Whitening agent free of indoor and outdoor color difference as well as preparation method and application of whitening agent

By grafting the fluorescent whitening agent on titanium dioxide and compounding it with modified polyvinyl alcohol, the problem of precipitation of the fluorescent whitening agent in the foaming material is solved, and the colorless color difference and high-performance whitening effect in indoor and outdoor is achieved, improving the Mechanics and stability of foaming materials.

CN118994731AInactive Publication Date: 2024-11-22BOXUN CHEMICAL TECHNOLOGY (HENAN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411041643.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing fluorescent whitening agents are prone to precipitation in foaming materials, resulting in chromatic aberration, and their ultraviolet absorption range is narrow, resulting in different reflective fluorescence intensity during indoor and outdoor use, resulting in chromatic aberration of products.

Method used

Modified titanium dioxide and modified polyvinyl alcohol are combined with foaming of specific ratios by grafting the fluorescent whitening agent 4,4'-diaminodisylene-2,2'-disulfonic acid on the titanium dioxide. , an indoor and outdoor color-free whitening agent with a wide ultraviolet absorption band and is not easy to precipitate.

Benefits of technology

The ultraviolet absorption range of foamed materials is expanded, the cell stability, mechanical properties and weather resistance are improved, the color difference is avoided, and the overall performance of foamed materials is improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the field of whitening agents, in particular to an indoor and outdoor color-difference-free whitening agent and a preparation method and application thereof.The indoor and outdoor color-difference-free whitening agent is prepared from, by weight, 75-85 parts of modified titanium dioxide, 10-15 parts of foaming agent and 10-20 parts of modified polyvinyl alcohol. The produced whitening agent free of indoor and outdoor color difference has a wide ultraviolet absorption wave band, is suitable for foaming material products, and can improve the mechanical property and foaming effect of foaming materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of brighteners, and in particular to a brightener with no color difference indoors and outdoors, and a preparation method and application thereof. Background Art

[0002] Fluorescent whitening agent, commonly known as white dye, is a fluorescent dye that contains conjugated double bonds in its structure and has planarity. The reason why fluorescent whitening agent can have a whitening effect on products is that it can absorb ultraviolet light and excite blue or blue-purple fluorescence, which can shield yellow light. Fluorescent whitening agents are mainly divided into several types according to the type of parent body, such as diphenylethylene type, coumarin type, and phthalamide. Among them, diphenylethylene type fluorescent whitening agents have the advantages of high fluorescence quantum yield, high chemical stability, and good whitening effect, and are widely used in textiles, plastics, detergents, cosmetics, papermaking and other fields. In foaming materials such as PVC and EVA, fluorescent whitening agents have the problem of easy precipitation and affecting the whitening effect. In addition, the existing fluorescent whitening agents absorb a narrow range of ultraviolet bands, so that when the products absorb light of different bands indoors and outdoors, the reflected fluorescence intensity is different, resulting in color difference of the products seen by the naked eye.

[0003] Patent CN115260115A discloses a fluorescent whitening agent with no color difference for indoor and outdoor use and a preparation method thereof. The raw materials for producing the fluorescent whitening agent with no color difference for indoor and outdoor use include the following components by weight: 4-methylphenylbenzoxazole, sulfur powder, xylene and refined solvent. The fluorescent whitening agent has a wide ultraviolet absorption band and can also absorb natural visible light. When applied to plastics, the color difference is very small. However, the fluorescent whitening agent with no color difference for indoor and outdoor use has a low molecular weight and is easily precipitated from the foaming material, causing the foaming material to turn yellow.

[0004] Patent CN109503890B discloses a chemical composite brightener for polyurethane sponge and a preparation method thereof, wherein the composite brightener comprises an inorganic brightener, a blue pigment, a fluorescent brightener, an anti-settling stabilizer, a solubilizer, a hue regulator, a dispersion medium and a free radical scavenger. The composite brightener can be used to prepare polyurethane sponge, and the prepared polyurethane sponge is not easy to delaminate, has a long-lasting whitening effect and is not easy to turn yellow under strong light, but the problem of easy precipitation of the fluorescent brightener is not solved.

