solution (mixed by hydroxyethyl methacrylate, NH4HCO3, and water in a volume mass ratio of 1mL:0.4g:10mL), and then acrylic acid (the amount added was 2 times the mass of hydroxyethyl methacrylate) and azobisisobutyronitrile (the amount added was 0.35% of the mass of hydroxyethyl methacrylate) were added and stirred at 75°C for 6h, and then the obtained product was filtered, washed and dried to obtain the final product.
[0030] Embodiment 2:
[0031] A method for preparing a material having both silicon removal and fluorine removal functions, the method comprising the following steps:
[0032] The coal-to-liquid residue was mixed and crushed, and then calcined at 800°C for 10 hours under argon gas protection to obtain the first product. The first product was immersed in a 10 wt% citric acid solution and stirred at 60°C and 200 rpm for 3 hours to obtain the second product.
[0033] Aluminum hydroxide trihydrate was calcined at 1200°C for 2h to obtain aluminum oxide. The obtained second product and aluminum oxide were mixed evenly at a mass ratio of 1:0.5 and then immersed in a hydroxyethyl methacrylate / NaHCO3 mixed solution (mixed with hydroxyethyl methacrylate, NaHCO3, and water at a volume mass ratio of 1mL:0.3g:15mL), and then methacrylic acid (the amount added was 1 times the mass of hydroxyethyl methacrylate) and ammonium persulfate (the amount added was 0.1% of the mass of hydroxyethyl methacrylate) were added and stirred at 80°C for 4h, and then the obtained product was filtered, washed and dried to obtain the final product.
[0034] Embodiment 3:
[0035] A method for preparing a material having both silicon removal and fluorine removal functions, the method comprising the following steps:
[0036] The coal-to-liquid residue was mixed and crushed, and then calcined at 1200° C. for 4 h under argon gas protection to obtain the first product. The first product was immersed in a 30 wt % acetic acid solution and stirred at 40° C. and 400 rpm for 1 h to obtain the second product.
[0037] Aluminum hydroxide trihydrate was calcined at 800°C for 4 hours to obtain aluminum oxide. The obtained second product and aluminum oxide were mixed evenly in a mass ratio of 1:0.1 and then immersed in a hydroxyethyl methacrylate / (NH4)2CO3 mixed solution (mixed with hydroxyethyl methacrylate, (NH4)2CO3, and water in a volume mass ratio of 1mL:0.5g:5mL), and then acrylic acid (the amount added was 3 times the mass of hydroxyethyl methacrylate) and potassium persulfate (the amount added was 0.6% of the mass of hydroxyethyl methacrylate) were added and stirred at 50°C for 7 hours, and then the obtained product was filtered, washed and dried to obtain the final product.
[0038] Embodiment 4:
[0039] A method for preparing a material having both silicon removal and fluorine removal functions, the method comprising the following steps:
[0040] The coal-to-liquid residue was mixed and crushed, and then calcined at 900° C. for 9 h under argon gas protection to obtain the first product. The first product was immersed in a 15 wt % citric acid solution and stirred at 50° C. and 300 rpm for 2 h to obtain the second product.
[0041] Aluminum hydroxide trihydrate was calcined at 1100°C for 3h to obtain aluminum oxide. The obtained second product and aluminum oxide were mixed evenly according to a mass ratio of 1:0.4 and then immersed in a hydroxyethyl methacrylate / CH3COONH4 mixed solution (mixed by hydroxyethyl methacrylate, CH3COONH4, and water according to a volume mass ratio of 1mL:0.5g:15mL), and then methacrylic acid (the amount added was 2 times the mass of hydroxyethyl methacrylate) and benzoyl peroxide (the amount added was 0.4% of the mass of hydroxyethyl methacrylate) were added and stirred at 100°C for 4h, and then the obtained product was filtered, washed and dried to obtain the final product.
[0042] Embodiment 5:
[0043] A method for preparing a material having both silicon removal and fluorine removal functions, the method comprising the following steps:
[0044] The coal-to-liquid residue was mixed and crushed, and then calcined at 1100° C. for 5 h under argon gas protection to obtain the first product. The first product was immersed in a 25 wt % citric acid solution and stirred at 40° C. and 400 rpm for 1 h to obtain the second product.
