High-performance benzocyclobutenyl polynorbornene composite material and preparation method thereof
Synthesis of benzocyclobutylene polynorbornene composite materials through ROMP technology, solving the problems of parasitic capacitance and POSS production in the prior art, achieving low dielectric constant and excellent performance materials, and meeting the electronic packaging technology need.
Patent Information
- Application Number
- CN202411261239.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-10
AI Technical Summary
The prior art is difficult to effectively reduce the inherent parasitic capacitance of the dielectric layer, and polyhedral oligosiloxane (POSS) has problems with long production cycles and high costs in industrial scale production, and the increase in the incorporation of its particles into polymer matrix will lead to The problems of particle aggregation and phase separation are lacking systematic experimental research to clarify the impact of organic-inorganic copolymerization on dielectric properties.
The benzocyclobutenyl polynorbornene composite material is synthesized by ring-opening polymerization (ROMP) technology. By designing the chemical structure and performance of new low-Dk materials, the type and proportion optimization of silanoxy groups can be achieved efficiently. The bottom-up synthesis strategy forms crosslinked polymers with trapezoidal or mesh structures to achieve complete crosslinking and low dielectric constant of the material.
It achieves a stable low dielectric constant and dielectric loss in the frequency range of 100-106Hz, demonstrates excellent thermal stability, hydrophobicity and mechanical properties, and meets the demand of advanced electronic packaging technology for low dielectric composite materials.
Smart Images

Figure CN118994539A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a high-performance benzocyclobutene-based polynorbornene composite material and a preparation method thereof, belonging to the technical field of high-performance electronic packaging resins. Background Art
[0002] With the rapid development of the integrated circuit industry, the chip feature size continues to shrink, while the internal wiring density has increased significantly, resulting in increasingly serious problems of resistance-capacitance delay, crosstalk noise, and power loss caused by metal resistance and parasitic capacitance between line layers. In order to solve these problems, the use of low-resistance metals such as copper is crucial, but more importantly, it is necessary to reduce the inherent parasitic capacitance of the dielectric layer. Therefore, it is urgent to develop new low-k dielectric constant ( D k ) insulating materials to cope with the rapid advancement of information technology.
[0003] Introducing inorganic nanopores into polymers can effectively reduce the dielectric constant of composite materials, and polyhedral oligosiloxane (POSS) is considered to be the basis for constructing such functional nanomaterials. POSS can be regarded as organic-inorganic hybrid nanostructures with different geometric shapes and symmetries. Its potential lies in the ability to reduce the dielectric constant and dielectric loss of polymers including polyimide, bismaleimide resin, polyarylether, polybenzoxazine, benzocyclobutene resin, polyolefin, cyanate resin and epoxy resin when used alone or in combination with other materials.
[0004] However, industrial large-scale production of high-purity POSS faces difficulties. In addition, POSS has inherent limitations. In addition to long production cycles and high costs, as the number of POSS particles incorporated into the polymer matrix increases, it will lead to particle aggregation and trigger phase separation problems. To address these issues, it is necessary to establish chemical connections between POSS and polymer chains to facilitate the production of various nanocomposites in a "bottom-up" manner, thereby overcoming the above challenges.
[0005] Ring-opening polymerization (ROMP) has emerged as a powerful and widely used technique for the synthesis of polymer materials. Norbornene-based monomers are widely employed due to their high ring strain properties, which promotes efficient polymerization propagation. Moreover, this class of monomers can be easily modified with various functional groups, enabling the synthesis of polymers with unique structures and properties. Due to this versatility, polynorbornenes with pendant groups have attracted much attention in nanocomposite research, ensuring excellent properties such as mechanical integrity and highly dispersed inorganic nanodomains. However, there is a lack of systematic experimental studies to clarify the specific effects of topological structure and particle dispersion on dielectric properties via efficient ROMP for organic-inorganic copolymerization.
