Preparation method of antibacterial polyvinyl alcohol film and product thereof

By introducing indole derivatives into polyvinyl alcohol films, the problem of insufficient mechanical strength and antibacterial properties of polyvinyl alcohol films is solved, and the effect of significantly improving the antibacterial effect and expanding the scope of application is achieved.

CN118994665APending Publication Date: 2024-11-22GUIZHOU MATERIAL IND TECH INSTITUE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410921335.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-10
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Polyvinyl alcohol films have poor mechanical strength and lack antibacterial properties after film formation, which limits their use range and life.

Method used

PEG is used as a plasticizer and crosslinking agent to introduce indole derivatives, and the antibacterial polyvinyl alcohol film is prepared by reacting double-ended amino polyethylene glycol with indole derivatives, and the antibacterial effect of indole is used to impart the film. Antibacteriality.

Benefits of technology

It significantly improves the antibacterial properties of polyvinyl alcohol films, expands its scope of application and use, and maintains phase transformation performance and plasticization effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994665A_ABST
    Figure CN118994665A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of an antibacterial polyvinyl alcohol film and a product thereof, and the preparation method comprises the following steps: pouring a PEG-NH2 mixed solution into an indoleacetic acid mixed solution for reaction, and freeze-drying to obtain a product NPEG / IAA; the preparation method comprises the following steps: adding PVA into dimethyl sulfoxide DMSO to prepare a PVA-DMSO solution, adding NPEG / IAA, heating until stirring for reaction, carrying out vacuum defoaming, pouring a film coating solution on a coating machine for film scraping, heating for drying, and uncovering the film to obtain the PVA / NPEG / IAA film. According to the invention, the amino-terminated polyethylene glycol molecules and the indole derivative are subjected to reaction grafting, and the introduced indole derivative is used as an antibacterial substance, so that the raw materials are easy to obtain, the cost is low, and the antibacterial effect is remarkable, and therefore, the polyvinyl alcohol film is endowed with antibacterial property and excellent mechanical strength; the defect that polyvinyl alcohol is lack of antibacterial property and mechanical property after film forming is overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of film preparation, and specifically relates to a preparation method of an antibacterial polyvinyl alcohol film and a product thereof. Background Art

[0002] Polyvinyl alcohol (PVA) film has outstanding hydrophilicity, oxygen barrier, oil resistance and chemical corrosion resistance, but it has problems such as poor mechanical strength after film formation and lack of antibacterial properties. Plasticizer molecules can be inserted between polymer molecular chains, weaken the intermolecular forces, increase the distance and activity space between polymer molecular chains, enhance the plasticity of polymers, and reduce the processing temperature of polymers. Organic small molecules such as polyols, amines, amides and metal ion compounds all have good plasticizing effects. By adding plasticizers to polyvinyl alcohol, the melting point of polyvinyl alcohol can be lowered while the decomposition temperature remains basically unchanged, solving the problem of polyvinyl alcohol being difficult to plasticize and improving the mechanical strength of polyvinyl alcohol film.

[0003] Obvious bacterial growth can be observed in polyvinyl alcohol solution after being stored at room temperature for a period of time. Polyvinyl alcohol after film formation also has no antibacterial effect, and its scope of use and life span will be limited due to bacterial growth and the formation of biofilm. Polyvinyl alcohol itself lacks antibacterial properties, and usually requires the addition of antibacterial molecules to impart antibacterial properties. Indole, as a typical nitrogen-containing polycyclic aromatic compound, is widely present in nature, including from animal feces, secretions of plant microorganisms, and remains of animals and plants. Studies have shown that indole derivatives have multiple pharmacological activities, such as antibacterial, antioxidant, anti-inflammatory and analgesic effects.

[0004] At present, Zhang Mo (Preparation and Performance Optimization of Polyethylene Glycol / Chitosan-based Composite Phase Change Materials) chemically cross-linked the aldehyde- and amino-modified polyethylene glycol with chitosan, and designed a polyvinyl alcohol / chitosan double network to further improve its heat storage performance. The addition of PVA improved the heat storage performance, thermal stability and shape stability of the raw materials. Summary of the invention

[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0006] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0007] Therefore, the object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing an antibacterial polyvinyl alcohol film.