[0045] Aluminum hydroxide trihydrate was calcined at 900°C for 3h to obtain aluminum oxide. The obtained second product and aluminum oxide were mixed evenly in a mass ratio of 1:0.2 and then immersed in a hydroxyethyl methacrylate / K2CO3 mixed solution (mixed with hydroxyethyl methacrylate, K2CO3, and water in a volume mass ratio of 1mL:0.3g:5mL), and then methacrylic acid (the amount added was 1 times the mass of hydroxyethyl methacrylate) and benzoyl peroxide (the amount added was 0.2% of the mass of hydroxyethyl methacrylate) were added and stirred at 100°C for 4h, and then the obtained product was filtered, washed and dried to obtain the final product.
[0046] Embodiment 6:
[0047] A method for preparing a material having both silicon removal and fluorine removal functions, the method comprising the following steps:
[0048] The coal-to-liquid residue was mixed and crushed, and then calcined at 1000° C. for 7 h under argon gas protection to obtain the first product. The first product was immersed in a 20 wt % acetic acid solution and stirred at 60° C. and 200 rpm for 2 h to obtain the second product.
[0049] Aluminum hydroxide trihydrate was calcined at 800°C for 3h to obtain aluminum oxide. The obtained second product and aluminum oxide were mixed evenly at a mass ratio of 1:0.5 and then immersed in a hydroxyethyl methacrylate / NH4HCO3 mixed solution (mixed with hydroxyethyl methacrylate, NH4HCO3, and water at a volume mass ratio of 1mL:0.4g:15mL), and then acrylic acid (the amount added was 3 times the mass of hydroxyethyl methacrylate) and potassium persulfate (the amount added was 0.5% of the mass of hydroxyethyl methacrylate) were added and stirred at 50°C for 7h, and then the obtained product was filtered, washed and dried to obtain the final product.
[0050] Comparative Example 1:
[0051] A method for preparing a material having both silicon removal and fluorine removal functions, the method comprising the following steps:
[0052] The coal-to-liquid residue was immersed in a 20 wt % acetic acid solution and stirred at 50° C. and 300 rpm for 2 hours to obtain a first product.
[0053] Aluminum hydroxide trihydrate was calcined at 1000°C for 3h to obtain aluminum oxide. The first product obtained and aluminum oxide were mixed evenly in a mass ratio of 1:0.3 and then immersed in a hydroxyethyl methacrylate / NH4HCO3 mixed solution (mixed with hydroxyethyl methacrylate, NH4HCO3, and water in a volume mass ratio of 1mL:0.4g:10mL), and then acrylic acid (the amount added was 2 times the mass of hydroxyethyl methacrylate) and azobisisobutyronitrile (the amount added was 0.35% of the mass of hydroxyethyl methacrylate) were added and stirred at 75°C for 6h, and then the obtained product was filtered, washed and dried to obtain the final product.
[0054] Comparative Example 2:
[0055] A method for preparing a material having both silicon removal and fluorine removal functions, the method comprising the following steps:
[0056] The coal-to-liquid residues were mixed and crushed, and then calcined at 1000° C. for 7 h under argon gas protection to obtain the first product.
[0057] Aluminum hydroxide trihydrate was calcined at 1000°C for 3h to obtain aluminum oxide. The first product obtained and aluminum oxide were mixed evenly in a mass ratio of 1:0.3 and then immersed in a hydroxyethyl methacrylate / NH4HCO3 mixed solution (mixed with hydroxyethyl methacrylate, NH4HCO3, and water in a volume mass ratio of 1mL:0.4g:10mL), and then acrylic acid (the amount added was 2 times the mass of hydroxyethyl methacrylate) and azobisisobutyronitrile (the amount added was 0.35% of the mass of hydroxyethyl methacrylate) were added and stirred at 75°C for 6h, and then the obtained product was filtered, washed and dried to obtain the final product.