[0005] Therefore, there is an urgent need in the market for a whitening agent that is suitable for foaming materials and is not easy to precipitate and has no color difference indoors and outdoors. Summary of the invention

[0006] In view of the problems existing in the prior art, the purpose of the present invention is to obtain a whitening agent with a wide ultraviolet absorption band, suitable for foaming materials, not easy to precipitate, and no color difference indoors and outdoors.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] The first aspect of the present invention provides a whitening agent with no color difference between indoors and outdoors, which comprises the following raw materials in parts by weight: 75-85 parts of modified titanium dioxide, 10-15 parts of foaming agent, and 10-20 parts of modified polyvinyl alcohol.

[0009] The present invention discloses a whitening agent with no color difference indoors and outdoors obtained by compounding modified titanium dioxide, a foaming agent and modified polyvinyl alcohol. The whitening agent has a wide ultraviolet absorption band, is suitable for foaming materials and is not easy to precipitate.

[0010] In some embodiments, the foaming agent is one or more of azobisisobutyronitrile, benzenesulfonylhydrazide, dinitrosopentamethylenetetramine, and azodicarbonamide.

[0011] Preferably, the blowing agent is azodicarbonamide.

[0012] In some embodiments, the method for preparing the modified titanium dioxide comprises the following steps:

[0013] A1. Add 3-isocyanate propyltrimethoxysilane and titanium dioxide into a reaction vessel, raise the temperature to 80-100° C. and react for 3-6 hours to obtain titanium dioxide containing an isocyanate group;

[0014] A2, adding the titanium dioxide containing isocyanate groups and ethylenediamine obtained in step A1 into a reaction vessel, heating to 80-100° C., reacting for 5-6 hours, to obtain titanium dioxide containing amino groups;

[0015] A3, dissolving 4,4'-diaminostilbene-2,2'-disulfonic acid in a 30-50wt% sodium hydroxide aqueous solution, then adding it to a mixed solution of cyanuric chloride and acetone, reacting at 2-5°C for 1-3h, and drying to obtain modified 4,4'-diaminostilbene-2,2'-disulfonic acid;

[0016] A4. Add the amino-containing titanium dioxide obtained in step A2, the modified 4,4'-diaminostilbene-2,2'-disulfonic acid obtained in step A3 and acetone into a reaction container, react at 70-90° C. for 2-4 hours, and obtain modified titanium dioxide after drying.

[0017] The present application prepares modified titanium dioxide by reacting titanium dioxide containing isocyanate groups with ethylenediamine, and reacting the titanium dioxide with a fluorescent brightener 4,4'-diaminostilbene-2,2'-disulfonic acid to achieve the loading of 4,4'-diaminostilbene-2,2'-disulfonic acid segments on titanium dioxide, making it difficult to precipitate from the foaming material. Adding modified titanium dioxide to the foaming material can not only make the foaming material have a wider ultraviolet absorption band, but also improve the foaming material's pore stability, mechanical properties and weather resistance. At the same time, the siloxane segments and 4,4'-diaminostilbene-2,2'-disulfonic acid segments on the modified titanium dioxide can promote the dispersion of titanium dioxide in the foaming material, further improving the various properties of the foaming material.

[0018] In some embodiments, the mass ratio of titanium dioxide to 3-isocyanatepropyltrimethoxysilane in step A1 is 1:(0.1-0.3).

[0019] The present application can further improve the foaming performance of the foaming material by selecting a specific ratio of 3-isocyanatepropyltrimethoxysilane. This may be because some isocyanate groups remaining on the modified titanium dioxide can react with ammonia water to release carbon dioxide, making the interior of the foaming material have a denser microporous structure, thereby improving the mechanical properties of the foaming material.

[0020] In some embodiments, the mass ratio of titanium dioxide containing isocyanate groups to ethylenediamine in step A2 is 1:(0.03-0.05).