[0006] At present, there is an urgent need to develop a simple and efficient "bottom-up" synthesis strategy and carefully design the type and proportion of the suspended silaneoxy groups in the ROMP main chain to optimize the chemical structure and properties of the resin material, thereby meeting the growing demand for BCB resins with different properties in the advanced electronic packaging and low dielectric composite materials markets. Summary of the invention
[0007] The purpose of the present invention is to provide a high-performance benzocyclobutene-based polynorbornene composite material, which has good comprehensive properties of dielectric materials, including thermal stability, good hydrophobicity and good mechanical properties; the molecular method of the composite material provided by the invention paves the way for the design of new low Dk materials and demonstrates an effective strategy for improving the performance of electronic packaging technology.
[0008] The benzocyclobutene-based polynorbornene crosslinked polymer provided by the present invention has a structural formula as shown in Formula I:
[0009] Formula I In the formula, R1, R2, and R3 are independently selected from C1-C4 alkyl or oxy groups; The alkyl group may be methyl, ethyl, propyl, isopropyl, n-butyl, isobutyl, etc. The oxy group may be a methoxy group or an ethoxy group; The value range of x is 1-100; the value range of y is 1-100.
[0010] The relationship formula of the high-performance benzocyclobutene-based polynorbornene composite material of the present invention can be expressed as C-XD-YB or C-XT-YB; Wherein: D / T represents polysiloxane cross-linked polymer; B represents benzocyclobutene polymer; Specifically, the high-performance benzocyclobutene-based polynorbornene composite material of the present invention is any one or more of the following polymers: 1) Polymer H-0D-100B: R1 is methyl, R2 and R3 are oxy groups, x is 0, and y is 100; 2) Polymer H-1D-99B: R1 is methyl, R2 and R3 are oxy groups, x is 1, and y is 99; 3) Polymer H-3D-97B: R1 is methyl, R2 and R3 are oxy groups, x is 3, and y is 97; 4) Polymer H-5D-95B: R1 is methyl, R2 and R3 are oxy groups, x is 5, and y is 95; 5) Polymer H-10D-90B: R1 is methyl, R2 and R3 are oxy groups, x is 10, and y is 90; 6) Polymer H-20D-80B: R1 is methyl, R2 and R3 are oxy groups, x is 20, and y is 80; 7) Polymer H-30D-70B: R1 is methyl, R2 and R3 are oxy groups, x is 30, and y is 70; 8) Polymer H-0T-100B: R1, R2 and R3 are oxy groups, x is 0, and y is 100; 9) Polymer H-1T-99B: R1, R2 and R3 are oxy groups, x is 1, and y is 99; 10) Polymer H-3T-97B: R1, R2 and R3 are oxy groups, x is 3, and y is 97; 11) Polymer H-5T-95B: R1, R2 and R3 are oxy groups, x is 5, and y is 95; 12) Polymer H-10T-90B: R1, R2 and R3 are oxy groups, x is 10, y is 90; 13) Polymer H-20T-80B: R1, R2 and R3 are oxy groups, x is 20, y is 80; 14) Polymer H-30T-70B: R1, R2 and R3 are oxy groups, x is 30, and y is 70.