[0058] Comparative Example 3:
[0059] A method for preparing a material having both silicon removal and fluorine removal functions, the method comprising the following steps:
[0060] Aluminum hydroxide trihydrate was calcined at 1000°C for 3h to obtain alumina. Coal-to-oil residue and alumina were mixed evenly in a mass ratio of 1:0.3 and then soaked in a hydroxyethyl methacrylate / NH4HCO3 mixed solution (mixed with hydroxyethyl methacrylate, NH4HCO3, and water in a volume mass ratio of 1mL:0.4g:10mL), and then acrylic acid (the amount added was 2 times the mass of hydroxyethyl methacrylate) and azobisisobutyronitrile (the amount added was 0.35% of the mass of hydroxyethyl methacrylate) were added and stirred at 75°C for 6h, and then the obtained product was filtered, washed and dried to obtain the final product.
[0061] Comparative Example 4:
[0062] A method for preparing a material having both silicon removal and fluorine removal functions, the method comprising the following steps:
[0063] Aluminum hydroxide trihydrate was calcined at 1000°C for 3h to obtain alumina. The obtained alumina was soaked in a hydroxyethyl methacrylate / NH4HCO3 mixed solution (mixed by hydroxyethyl methacrylate, NH4HCO3, and water in a volume mass ratio of 1mL:0.4g:10mL), and then acrylic acid (the added amount was 2 times the mass of hydroxyethyl methacrylate) and azobisisobutyronitrile (the added amount was 0.35% of the mass of hydroxyethyl methacrylate) were added and stirred at 75°C for 6h, and then the obtained product was filtered, washed and dried to obtain the final product.
[0064] Comparative Example 5:
[0065] A method for preparing a material having both silicon removal and fluorine removal functions, the method comprising the following steps:
[0066] The coal-to-liquid residue was mixed and crushed, and then calcined at 1000° C. for 7 h under argon gas protection to obtain the first product. The first product was immersed in a 20 wt % acetic acid solution and stirred at 50° C. and 300 rpm for 2 h to obtain the second product.
[0067] The obtained second product and alumina are mixed evenly and then immersed in a hydroxyethyl methacrylate / NH4HCO3 mixed solution (mixed by hydroxyethyl methacrylate, NH4HCO3, and water in a volume mass ratio of 1mL:0.4g:10mL), and then acrylic acid (the added amount is twice the mass of hydroxyethyl methacrylate) and azobisisobutyronitrile (the added amount is 0.35% of the mass of hydroxyethyl methacrylate) are added, and the mixture is stirred at 75°C for 6h, and then the obtained product is filtered, washed and dried to obtain the final product.
[0068] Comparative Example 6:
[0069] A method for preparing a material having both silicon removal and fluorine removal functions, the method comprising the following steps:
[0070] A hydroxyethyl methacrylate / NH4HCO3 mixed solution (mixed by hydroxyethyl methacrylate, NH4HCO3, and water in a volume mass ratio of 1mL:0.4g:10mL) was prepared, and then acrylic acid (the added amount was twice the mass of hydroxyethyl methacrylate) and azobisisobutyronitrile (the added amount was 0.35% of the mass of hydroxyethyl methacrylate) were added, and the mixture was stirred at 75°C for 6h, and then the obtained product was filtered, washed and dried to obtain the final product.
[0071] Comparative Example 7:
[0072] A method for preparing a material having both silicon removal and fluorine removal functions, the method comprising the following steps:
[0073] The coal-to-liquid residue was mixed and crushed, and then calcined at 1000° C. for 7 h under argon gas protection to obtain the first product. The first product was immersed in a 20 wt % acetic acid solution and stirred at 50° C. and 300 rpm for 2 h to obtain the second product.
[0074] Aluminum hydroxide trihydrate was calcined at 1000° C. for 3 h to obtain aluminum oxide. The obtained second product and aluminum oxide were mixed evenly in a mass ratio of 1:0.3 to obtain a final product.