[0021] The present application can further improve the foaming performance of the foaming material by specifically regulating the ratio of titanium dioxide containing isocyanate groups and ethylenediamine. This may be because by strictly controlling the ratio of the two, some isocyanate groups can still remain after the reaction of ethylenediamine and modified titanium dioxide, which can react with ammonia water to release carbon dioxide, so that the interior of the foaming material has a denser microporous structure, thereby improving the mechanical properties of the foaming material.

[0022] In some embodiments, the mass ratio of the amino-containing titanium dioxide to the modified 4,4'-diaminostilbene-2,2'-disulfonic acid in step A4 is 1:(0.2-0.4).

[0023] The present application can further improve the whitening effect of the whitening agent and the mechanical properties of the foaming material by selecting a specific ratio of modified 4,4'-diaminostilbene-2,2'-disulfonic acid. This may be because under this ratio, more modified 4,4'-diaminostilbene-2,2'-disulfonic acid segments can be grafted onto titanium dioxide, so that the modified titanium dioxide has better compatibility with the foaming material, and the residual modified 4,4'-diaminostilbene-2,2'-disulfonic acid in the system is less and less difficult to precipitate, so that the foaming material is less likely to have color difference during long-term use.

[0024] In some embodiments, the method for preparing the modified polyvinyl alcohol comprises the following steps:

[0025] B1. Add vinyl acetate, methanol and 30-40 wt% styrene toluene solution into a reaction vessel, heat to 60-70°C, stir for 5-10 min, add azobisisobutyronitrile, react for 6h-7h, and obtain a polymer after drying;

[0026] B2. Add the polymer obtained in step B1 and methanol into a reaction container, heat to 30° C.-50° C., add 4-6 wt % of a methanol solution of sodium hydroxide, react for 10 min-30 min, wash and dry to obtain modified polyvinyl alcohol.

[0027] In some embodiments, the number average molecular weight of the polymer is 2000-4000.

[0028] The present application introduces polyvinyl alcohol containing some styrene chain segments into the whitening agent system. The polyvinyl alcohol chain segments can adjust the viscosity of the foaming material, and the low molecular weight modified polyvinyl alcohol can decompose during heating to produce water vapor, carbon dioxide, ethylene and other gases, which can further reduce the density of the foaming material and make the interior of the foaming material have denser micropores. The styrene chain segments can enhance the compatibility of the polyvinyl alcohol chain segments with the foaming material and increase the rigidity of the foaming material. The styrene chain segments can also produce π-π effects with the benzene rings on the modified titanium dioxide, thereby improving the compatibility among the foaming material, modified titanium dioxide and modified polyvinyl alcohol, and thus improving the mechanical properties of the foaming material.

[0029] In some embodiments, the mass ratio of the vinyl acetate to a 30-40 wt % styrene toluene solution is 1:(1.1-1.3).

[0030] The present application can ensure that the modified polyvinyl alcohol has good compatibility with the foaming material and that the brightener has good foaming performance by selecting a specific ratio of 30-40wt% styrene toluene solution.

[0031] The second aspect of the present invention provides a method for preparing a whitening agent with no color difference between indoors and outdoors, comprising the following steps: adding a foaming agent and modified polyvinyl alcohol to modified titanium dioxide, and stirring at room temperature for 5-15 minutes to obtain the whitening agent.

[0032] The third aspect of the present invention provides an application of a whitening agent with no color difference indoors and outdoors. The whitening agent can be used in PVC or EVA foaming polymers, and the addition amount is 2.5-3.5wt% of the polymer. At the same time, 25-28wt% of ammonia water needs to be added, and the addition amount is 0.5-1wt% of the polymer.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] (1) The present invention obtains a whitening agent with no color difference indoors and outdoors by compounding modified titanium dioxide, a foaming agent and modified polyvinyl alcohol. The whitening agent has a wide ultraviolet absorption band and is not easy to precipitate from the foaming material, and can improve the foaming effect and mechanical properties of the foaming material.