[0011] The present invention also provides a method for preparing the high-performance benzocyclobutene-based polynorbornene composite material, comprising the following steps: S1 and 5-vinylbicyclo[2.2.1]hept-2-ene are subjected to hydrosilylation reaction with dimethoxysilane hydride or trimethoxysilane hydride in the presence of catalyst I to obtain siloxane precursor II and siloxane precursor III; The structure of the 5-vinylbicyclo[2.2.1]hept-2-ene is ; The structures of the dimethoxysilane and the trimethoxysilane monomers are respectively , ; The structures of the siloxane precursor II and the siloxane precursor III are respectively , ; S2, 5-vinylbicyclo[2.2.1]hept-2-ene and silylbenzenecyclobutene react with each other under the action of the catalyst I to obtain a norbornene-modified benzocyclobutene monomer; The structure of the silicon hydrogen benzocyclobutene is ; The structure of the benzocyclobutene precursor IV is ; S3, the siloxane precursor II or the siloxane precursor III and the benzocyclobutene precursor IV are subjected to a ROMP polymerization reaction under the action of a catalyst II to obtain a linear benzocyclobutene-based polynorbornene represented by formula V;
[0012] Formula V In formula V, R1, R2, and R3 are selected from C1-C4 alkyl or alkoxy groups; S4, the linear benzocyclobutenyl polynorbornene represented by formula V is subjected to a condensation reaction under the action of catalyst III to obtain a benzocyclobutenyl polynorbornene crosslinked product represented by formula VI;
[0013] Formula VI In formula VI, R1, R2, and R3 are selected from C1-C-4 alkyl or oxy groups; S5. The benzocyclobutene-based polynorbornene crosslinked product shown in formula VI is thermally cured at high temperature to generate the high-performance benzocyclobutene-based polynorbornene composite material.
[0014] In the preparation method of the present invention, in step S1, the molar ratio of the 5-vinylbicyclo[2.2.1]hept-2-ene to the dimethoxysilane or the trimethoxysilane is 1:1-1.5; The catalyst I is a Karstedt catalyst; The molar ratio of the catalyst I to the trimethoxysilane or the dimethoxysilane is 1:50-100; The conditions of the hydrosilylation reaction are: temperature of 70-90° C. and time of 1-4 h.
[0015] In the preparation method of the present invention, in step S1, the molar ratio of the 5-vinylbicyclo[2.2.1]hept-2-ene to the silylbenzenecyclobutene is 1:1-1.5; The molar ratio of the catalyst I to the silicon hydrogen benzocyclobutene is 1:50-60; The conditions of the hydrosilylation reaction are: temperature of 70-90° C. and time of 1-4 h.
[0016] In the preparation method of the present invention, in step S3, the catalyst II is a Grubbs catalyst; The molar ratio of the catalyst II to the benzocyclobutene precursor IV is 1:50-60; The ROMP polymerization reaction is carried out in an organic solvent I, wherein the organic solvent I is one or more of tetrahydrofuran, toluene, dichloromethane and dioxane; The conditions of the ROMP polymerization reaction are: temperature of 20-40° C. and time of 1-3 h.
[0017] According to the different types of precursors and the introduction ratios, the silsesquioxane precursors shown in Formula V include crosslinkers 0D-100B, crosslinkers 1D-99B, crosslinkers 3D-97B, crosslinkers 5D-95B, crosslinkers 10D-90B, crosslinkers 20D-80B, crosslinkers 30D-70B crosslinkers 1T-99B, crosslinkers 3T-97B, crosslinkers 5T-95B, crosslinkers 10T-90B, crosslinkers 20T-80B, and crosslinkers 30T-70B; in: Cross-linked product 0D-100B: R1 is methyl, R2 and R3 are methoxy, x is 0, and y is 100; Cross-linked product 1D-99B: R1 is methyl, R2 and R3 are methoxy, x is 1, and y is 99; Cross-linked compound 3D-97B: R1 is methyl, R2 and R3 are methoxy, x is 3, and y is 97; Cross-linked compound 5D-95B: R1 is methyl, R2 and R3 are methoxy, x is 5, and y is 95; Cross-linked product 10D-90B: R1 is methyl, R2 and R3 are methoxy, x is 10, and y is 90; Cross-linked product 20D-80B: R1 is methyl, R2 and R3 are methoxy, x is 20, and y is 80; Cross-linked product 30D-70B: R1 is methyl, R2 and R3 are methoxy, x is 30, and y is 70; Cross-linked product 0T-100B: R1, R2 and R3 are methoxy, x is 0, and y is 100; Cross-linked substance 1T-99B: R1, R2 and R3 are methoxy, x is 1, and y is 99; Cross-linked compound 3T-97B: R1, R2 and R3 are methoxy, x is 3, and y is 97; Cross-linked compound 5T-95B: R1, R2 and R3 are methoxy, x is 5, and y is 95; Cross-linked product 10T-90B: R1, R2 and R3 are methoxy, x is 10, and y is 90; Cross-linked product 20T-80B: R1, R2 and R3 are methoxy, x is 20, and y is 80; Cross-linked product 30T-70B: R1, R2 and R3 are methoxy, x is 30, and y is 70; In the preparation method of the present invention, in step S4, the catalyst III is one or more of hydrochloric acid, sulfuric acid, nitric acid and trifluoroacetic acid; By adding the catalyst III, the pH of the reaction system is adjusted to 3-6; The condensation reaction is carried out in an organic solvent II; the organic solvent II is one or more of tetrahydrofuran, dioxane, acetonitrile and dimethyl sulfoxide; The conditions of the condensation reaction are: temperature of 20-30°C and time of 12-15h; In the preparation method of the present invention, in step S5, the temperature of the thermal curing can be 250-350°C.