[0008] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing an antibacterial polyvinyl alcohol film, comprising:

[0009] Take PEG and heat it in deionized water to dissolve it, add p-aminobenzoic acid, stir it at room temperature until it becomes viscous, and freeze-dry it to obtain PEG-NH2;

[0010] Dissolve indoleacetic acid in dimethylacetamide, add carbodiimide hydrochloride EDCl and 4-dimethylaminopyridine DMAP, and stir evenly at room temperature to obtain an indoleacetic acid mixed solution;

[0011] Dissolving PEG-NH2 in dimethylacetamide to prepare a PEG-NH2 mixed solution;

[0012] The PEG-NH2 mixture was poured into the indoleacetic acid mixture for reaction, and freeze-dried to obtain the product NPEG / IAA;

[0013] PVA is added to dimethyl sulfoxide (DMSO) to prepare PVA-DMSO solution, NPEG / IAA is added, the temperature is raised to stir for reaction, vacuum degassing is performed, the coating liquid is poured onto a coating machine and the film is scraped, and the film is peeled off after heating and drying to obtain a PVA / NPEG / IAA film.

[0014] As a preferred embodiment of the preparation method of the present invention, the PEG is heated and dissolved in deionized water, wherein the heating temperature is 60-80°C.

[0015] As a preferred embodiment of the preparation method of the present invention, the molar ratio of PEG to p-aminobenzoic acid is 1:12-15.

[0016] As a preferred embodiment of the preparation method of the present invention, the ratio of indoleacetic acid, dimethylacetamide, carbodiimide hydrochloride and 4-dimethylaminopyridine in the indoleacetic acid mixed solution is 0.4g:20mL:0.35g:0.03g.

[0017] As a preferred embodiment of the preparation method of the present invention, the PEG-NH2 mixed solution comprises PEG-NH2 and dimethylacetamide in a ratio of 0.3 g:10 mL.

[0018] As a preferred embodiment of the preparation method of the present invention, the PEG-NH2 mixed solution is poured into the indoleacetic acid mixed solution for reaction, wherein the ratio of PEG-NH2 to indoleacetic acid is 0.2-0.3 g:0.4 g.

[0019] As a preferred embodiment of the preparation method of the present invention, the reaction time is 12 to 24 hours.

[0020] As a preferred embodiment of the preparation method of the present invention, wherein: PVA is added into dimethyl sulfoxide (DMSO) to prepare a PVA-DMSO solution, wherein the mass concentration of the solution is 8-10%.

[0021] As a preferred solution of the preparation method of the present invention, the mass percentage of NPEG / IAA in the PVA-DMSO solution is 8-10%.

[0022] Another object of the present invention is to overcome the deficiencies in the prior art and provide an antibacterial polyvinyl alcohol film prepared by a method for preparing the antibacterial polyvinyl alcohol film.

[0023] Beneficial effects of the present invention:

[0024] (1) The present invention uses polyethylene glycol as a plasticizer and a crosslinking agent, and introduces indole derivatives to prepare a polyvinyl alcohol antibacterial film. The hydroxyl group at the end of the long chain of polyethylene glycol has high reactivity and is easy to be modified. In addition, its long chain is inert and can still retain its own phase change properties after modification, and has a good plasticizing effect.

[0025] (2) In the present invention, polyethylene glycol molecules with double-terminal amino groups are reacted and grafted with indole derivatives. The introduced indole derivatives are not only easy to obtain raw materials and low in cost as antibacterial substances, but also have significant antibacterial effects, thereby giving the polyvinyl alcohol film antibacterial properties, overcoming the deficiency of polyvinyl alcohol lacking antibacterial properties after film formation, and helping to expand its scope of application and field of use. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0027] Figure 1 This is a comparison chart of the inhibition zones before and after polyvinyl alcohol is loaded with indole in an embodiment of the present invention. DETAILED DESCRIPTION

[0028] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0029] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0030] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0031] In the embodiment of the present invention, indole is one of indoleacetic acid, indolepropionic acid and indolebutyric acid;

[0032] The polyethylene glycol is one of PEG 2000, PEG 4000, PEG 6000, and PEG 8000;

[0033] The polyvinyl alcohol is one of 0588, 0788, 2488, 1799, 1788, Kuraray 217 and 117.