[0035] (2) The present application grafts the fluorescent brightener 4,4'-diaminostilbene-2,2'-disulfonic acid onto titanium dioxide, making it difficult for the fluorescent brightener to precipitate from the foaming material. Adding the modified titanium dioxide to the foaming material can not only make the foaming material have a wider ultraviolet absorption band, but also improve the foaming effect and mechanical properties of the foaming material. At the same time, the siloxane segments and 4,4'-diaminostilbene-2,2'-disulfonic acid segments on the modified titanium dioxide can promote the dispersion of titanium dioxide in the foaming material, further improving the various properties of the foaming material. In addition, the present application limits the ratio of each substance so that some isocyanate groups remaining on the modified titanium dioxide can react with ammonia water to release carbon dioxide, thereby forming a denser microporous structure inside the foaming material.

[0036] (3) The present invention introduces polyvinyl alcohol containing some styrene chain segments into the whitening agent system, wherein the polyvinyl alcohol chain segments can reduce the density of the foaming material by adjusting the viscosity of the foaming material and generating gas through decomposition, and the benzene ring can increase the rigidity of the foaming material and can also produce π-π effect with the benzene ring on the modified titanium dioxide, thereby improving the compatibility among the foaming material, modified titanium dioxide and modified polyvinyl alcohol, thereby improving the mechanical properties of the foaming material. DETAILED DESCRIPTION

[0037] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0038] In the following examples and comparative examples, except for modified titanium dioxide and modified polyvinyl alcohol, the other compounds and related reagents used can be purchased from the market, among which the model of titanium dioxide is R-105, purchased from Shijiazhuang Yayou Chemical Co., Ltd.; the model of PVC resin is P450, purchased from Yuyao Ruijing Plastic Chemical Co., Ltd.

[0039] Preparation Example 1

[0040] The preparation method of modified titanium dioxide-1 comprises the following steps:

[0041] A1. Add 2 g of 3-isocyanatepropyltrimethoxysilane and 10 g of titanium dioxide into a reaction container, raise the temperature to 90° C. and react for 4 h to obtain titanium dioxide containing an isocyanate group;

[0042] A2, adding 10g of titanium dioxide containing isocyanate groups obtained in step A1 and 0.4g of ethylenediamine into a reaction container, heating to 90°C, reacting for 5.5h, to obtain titanium dioxide containing amino groups;

[0043] A3, 5g of 4,4'-diaminostilbene-2,2'-disulfonic acid was dissolved in 10g of 40wt% sodium hydroxide aqueous solution, and then added to a mixed solution of 5g of cyanuric chloride and 20g of acetone, reacted at 3°C ​​for 2h, and dried to obtain modified 4,4'-diaminostilbene-2,2'-disulfonic acid;

[0044] A4. Add 10 g of amino-containing titanium dioxide obtained in step A2, 3 g of modified 4,4'-diaminostilbene-2,2'-disulfonic acid obtained in step A3 and 30 g of acetone into a reaction container, and react at 80° C. for 3 h to obtain modified titanium dioxide-1.

[0045] Preparation Example 2

[0046] The preparation method of modified titanium dioxide-2 comprises the following steps:

[0047] A1. Add 0.5 g of 3-isocyanatepropyltrimethoxysilane and 10 g of titanium dioxide into a reaction container, heat to 90° C. and react for 4 h to obtain titanium dioxide containing an isocyanate group;

[0048] A2, adding 10g of titanium dioxide containing isocyanate groups obtained in step A1 and 0.4g of ethylenediamine into a reaction container, heating to 90°C, reacting for 5.5h, to obtain titanium dioxide containing amino groups;

[0049] A3, 5g of 4,4'-diaminostilbene-2,2'-disulfonic acid was dissolved in 10g of 40wt% sodium hydroxide aqueous solution, and then added to a mixed solution of 5g of cyanuric chloride and 20g of acetone, reacted at 3°C ​​for 2h, and dried to obtain modified 4,4'-diaminostilbene-2,2'-disulfonic acid;

[0050] A4. Add 10 g of amino-containing titanium dioxide obtained in step A2, 3 g of modified 4,4'-diaminostilbene-2,2'-disulfonic acid obtained in step A3 and 30 g of acetone into a reaction container, and react at 80° C. for 3 h to obtain modified titanium dioxide-2.