[0018] The present invention further provides a packaging material, which is made of the above-mentioned benzocyclobutene-based polynorbornene composite material.
[0019] Compared with the prior art, the present invention has the following beneficial effects: The present invention uses an innovative "bottom-up" synthesis strategy to manufacture high-performance benzocyclobutene-based polynorbornene composites, which covalently integrates organoalkoxysilanes and BCB as pendant groups of polynorbornene through ROMP polymerization. After hydrolysis and programmed thermal curing, these linear polymers can be fully cross-linked to form ladder-shaped or network-like siloxane structures with inherent porosity. 0 -10 6 In the Hz frequency range, the material of the present invention exhibits a stable low dielectric constant (dielectric constant <2.25) and dielectric loss factor (dielectric loss <2.27×10⁻³). In addition, the new material of the present invention exhibits excellent comprehensive properties in many aspects, including excellent thermal stability (thermal decomposition temperature T d5% >440℃), good hydrophobicity (contact angle greater than 100º) and excellent mechanical properties. The molecular design method provided by this invention paves the way for the development of new low dielectric constant materials and demonstrates an effective strategy to improve the performance of electronic packaging technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 is the H NMR spectrum of the trimethoxysilicon precursor (TMSi) prepared in Example 1 of the present invention; Figure 2 is the H NMR spectrum of the dimethoxy silicon precursor (DMSi) prepared in Example 1 of the present invention; Figure 3 This is the H NMR spectrum of the benzocyclobutene silicon hydrogen precursor prepared in Example 1 of the present invention; Figure 4 This is the H NMR spectrum of the linear 0D-100B cross-linked product prepared in Example 1 of the present invention; Figure 5 This is a comparison chart of dielectric properties tests of 12 kinds of cured products prepared in Example 4 of the present invention; Figure 6 This is a comparison chart of thermal stability tests of 12 kinds of cured products prepared in Example 4 of the present invention; Figure 7 This is a comparison chart of mechanical properties tests of 12 kinds of cured products prepared in Example 4 of the present invention; Figure 8 This is a comparison chart of contact angle tests of 12 kinds of cured products prepared in Example 4 of the present invention. DETAILED DESCRIPTION
[0021] The present invention will be further described below in conjunction with specific embodiments, but the present invention is not limited to the following embodiments.
[0022] Unless otherwise specified, the experimental methods used in the following examples are conventional methods.
[0023] Unless otherwise specified, the reagents, materials, instruments, etc. used in the following examples can be obtained from commercial sources.
[0024] Example 1. Preparation of ROMP polymer precursor Under an inert atmosphere, Karstedt's catalyst (1.92 g, 5 mmol) was dissolved in 5-vinylbicyclo[2.2.1]hept-2-ene (69.2 g, 200 mmol) and added to a 250 mL three-necked flask; nitrogen was bubbled in an ice / water bath for 15 min, and trialkoxysilane (24.5 g, 200 mmol) was added under nitrogen protection, heated in an oil bath for 2 hours, and then cooled to room temperature; then, the precursor III was obtained by reduced pressure distillation, and the fraction temperature was 120 °C.