[0034] Film testing method in the embodiment of the present invention:

[0035] Mechanical properties: The tensile strength and elongation at break of the film were determined using the national standard GB / T 1040.3-2006 Test of tensile properties of plastics Part 3 Test conditions for thin plastics and sheets;

[0036] Antibacterial properties: The concentration is 10 7 cfu / mL of Escherichia coli suspension was used for antibacterial test. The film was cut into 6 mm discs and placed on the plate evenly coated with the bacterial suspension. The film discs were gently pressed to make them fully contact. Three parallel groups were used for each group.

[0037] After incubation at 37°C for 24 h, the diameter of the inhibition zone was measured and the average value was taken.

[0038] Example 1

[0039] (1) Take a certain amount of PEG6000 and heat it to 70°C in deionized water to dissolve it. Add p-aminobenzoic acid (PABA) with a molar ratio of PEG to PABA of 1:15. Stir at room temperature until it becomes viscous. The product (PEG-NH2) is freeze-dried and set aside.

[0040] (2) 0.4 g of indoleacetic acid (IAA, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., purity 98%) was dissolved in 20 mL of dimethylacetamide (DMAc), 0.35 g of carbodiimide hydrochloride (EDCl) and 0.03 g of 4-dimethylaminopyridine (DMAP) were added, and stirred at room temperature;

[0041] 0.3 g of PEG-NH2 solution dissolved in 10 mL of DMAc was poured into the solution and the reaction was continued for 24 h. The product NPEG / IAA was obtained by freeze drying.

[0042] (3) PVA was added to dimethyl sulfoxide (DMSO) to prepare a 10% solution, and 2% by mass of NPEG / IAA was added at the same time. The temperature was raised to 90°C and stirred for reaction for 2 h. After vacuum degassing, the coating solution was poured onto a coating machine and scraped. After heating and drying at 40°C, the film was peeled off to obtain a PVA / NPEG6000 / IAA film.

[0043] Comparison of inhibition zones before and after polyvinyl alcohol loading with indole Figure 1 .

[0044] Example 2

[0045] (1) Take a certain amount of PEG2000 and heat it to 70°C in deionized water to dissolve it. Add p-aminobenzoic acid (PABA) with a molar ratio of PEG to PABA of 1:15. Stir at room temperature until it becomes viscous. The product (PEG-NH2) is freeze-dried and set aside.

[0046] (2) 0.4 g of indoleacetic acid (IAA, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., purity 98%) was dissolved in 20 mL of dimethylacetamide (DMAc), 0.35 g of carbodiimide hydrochloride (EDCl) and 0.03 g of 4-dimethylaminopyridine (DMAP) were added, and stirred at room temperature;

[0047] 0.3 g of PEG-NH2 solution dissolved in 10 mL of DMAc was poured into the solution and the reaction was continued for 24 h. The product NPEG / IAA was obtained by freeze drying.

[0048] (3) PVA was added to dimethyl sulfoxide (DMSO) to prepare a 10% solution, and 2% by mass of NPEG / IAA was added at the same time. The temperature was raised to 90°C and stirred for reaction for 2 h. After vacuum degassing, the coating solution was poured onto a coating machine and scraped. After heating and drying at 40°C, the film was peeled off to obtain a PVA / NPEG2000 / IAA film.

[0049] Example 3

[0050] (1) Take a certain amount of PEG4000 and heat it to 70°C in deionized water to dissolve it. Add p-aminobenzoic acid (PABA) with a molar ratio of PEG to PABA of 1:15. Stir at room temperature until it becomes viscous. The product (PEG-NH2) is freeze-dried and set aside.

[0051] (2) 0.4 g of indoleacetic acid (IAA, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., purity 98%) was dissolved in 20 mL of dimethylacetamide (DMAc), 0.35 g of carbodiimide hydrochloride (EDCl) and 0.03 g of 4-dimethylaminopyridine (DMAP) were added, and stirred at room temperature;

[0052] 0.3 g of PEG-NH2 solution dissolved in 10 mL of DMAc was poured into the solution and the reaction was continued for 24 h. The product NPEG / IAA was obtained by freeze drying.

[0053] (3) PVA was added to dimethyl sulfoxide (DMSO) to prepare a 10% solution, and 2% by mass of NPEG / IAA was added at the same time. The temperature was raised to 90°C and stirred for reaction for 2 h. After vacuum degassing, the coating solution was poured onto a coating machine and scraped. After heating and drying at 40°C, the film was peeled off to obtain a PVA / NPEG4000 / IAA film.