[0051] Preparation Example 3

[0052] The preparation method of modified titanium dioxide-3 comprises the following steps:

[0053] A1. Add 2 g of 3-isocyanatepropyltrimethoxysilane and 10 g of titanium dioxide into a reaction container, raise the temperature to 90° C. and react for 4 h to obtain titanium dioxide containing an isocyanate group;

[0054] A2, adding 10g of titanium dioxide containing isocyanate groups obtained in step A1 and 0.6g of ethylenediamine into a reaction container, heating to 90°C, reacting for 5.5h, to obtain titanium dioxide containing amino groups;

[0055] A3, 5g of 4,4'-diaminostilbene-2,2'-disulfonic acid was dissolved in 10g of 40wt% sodium hydroxide aqueous solution, and then added to a mixed solution of 5g of cyanuric chloride and 20g of acetone, reacted at 3°C ​​for 2h, and dried to obtain modified 4,4'-diaminostilbene-2,2'-disulfonic acid;

[0056] A4. Add 10 g of amino-containing titanium dioxide obtained in step A2, 3 g of modified 4,4'-diaminostilbene-2,2'-disulfonic acid obtained in step A3 and 30 g of acetone into a reaction container, and react at 80° C. for 3 h to obtain modified titanium dioxide-3.

[0057] Preparation Example 4

[0058] The preparation method of modified titanium dioxide-4 comprises the following steps:

[0059] A1. Add 2 g of 3-isocyanatepropyltrimethoxysilane and 10 g of titanium dioxide into a reaction container, raise the temperature to 90° C. and react for 4 h to obtain titanium dioxide containing an isocyanate group;

[0060] A2, adding 10g of titanium dioxide containing isocyanate groups obtained in step A1 and 0.4g of ethylenediamine into a reaction container, heating to 90°C, reacting for 5.5h, to obtain titanium dioxide containing amino groups;

[0061] A3, 5g of 4,4'-diaminostilbene-2,2'-disulfonic acid was dissolved in 10g of 40wt% sodium hydroxide aqueous solution, and then added to a mixed solution of 5g of cyanuric chloride and 20g of acetone, reacted at 3°C ​​for 2h, and dried to obtain modified 4,4'-diaminostilbene-2,2'-disulfonic acid;

[0062] A4. Add 10 g of amino-containing titanium dioxide obtained in step A2, 1 g of modified 4,4'-diaminostilbene-2,2'-disulfonic acid obtained in step A3 and 30 g of acetone into a reaction container, and react at 80° C. for 3 h to obtain modified titanium dioxide-4.

[0063] Preparation Example 5

[0064] The preparation method of modified polyvinyl alcohol-1 comprises the following steps:

[0065] B1. Add 10 g of vinyl acetate, 20 g of methanol and 12 g of a 35 wt% toluene solution of styrene into a reaction vessel, heat to 65° C., stir for 7 min, add 0.1 g of azobisisobutyronitrile, and dry to obtain a polymer with a number average molecular weight of 3000;

[0066] B2. Add 12 g of the polymer obtained in step B1 and 20 g of methanol into a reaction container, heat to 40° C., add 10 g of a 5 wt % methanol solution of sodium hydroxide, react for 20 min, wash and dry to obtain modified polyvinyl alcohol-1.

[0067] Preparation Example 6

[0068] The preparation method of modified polyvinyl alcohol-2 comprises the following steps:

[0069] B1. Add 10 g of vinyl acetate, 20 g of methanol and 14 g of a 35 wt% toluene solution of styrene into a reaction vessel, heat to 65° C., stir for 7 min, add 0.1 g of azobisisobutyronitrile, and dry to obtain a polymer with a number average molecular weight of 3000;

[0070] B2. Add 12 g of the polymer obtained in step B1 and 20 g of methanol into a reaction container, heat to 40° C., add 10 g of a 5 wt % methanol solution of sodium hydroxide, react for 20 min, wash and dry to obtain modified polyvinyl alcohol-2.