[0025] According to the above operation steps, the trialkoxysilane hydride monomer was replaced with a dialkoxysilane hydride monomer and a benzocyclobutenesilane hydride monomer, and the fraction temperatures were 110° C. and 180° C., respectively. The obtained precursors were recorded as precursors II and IV, respectively.
[0026] The NMR hydrogen spectrum and NMR carbon spectrum of the precursor prepared in this example are as follows: Figure 1-3 Shown Example 2: Preparation of Linear Benzocyclobutene-Based Polynorbornene Polymer Grubbs II catalyst, precursor II and precursor IV were dissolved in anhydrous dichloromethane at a certain molar ratio (2 / 0 / 100, 2 / 1 / 99, 2 / 3 / 97, 2 / 5 / 95, 2 / 10 / 90, 2 / 20 / 80, 2 / 30 / 70) to a concentration of 10mmol / 80 mL, and polymerized in a nitrogen atmosphere glove box for 30 minutes. The solvent was poured into methanol and poured out from the precipitated polymer. The above "re-dissolve precipitation" step was repeated twice. The product was a viscous liquid named XD-YB (X+Y=100; X=0, 1, 3, 5, 10, 20, 30).
[0027] According to the above operation steps, the precursor formula II was replaced by the precursor formula III, and the other parameters remained unchanged. These polymers were named XT-YB (X+Y=100; X=0, 1, 3, 5, 10, 20, 30).
[0028] The H NMR spectrum of the linear benzocyclobutene-based polynorbornene polymer 0X-100B prepared in this example is as follows: Figure 4 shown.
[0029] Example 3: Preparation of benzocyclobutene-based polynorbornene crosslinked products The polymer XD-YB (10 mmol) was dissolved in 200 mL of tetrahydrofuran solution. Subsequently, an appropriate amount of 0.1 mol / L hydrochloric acid and 3 mL of deionized water were added to adjust the solution pH to about 3. The mixture was stirred at room temperature for 10 hours, and then the solution was dried over anhydrous magnesium sulfate (MgSO4). Next, a small amount of silica gel was used for vacuum filtration to remove insoluble matter, and the solvent was removed by rotary evaporation. The resulting liquid was named H-XD-YB.
[0030] According to the above operation steps, other parameters remained unchanged to prepare polymer H-XT-YB (X+Y=100; X=0, 1, 3, 5, 10, 20, 30).
[0031] Example 4: Preparation of benzocyclobutene-based polynorbornene composite material The disc-shaped mold product obtained in Example 3 was cured at 280° C. in a nitrogen atmosphere for 3 h; the composite resins after curing were C-XD-YB and C-XT-YB (X+Y=100; X=0, 1, 3, 5, 10, 20, 30), respectively.
[0032] The dielectric properties and thermodynamic properties of the 12 high-performance benzocyclobutene-based polynorbornene composite materials obtained in Example 4 were tested, and the test method was as follows: The test method for dielectric properties is: dielectric constant tester method.
[0033] The testing method for mechanical properties is: dynamic mechanical analyzer method.
[0034] The test method for thermal properties is: thermogravimetric analyzer method.
[0035] The test method for hydrophobic performance is: contact angle tester.
[0036] Table 1 is a comparison of the dielectric properties, mechanical properties and thermal properties of different cured products. Figure 5 This is a comparison chart of the dielectric properties of different cured products. Figure 6 This is a comparison chart of thermal stability tests of different cured products. Figure 7 This is a comparison chart of mechanical properties tests of different cured products. Figure 8 This is a comparison chart of contact angle tests of different cured products.