[0054] Example 4

[0055] (1) Take a certain amount of PEG8000 and heat it to 70°C in deionized water to dissolve it. Add p-aminobenzoic acid (PABA) with a molar ratio of PEG to PABA of 1:15. Stir at room temperature until it becomes viscous. The product (PEG-NH2) is freeze-dried and set aside.

[0056] (2) 0.4 g of indoleacetic acid (IAA, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., purity 98%) was dissolved in 20 mL of dimethylacetamide (DMAc), 0.35 g of carbodiimide hydrochloride (EDCl) and 0.03 g of 4-dimethylaminopyridine (DMAP) were added, and stirred at room temperature;

[0057] 0.3 g of PEG-NH2 solution dissolved in 10 mL of DMAc was poured into the solution and the reaction was continued for 24 h. The product NPEG / IAA was obtained by freeze drying.

[0058] (3) PVA was added to dimethyl sulfoxide (DMSO) to prepare a 10% solution, and 2% by mass of NPEG / IAA was added at the same time. The temperature was raised to 90°C and stirred for reaction for 2 h. After vacuum degassing, the coating solution was poured onto a coating machine and scraped. The film was dried at 40°C and then peeled off to obtain a PVA / NPEG8000 / IAA film.

[0059] Comparative Example 1 (PVA)

[0060] PVA was added to DMSO to prepare a 10% solution, and the temperature was raised to 90°C and stirred for reaction for 2 hours. After vacuum degassing, the coating solution was poured onto a coating machine to scrape the film, and the film was removed after heating and drying at 40°C.

[0061] Comparative Example 2 (PVA / PEG)

[0062] PVA was added to DMSO to prepare a 10% solution, and 2% by mass of PEG was added at the same time, and the temperature was raised to 90°C and stirred for reaction for 2 hours;

[0063] After vacuum degassing, pour the above coating liquid onto a coating machine to scrape the film, heat and dry at 40°C, and then peel off the film.

[0064] Comparative Example 3 (PVA / IAA)

[0065] Take 0.4g IAA (purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., purity 98%) and dissolve it in 20mL DMAc, add 0.35g EDCl and 0.03g DMAP, and stir evenly at room temperature;

[0066] PVA was added to DMSO to prepare a 10% solution, the temperature was raised to 90°C and stirred for reaction for 2 hours. After complete dissolution, the temperature was lowered to 40°C, and the above-mentioned IAA solution (2% mass fraction) was added to continue the reaction for 5 hours. After vacuum degassing of the coating liquid, it was poured onto a coating machine for film scraping, and the film was removed after heating and drying at 40°C.

[0067] The experimental results are shown in Table 1.

[0068] Table 1

[0069] Tensile strength / MPa Elongation at break / % Inhibition zone / mm Example 1 (PVA / NPEG6000 / IAA) 31.75 341.94 15.6 Example 2 (PVA / NPEG2000 / IAA) 23.65 254.84 16.14 Example 3 (PVA / NPEG4000 / IAA) 28.77 263.14 16.53 Example 4 (PVA / NPEG8000 / IAA) 27.42 222.13 15.24 Comparative Example 1 (PVA) 17.59 210.8 0 Comparative Example 2 (PVA / PEG6000) 39.04 474.73 0 Comparative Example 3 (PVA / IAA) 17.01 204.83 17.2

[0070] As can be seen from Table 1, after adding PEG, the intermolecular hydrogen bonding effect improves the mechanical properties of the film; the tensile strength and elongation at break increase with the increase of NPEG molecular weight. When the molecular weight is 8000, due to the large molecular weight, the cross-linking effect between PVA and NPEG reaches saturation, and the mechanical properties no longer increase; after adding IAA, the cross-linking of PVA is destroyed, and defects are prone to occur, resulting in a decrease in mechanical properties; IAA gives the film antibacterial properties, and a clear inhibition zone appears compared to the film without adding IAA.

[0071] In Comparative Example 3, 2% by mass of IAA is directly added to PVA. In Example 1, modified PEG / IAA is added to PVA, wherein the grafted amount of IAA is less than 2% by mass. Therefore, the diameter of the inhibition zone is smaller than that of Comparative Example 3.

[0072] Comparative Example 4

[0073] Without adding EDCl and DMAP as activators, the remaining experimental conditions were the same as those in Example 1, and the specific conditions were as follows:

[0074] (1) Take a certain amount of PEG6000 and heat it to 70°C in deionized water to dissolve it. Add p-aminobenzoic acid (PABA) with a molar ratio of PEG to PABA of 1:15. Stir at room temperature until it becomes viscous. The product (PEG-NH2) is freeze-dried and set aside.