[0071] Preparation Example 7

[0072] The preparation method of modified polyvinyl alcohol-3 comprises the following steps:

[0073] B1. Add 10 g of vinyl acetate, 20 g of methanol and 12 g of a 35 wt% toluene solution of styrene into a reaction vessel, heat to 65° C., stir for 7 min, add 0.1 g of azobisisobutyronitrile, and dry to obtain a polymer with a number average molecular weight of 5000;

[0074] B2. Add 12 g of the polymer obtained in step B1 and 20 g of methanol into a reaction container, heat to 40° C., add 10 g of a 5 wt % methanol solution of sodium hydroxide, react for 20 min, wash and dry to obtain modified polyvinyl alcohol-3.

[0075] Preparation Example 9

[0076] The preparation method of polyvinyl alcohol comprises the following steps:

[0077] B1. Add 10 g of vinyl acetate and 20 g of methanol into a reaction vessel, heat to 65° C., stir for 7 min, and add 0.1 g of azobisisobutyronitrile to obtain a polymer with a number average molecular weight of 3000;

[0078] B2. Add 12 g of the polymer obtained in step B1 and 20 g of methanol into a reaction container, heat to 40° C., add 10 g of a 5 wt % methanol solution of sodium hydroxide, react for 20 min, wash and dry to obtain polyvinyl alcohol.

[0079] Example 1

[0080] A whitening agent with no color difference between indoors and outdoors comprises the following raw materials, measured in parts by weight: 80 parts of modified titanium dioxide-1, 12 parts of azodicarbonamide, and 15 parts of modified polyvinyl alcohol-1.

[0081] The preparation method of the whitening agent with no color difference between indoor and outdoor in this embodiment comprises the following steps: adding azodicarbonamide and modified polyvinyl alcohol-1 to modified titanium dioxide-1, stirring at room temperature for 10 minutes, and obtaining the whitening agent.

[0082] Example 2

[0083] A whitening agent with no color difference between indoors and outdoors comprises the following raw materials, measured in parts by weight: 75 parts of modified titanium dioxide-1, 10 parts of azodicarbonamide, and 10 parts of modified polyvinyl alcohol-1.

[0084] The preparation method of the whitening agent with no color difference between indoor and outdoor in this embodiment comprises the following steps: adding azodicarbonamide and modified polyvinyl alcohol-1 into modified titanium dioxide-1, stirring at room temperature for 5 minutes, and obtaining the whitening agent.

[0085] Example 3

[0086] A whitening agent with no color difference between indoors and outdoors comprises the following raw materials, measured in parts by weight: 85 parts of modified titanium dioxide-1, 15 parts of azodicarbonamide, and 20 parts of modified polyvinyl alcohol-1.

[0087] The preparation method of the whitening agent with no color difference between indoor and outdoor in this embodiment comprises the following steps: adding azodicarbonamide and modified polyvinyl alcohol-1 to modified titanium dioxide-1, stirring at room temperature for 15 minutes, and obtaining the whitening agent.

[0088] Example 4

[0089] A whitening agent with no color difference for indoor and outdoor use and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified titanium dioxide-1 is replaced by modified titanium dioxide-2.

[0090] Example 5

[0091] A whitening agent with no color difference for indoor and outdoor use and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified titanium dioxide-1 is replaced by modified titanium dioxide-3.

[0092] Example 6

[0093] A whitening agent with no color difference for indoor and outdoor use and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified titanium dioxide-1 is replaced by modified titanium dioxide-4.

[0094] Example 7

[0095] A whitening agent with no color difference between indoors and outdoors and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified polyvinyl alcohol-1 is replaced by modified polyvinyl alcohol-2.

[0096] Example 8

[0097] A whitening agent with no color difference between indoors and outdoors and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified polyvinyl alcohol-1 is replaced by modified polyvinyl alcohol-3.