[0037] Table 1 Comparison of dielectric properties, mechanical properties and thermal properties of different cured products
[0038] From the above test results, we can see that: (1) Dielectric properties: as shown in Table 1 and Figure 5 As shown, at low frequencies 1-10 6 In the Hz range, the dielectric constants of the 12 cured products are all less than 2.6, especially the dielectric constant of the C-5T-95B cured product is only 2.25. It can be seen that the cured product prepared by the present invention has excellent low dielectric properties.
[0039] (2) Mechanical properties: as shown in Table 1 and Figure 7 As shown in the figure, at room temperature, the storage modulus of the six cured products is higher than 3.4 GPa, especially the storage modulus of C-10D-90B and C-20T-80B is as high as 3.9 GPa and 4.1 GPa respectively. It can be seen that the cured product prepared by the present invention has excellent mechanical properties.
[0040] (3) Thermal properties: as shown in Table 1 and Figure 6 As shown, the thermal decomposition temperatures of the 12 kinds of cured products are at least 429° C., and in particular, the thermal decomposition temperature of C-10T-90B is as high as 443° C. It can be seen that the cured products prepared by the present invention have stable thermal properties.
[0041] (4) Hydrophobic properties: Figure 8 As shown, the contact angles of the 12 cured products are all greater than 95°, especially the contact angle of C-5T-95B is as high as 105°. It can be seen that the cured product prepared by the present invention has good hydrophobic properties.
[0042] Although the present invention has been described in detail above with general descriptions and specific embodiments, it is obvious to those skilled in the art that some modifications or improvements may be made thereto based on the present invention. Therefore, these modifications or improvements made without departing from the spirit of the present invention all fall within the scope of protection claimed by the present invention.
Claims
1. A benzocyclobutene-based polynorbornene composite material, the structural formula of which is shown in Formula I: Formula I In the formula, R 1 , R 2 , R 3 Independently selected from C1-C4 alkyl or oxy; The value range of x is 1-100; the value range of y is 1-100.
2. The composite material according to claim 1, Features: The benzocyclobutene-based polynorbornene composite material is any one of the following 1)-14): 1) Composite material C-0D-100B: R 1 is methyl, R 2 and R 3 is an oxygen radical, x is 0, y is 100; 2) Composite material C-1D-99B: R 1 is methyl, R 2 and R 3 is an oxygen radical, x is 1, y is 99; 3) Composite material C-3D-97B: R 1 is methyl, R 2 and R 3 is an oxygen radical, x is 3, y is 97; 4) Composite material C-5D-95B: R 1 is methyl, R 2 and R 3 is an oxygen radical, x is 5, y is 95; 5) Composite material C-10D-90B: R 1 is methyl, R 2 and R 3 is an oxygen radical, x is 10, y is 90; 6) Composite material C-20D-80B: R 1 is methyl, R 2 and R 3 is an oxygen radical, x is 20, y is 80; 7) Composite material C-30D-70B: R 1 is methyl, R 2 and R 3 is an oxygen radical, x is 30, y is 70; 8) Composite material C-0T-100B: R 1 , R 2 and R 3 is an oxygen radical, x is 0, y is 100; 9) Composite C-1T-99B: R 1 , R 2 and R 3 is an oxygen radical, x is 1, y is 99; 10) Composite C-3T-97B: R 1 , R 2 and R 3 is an oxygen radical, x is 3, y is 97; 11) Composite material C-5T-95B: R 1 , R 2 and R 3 is an oxygen radical, x is 5, y is 95; 12) Composite C-10T-90B: R 1 , R 2 and R 3 is an oxygen radical, x is 10, y is 90; 13) Composite material C-20T-80B: R 1 , R 2 and R 3 is an oxygen radical, x is 20, y is 80; 14) Composite material C-30T-70B: R 1 , R 2 and R 3 is an oxygen group, x is 30, and y is 70.