[0075] (2) 0.4 g of indoleacetic acid (IAA, purchased from Shanghai Aladdin Biochemical Technology Co., Ltd., purity 98%) was dissolved in 20 mL of dimethylacetamide (DMAc), and stirred at room temperature to obtain a mixed solution;

[0076] 0.3 g of PEG-NH2 solution dissolved in 10 mL of DMAc was poured into the solution and the reaction was continued for 24 h. The product NPEG / IAA was obtained by freeze drying.

[0077] (3) PVA was added to dimethyl sulfoxide (DMSO) to prepare a 10% solution, and 2% by mass of NPEG / IAA was added at the same time. The temperature was raised to 90°C and stirred for reaction for 2 h. After vacuum degassing, the coating solution was poured onto a coating machine and scraped. The film was dried at 40°C and then peeled off to obtain a thin film.

[0078] The measurement results are shown in Table 2.

[0079] Table 2

[0080] Tensile strength / MPa Elongation at break / % Inhibition zone / mm Example 1 (PVA / NPEG6000 / IAA) 31.75 341.94 15.6 Comparative Example 4 (PVA / NPEG6000 / IAA) 38.83 440.90 10.4

[0081] As can be seen from Table 2, the amidation reaction between the aminated PEG and IAA occurs, and the antibacterial effect of the film is obvious. When no activator is added, the amidation reaction is weakened, and the antibacterial effect of the film is affected; however, after PEG is aminated, the hydrogen bonding effect with PVA is weakened, and the mechanical properties are lower than those of the film with direct addition of PEG.

[0082] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.

Claims

1. A method for preparing an antibacterial polyvinyl alcohol film, Features: include, Take PEG and heat it in deionized water to dissolve it, add p-aminobenzoic acid, stir it at room temperature until it becomes viscous, and freeze-dry it to obtain PEG-NH 2 ; Dissolve indoleacetic acid in dimethylacetamide, add carbodiimide hydrochloride EDCl and 4-dimethylaminopyridine DMAP, and stir evenly at room temperature to obtain an indoleacetic acid mixed solution; PEG-NH 2 Dissolve in dimethylacetamide to prepare PEG-NH 2 Mixed liquid; PEG-NH 2 The mixed solution is poured into the indoleacetic acid mixed solution for reaction, and freeze-dried to obtain the product NPEG / IAA; PVA is added to dimethyl sulfoxide (DMSO) to prepare PVA-DMSO solution, NPEG / IAA is added, the temperature is raised to stir for reaction, vacuum degassing is performed, the coating liquid is poured onto a coating machine and the film is scraped, and the film is peeled off after heating and drying to obtain a PVA / NPEG / IAA film.

2. The preparation method according to claim 1, Features: The PEG is heated and dissolved in deionized water, wherein the heating temperature is 60-80°C.

3. The preparation method according to claim 1 or 2, Features: The molar ratio of PEG to p-aminobenzoic acid is 1:12-15.

4. The preparation method according to claim 3, Features: The indoleacetic acid mixed solution comprises indoleacetic acid, dimethylacetamide, carbodiimide hydrochloride and 4-dimethylaminopyridine in a ratio of 0.4 g:20 mL:0.35 g:0.03 g.

5. The preparation method according to claim 1 or 4, Features: The PEG-NH 2 The mixture, in which PEG-NH 2 The ratio with dimethylacetamide is 0.3g:10mL.

6. The preparation method according to claim 5, Features: The PEG-NH 2 The mixture was poured into the indoleacetic acid mixture for reaction, wherein PEG-NH 2 The ratio with indoleacetic acid is 0.2~0.3g:0.4g.

7. The preparation method according to claim 6, Features: The reaction time is 12 to 24 hours.

8. The preparation method according to claim 1, Features: The PVA is added into dimethyl sulfoxide (DMSO) to prepare a PVA-DMSO solution, wherein the mass concentration of the solution is 8-10%.

9. The preparation method according to claim 1 or 8, Features: The mass percentage of the NPEG / IAA in the PVA-DMSO solution is 8-10%.

10. The PVA / NPEG / IAA film prepared by the preparation method according to any one of claims 1 to 9.