[0075] Experiment 1: Comparison of the efficiency of different materials in treating steel wastewater
[0076] Experimental objects: Materials of Examples 1 to 6 and Comparative Examples 1 to 7
[0077] Experimental method: Take the wastewater discharged from a steel plant in Hebei Province as the sample to be tested. The indicators of the wastewater before treatment are: TDS concentration is 450mg / L, TOC concentration is 124mg / L, fluoride concentration is 253mg / L, and soluble silicon is 186mg / L. The wastewater to be tested is divided into 13 groups, each group is 500mL, and the materials obtained in Examples 1 to 6 and Comparative Examples 1 to 7 are added respectively according to the amount of wastewater with a material-liquid ratio of 20mg / 100mL. Stir continuously for 10min at a speed of 400rpm and then stand for 10h. Then take the supernatant of each group to detect the indicators of the wastewater. The results are shown in Table 1:
[0078] Table 1 Wastewater indicators after treatment
[0079] Group TDS(mg / L) TOC(mg / L) Fluoride (mg / L) Soluble silicon (mg / L) Example 1 89 14 28 16 Example 2 92 15 30 17 Example 3 87 13 25 14 Example 4 90 15 27 15 Example 5 95 18 32 21 Example 6 93 16 31 19 Comparative Example 1 98 22 36 25 Comparative Example 2 116 35 48 34 Comparative Example 3 143 59 77 60 Comparative Example 4 318 87 156 132 Comparative Example 5 187 72 101 85 Comparative Example 6 398 101 223 168 Comparative Example 7 163 65 82 71
[0080] It can be seen from the results in Table 1 that, compared with Comparative Examples 1 to 7, the materials of Examples 1 to 6 of the present invention can effectively remove various pollutants such as soluble silicon, fluoride ions, TOC and TDS contained in wastewater. The indicators of wastewater treated with the materials of the present invention are significantly reduced, among which the contents of fluoride and soluble silicon are significantly reduced. This result shows that the materials of the present invention are particularly suitable for the effective treatment of high-concentration silicon-fluoride wastewater.
[0081] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes by using the methods and technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a material having both silicon removal and fluorine removal functions, characterized in that: The method comprises the following steps: The coal-to-liquid residue is mixed and crushed, and then calcined at 800 to 1200° C. for 4 to 10 hours under the protection of an inert gas to obtain a first product; The obtained first product is immersed in acid and stirred at 40-60° C. and 200-400 rpm for 1-3 hours to obtain a second product; The obtained second product and alumina are mixed evenly in a mass ratio of 1:0.1-0.5 and then immersed in a hydroxyethyl methacrylate / pore-forming agent blend, and then acrylic acid monomer and initiator are added and stirred at 30-100° C. for 4-8 hours, and then the obtained product is filtered, washed and dried to obtain the final product.
2. The preparation method according to claim 1, characterized in that: The acid is an inorganic acid or an organic acid; the inorganic acid is selected from at least one of hydrochloric acid, nitric acid, carbonic acid, phosphoric acid, and boric acid, and the organic acid is selected from at least one of acetic acid, oxalic acid, malic acid, citric acid, and tartaric acid.
3. The preparation method according to claim 1 or 2, characterized in that: The mass fraction of the acid is 10 to 30 wt %.
4. The preparation method according to claim 1, characterized in that: The alumina is obtained by calcining aluminum hydroxide trihydrate, and the calcination conditions are: temperature 800-1200° C., time 2-4 hours.
5. The preparation method according to claim 1, characterized in that: The hydroxyethyl methacrylate / pore-forming agent mixed liquid is prepared by mixing hydroxyethyl methacrylate, pore-forming agent and water in a volume mass ratio of 1 mL: 0.3-0.5 g: 5-15 mL.
6. The preparation method according to claim 1 or 5, characterized in that: The pore former is selected from at least one of NaHCO3, K2CO3, K2C2O4, (NH4)2CO3, NH4HCO3 or CH3COONH4.
7. The preparation method according to claim 1, characterized in that: The acrylic acid monomer is acrylic acid and / or methacrylic acid.
8. The preparation method according to claim 1 or 7, characterized in that: The amount of the acrylic acid monomer added is 1 to 3 times the mass of hydroxyethyl methacrylate.
9. The preparation method according to claim 1, characterized in that: The initiator is selected from any one of benzoyl peroxide, lauroyl peroxide, azobisisobutyronitrile, ammonium persulfate, potassium persulfate and sodium persulfate.
10. The preparation method according to claim 1 or 9, characterized in that: The added amount of the initiator is 0.1-0.6% of the mass of hydroxyethyl methacrylate.