[0098] Comparative Example 1

[0099] A whitening agent with no color difference for indoor and outdoor use and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified titanium dioxide-1 is replaced by titanium dioxide.

[0100] Comparative Example 2

[0101] A whitening agent with no color difference between indoors and outdoors and a preparation method thereof. The specific implementation method is the same as that of Example 1, except that an equal amount of modified polyvinyl alcohol-1 is replaced by polyvinyl alcohol.

[0102] Performance Testing

[0103] (1) Ultraviolet absorption: The ultraviolet absorption wavelength range of the whitening agent with no color difference indoors and outdoors obtained in the above-mentioned embodiments and comparative examples was measured using an ultraviolet-visible spectrophotometer;

[0104] (2) Mechanical properties and density of foam materials:

[0105] Sample preparation: 3 g of the brightener with no color difference between indoor and outdoor obtained in the above embodiments and comparative examples were mixed with 0.7 g of 26 wt% ammonia water and 100 g of PVC resin in an internal mixer for 7 min to obtain a premix, and the obtained premix was subjected to compression foaming at a foaming temperature of 200° C., a pressure of 10 MPa, and a foaming time of 10 min to obtain a PVC foam material.

[0106] The tensile strength of the foamed material was tested according to ASTM D638, and the density of the foamed material was tested using a plastic density tester.

[0107] The test results are shown in Table 1:

[0108] Table 1

[0109]

[0110] Wavelength (nm) Wavelength (nm) (MPa) <![CDATA[(g / cm 3 )]]> Example 1 153 402 3.57 0.22 Example 2 155 398 3.33 0.27 Example 3 151 395 3.38 0.24 Example 4 152 397 3.15 0.32 Example 5 154 393 2.74 0.33 Example 6 171 384 2.98 0.26 Example 7 158 392 3.24 0.31 Example 8 153 395 2.52 0.33 Comparative Example 1 247 353 2.53 0.26 Comparative Example 2 158 394 2.22 0.35

[0111] It can be seen from the data in Table 1 that the whitening agent with no color difference indoors and outdoors in Examples 1-3 of the present invention has a wider ultraviolet absorption band and the foaming material using the whitening agent has better foaming performance and mechanical properties. From the comparison between Examples 4 and 5 and Example 1, it can be seen that changing the ratio of 3-isocyanatepropyltrimethoxysilane and ethylenediamine will make the residual isocyanate groups in the system insufficient to react with ammonia water to release carbon dioxide, so that the mechanical properties of the foaming material will be reduced and the density will be increased; from the comparison between Example 6 and Example 1, it can be seen that changing the ratio of modified 4,4'-diaminostilbene-2,2'-disulfonic acid will make the grafting rate of the fluorescent whitening agent chain segment lower, and the compatibility of modified titanium dioxide with the foaming material is not good, so that the mechanical properties of the foaming material will be reduced and the ultraviolet absorption wavelength range will be reduced; from the comparison between Example 7 and Example 1, it can be seen that adding a change in the ratio of styrene will make the modified polyethylene The large number of rigid segments on the enol cannot well adjust the viscosity of the foaming material, thereby increasing the density of the foaming material; from the comparison between Example 8 and Example 1, it can be seen that changing the molecular weight of the polymer will make it difficult for the modified polyvinyl alcohol to decompose the gas, thereby increasing the density of the foaming material, and will affect the compatibility of the modified titanium dioxide with the foaming material, thereby reducing the mechanical properties of the foaming material; from the comparison between Comparative Example 1 and Example 1, it can be seen that without modifying the titanium dioxide, the ultraviolet absorption wavelength range of the brightener is narrow, and the mechanical properties of the foaming material deteriorate; from the comparison between Comparative Example 2 and Example 1, it can be seen that without modifying the polyvinyl alcohol, the compatibility of the brightener with the foaming material is poor, thereby reducing the mechanical properties of the foaming material.