3. The method for preparing the benzocyclobutene-based polynorbornene composite material according to claim 1 or 2, comprising the following steps: S1 and 5-vinylbicyclo[2.2.1]hept-2-ene are subjected to hydrosilylation reaction with dimethoxysilane hydride or trimethoxysilane hydride in the presence of catalyst I to obtain siloxane precursor II and siloxane precursor III; S2, 5-vinylbicyclo[2.2.1]hept-2-ene and silylbenzenecyclobutene undergo a hydrosilylation reaction under the action of the catalyst I to obtain a benzocyclobutene precursor IV; S3, the siloxane precursor II or the siloxane precursor III and the benzocyclobutene precursor IV are subjected to a ROMP polymerization reaction under the action of a catalyst II to obtain a linear benzocyclobutene-based polynorbornene represented by formula V; Formula V In Formula V, R 1 , R 2 , R 3 An alkyl or alkoxy group selected from C1-C4; S4, the linear benzocyclobutenyl polynorbornene represented by formula V is subjected to a condensation reaction under the action of catalyst III to obtain a benzocyclobutenyl polynorbornene crosslinked product represented by formula VI; Formula VI In Formula VI, R 1 , R 2 , R 3 An alkyl or oxy group selected from C1-C4; S5. The benzocyclobutene-based polynorbornene crosslinked product shown in formula VI is thermally cured at high temperature to generate the benzocyclobutene-based polynorbornene composite material.
4. The preparation method according to claim 3, Features: In step S1, the molar ratio of the 5-vinylbicyclo[2.2.1]hept-2-ene to the dimethoxysilane or the trimethoxysilane is 1:1-1.5; The catalyst I is a Karstedt catalyst; The molar ratio of the catalyst I to the trimethoxysilane or the dimethoxysilane is 1:50-100; The conditions of the hydrosilylation reaction are: temperature of 70-90° C. and time of 1-4 h.
5. The preparation method according to claim 3 or 4, Features: In step S2, the molar ratio of the 5-vinylbicyclo[2.2.1]hept-2-ene to the silylbenzenecyclobutene is 1:1-1.5; The molar ratio of the catalyst I to the silicon hydrogen benzocyclobutene is 1:50-60; The conditions of the hydrosilylation reaction are: temperature of 70-90° C. and time of 1-4 h.
6. The preparation method according to any one of claims 3 to 5, Features: In step S2, the catalyst II is a Grubbs catalyst; The molar ratio of the catalyst II to the benzocyclobutene precursor IV is 1:50-60; The ROMP polymerization reaction is carried out in an organic solvent I, wherein the organic solvent I is one or more of tetrahydrofuran, toluene, dichloromethane and dioxane; The conditions of the ROMP polymerization reaction are: temperature of 20-40° C. and time of 1-3 h.
7. The preparation method according to any one of claims 3 to 6, Features: In step S3, the catalyst III is one or more of hydrochloric acid, sulfuric acid, nitric acid and trifluoroacetic acid; By adding the catalyst III, the pH of the reaction system is adjusted to 3-6; The condensation reaction is carried out in an organic solvent II; the organic solvent II is one or more of tetrahydrofuran, dioxane, acetonitrile and dimethyl sulfoxide; The conditions of the condensation reaction are: temperature of 20-30°C and time of 12-15h.
8. The preparation method according to any one of claims 3 to 7, Features: In step S5, the temperature of the thermal curing is 250-350°C.
9. A packaging material made from the benzocyclobutene-based polynorbornene composite material according to claim 1 or 2.
Citation Information
Patent Citations
Benzocyclobutene monomers containing siloxane and imide structure and synthesis and application thereof
CN102503970A
Benzocyclobutene functional organic silicone resin and preparation method thereof
CN107987278A
Polynorbornene mesogen-jacketed liquid crystal polymer with side chain containing polyhedral oligomeric silsesquioxane and preparation method thereof
CN113307952A
Cited By
Anthryl siloxane benzocyclobutene photoetching resin based on ultraviolet light response, preparation method and application thereof and packaging material
CN122255419A