[0112] The above implementation modes are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the content of the present invention and implement it, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A whitening agent with no color difference indoors and outdoors, characterized in that: The invention comprises the following raw materials in parts by weight: 75-85 parts of modified titanium dioxide, 10-15 parts of foaming agent and 10-20 parts of modified polyvinyl alcohol.

2. The brightener with no color difference indoors and outdoors according to claim 1, characterized in that: The foaming agent is one or more of azobisisobutyronitrile, benzenesulfonyl hydrazide, dinitrosopentamethylenetetramine and azodicarbonamide.

3. The brightener with no color difference indoors and outdoors according to claim 1, characterized in that: The preparation method of the modified titanium dioxide comprises the following steps: A1. Add 3-isocyanate propyltrimethoxysilane and titanium dioxide into a reaction vessel, raise the temperature to 80-100° C. and react for 3-6 hours to obtain titanium dioxide containing an isocyanate group; A2, adding the titanium dioxide containing isocyanate groups and ethylenediamine obtained in step A1 into a reaction vessel, heating to 80-100° C., reacting for 5-6 hours, to obtain titanium dioxide containing amino groups; A3, dissolving 4,4'-diaminostilbene-2,2'-disulfonic acid in a 30-50wt% sodium hydroxide aqueous solution, then adding it to a mixed solution of cyanuric chloride and acetone, reacting at 2-5°C for 1-3h, and drying to obtain modified 4,4'-diaminostilbene-2,2'-disulfonic acid; A4. Add the amino-containing titanium dioxide obtained in step A2, the modified 4,4'-diaminostilbene-2,2'-disulfonic acid obtained in step A3 and acetone into a reaction container, react at 70-90° C. for 2-4 hours, and obtain modified titanium dioxide after drying.

4. The brightener with no color difference indoors and outdoors according to claim 3, characterized in that: The mass ratio of titanium dioxide to 3-isocyanatepropyltrimethoxysilane in step A1 is 1:(0.1-0.3).

5. The brightener with no color difference indoors and outdoors according to claim 3, characterized in that: The mass ratio of titanium dioxide containing isocyanate groups to ethylenediamine in step A2 is 1:(0.03-0.05).

6. The brightener with no color difference indoors and outdoors according to claim 3, characterized in that: The mass ratio of the amino-containing titanium dioxide to the modified 4,4'-diaminostilbene-2,2'-disulfonic acid in step A4 is 1:(0.2-0.4).

7. The brightener with no color difference indoors and outdoors according to claim 1, characterized in that: The preparation method of the modified polyvinyl alcohol comprises the following steps: B1. Add vinyl acetate, methanol and 30-40 wt% styrene toluene solution into a reaction vessel, heat to 60-70° C., stir for 5-10 min, add azobisisobutyronitrile, react for 6-7 h, and obtain a polymer after drying; B2. Add the polymer obtained in step B1 and methanol into a reaction container, heat to 30-50° C., add 4-6 wt % of a methanol solution of sodium hydroxide, react for 10-30 min, wash and dry to obtain modified polyvinyl alcohol.

8. The brightener with no color difference indoors and outdoors according to claim 7, characterized in that: The mass ratio of the vinyl acetate to a toluene solution containing 30-40 wt% styrene is 1:(1.1-1.3).

9. A method for preparing a whitening agent with no color difference indoors and outdoors according to any one of claims 1 to 8, characterized in that: The method comprises the following steps: adding a foaming agent and modified polyvinyl alcohol into the modified titanium dioxide, and stirring at room temperature for 5-15 minutes to obtain the obtained product.

10. Use of the brightener with no color difference between indoor and outdoor use according to any one of claims 1 to 8 or the brightener with no color difference between indoor and outdoor use obtained by the preparation method of claim 9, characterized in that: The whitening agent with no color difference between indoor and outdoor is used in PVC or EVA foaming polymer, and the addition amount is 2.5-3.5wt% of the polymer. At the same time, 25-28wt% of ammonia water needs to be added, and the addition amount is 0.5-1wt% of the polymer.