Resin composition and product thereof

A resin composition was prepared by prepolymerization of polyphenylene ether resin containing unsaturated carbon-carbon double bonds and compound of formula (1). This composition solved the problem of insufficient performance of existing resin compositions under high temperature and high humidity conditions, improved the glass transition temperature and copper foil tensile strength, reduced dielectric loss and thermal expansion rate, and enhanced the stability of dielectric properties.

CN118994875AActive Publication Date: 2024-11-22TAIGUO ELECTRONIC MATERIALS (HUANGSHI) CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411061328.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-22
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

Existing resin compositions exhibit defects such as low glass transition temperature, insufficient tensile strength to copper foil, high dielectric loss, high Z-axis thermal expansion coefficient, large dielectric loss thermal change rate, and large dielectric loss hygrothermal change rate under high temperature and high humidity conditions, which cannot meet the application requirements of complex electronic and electrical products.

Method used

A prepolymer was formed by reacting a polyphenylene ether resin containing unsaturated carbon-carbon double bonds with a compound of formula (1). A resin composition was prepared by combining an appropriate curing accelerator and a molecular weight regulator, avoiding the use of epoxy resin and adding other components such as polyolefins and silicone resins to form a prepreg, resin film and laminate.

Benefits of technology

The glass transition temperature was increased, the tensile strength of the copper foil was enhanced, the dielectric loss and thermal expansion rate were reduced, and the stability of dielectric properties was improved, especially the dielectric loss change rate was significantly reduced in high temperature and high humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994875A_ABST
    Figure CN118994875A_ABST
Patent Text Reader

Abstract

The invention discloses a resin composition which comprises the following components or prepolymers thereof: 100 parts by weight of polyphenyl ether resin containing unsaturated carbon-carbon double bonds and 10-50 parts by weight of a compound shown in a formula (1). In addition, the invention also discloses a product prepared from the resin composition, the product comprises a prepreg, a resin film, a laminated plate or a printed circuit board, and at least one of characteristics such as glass transition temperature, copper foil tension, dielectric loss, Z-axis thermal expansion rate, dielectric loss thermal change rate and dielectric loss damp-heat change rate is improved. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention mainly relates to a resin composition and products made from the same, and in particular to a resin composition that can be applied to prepregs, resin films, laminates (such as copper foil substrates, or copper clad laminates) and printed circuit boards and products made from the same. Background Art

[0002] As the substrate of printed circuit boards, the technical level of copper clad laminates directly affects the performance and reliability of printed circuit boards. With the rapid development of electronic information technology, the application scenarios of electronic and electrical products are increasing, and the application scenarios of printed circuit boards are becoming more and more complex, such as high temperature and high humidity outdoor environments, which puts higher requirements on the characteristics of copper clad laminates.

[0003] There is a method of adding a crosslinking agent to a resin combination in the prior art to improve the degree of crosslinking and curing of the resin, thereby improving the characteristics of the substrate. However, conventional crosslinking agents cannot meet the current substrate characteristics needs, such as crosslinking agent divinylbenzene (DVB), which has a relatively low boiling point and is easily volatilized during the process of resin heat curing, so that the crosslinking effect cannot be effectively brought into play, and for example crosslinking agent triallyl isocyanurate (TAIC), as the printed circuit board is used for a long time or when the printed circuit board is applied to the harsh environment such as high heat and high humidity, the substrate dielectric aging is obvious. In short, at present, various types of resin combinations including conventional crosslinking agents still have one or more defects such as low glass transition temperature, low tension on copper foil, high dielectric loss, high Z-axis thermal expansion rate, large dielectric loss thermal change rate, large dielectric loss wet heat change rate. Therefore, there is a need to develop a novel resin combination and products such as copper-clad laminates thereof in order to overcome one or more of the above-mentioned defects. Summary of the invention

[0004] In view of the problems encountered in the prior art, especially the inability of existing materials to meet one or more of the above-mentioned technical problems, the main purpose of the present invention is to provide a resin composition and a product made of the resin composition that can overcome at least one of the above-mentioned technical problems.

[0005] In one aspect, the present invention provides a resin composition comprising the following components or prepolymers thereof:

[0006] (A) 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds; and

[0007] (B) 10 to 50 parts by weight of a compound of formula (1);

[0008]

[0009] In formula (1), n ​​represents the average number of repeating units, and n is a value of 0 to 4; when n is 0, R is a hydrogen atom or a vinyl group; when n is not 0, R is a vinyl group;

[0010] The prepolymer is obtained by prepolymerization of a mixture, and the mixture at least includes the component (A) and the component (B).

[0011] For example, in one embodiment, the polyphenylene ether resin containing unsaturated carbon-carbon double bonds includes any one of vinylbenzyl polyphenylene ether resin, (meth)acryl polyphenylene ether resin, vinyl polyphenylene ether resin, and allyl polyphenylene ether resin, or a combination thereof.

[0012] For example, in one embodiment, the compound of formula (1) includes a compound of formula (1-1), a compound of formula (1-2), or a combination thereof:

[0013]

[0014] For example, in one embodiment, the compound of formula (1) includes a structure in which n is not 0 and R is a vinyl group.

[0015] For example, in one embodiment, the conversion rate of the prepolymerization reaction is between 10% and 99%.

[0016] For example, in one embodiment, the resin composition does not contain epoxy resin.

[0017] For example, in one embodiment, the resin composition further comprises polyolefin, a cross-linking agent containing unsaturated carbon-carbon double bonds different from the compound of formula (1), a silicone resin, a benzoxazine resin, a polyester resin, a phenolic resin, an amine curing agent, a polyamide, a polyimide, styrene maleic anhydride, a maleimide resin, a cyanate resin, a maleimide triazine resin or a combination thereof.

[0018] For example, in one embodiment, the resin composition further includes a hardening accelerator, an inhibitor, a flame retardant, an inorganic filler, a surface treatment agent, a colorant, a toughening agent, a solvent or a combination thereof.

[0019] On the other hand, in order to achieve the above-mentioned object, the present invention also discloses a product made of the above-mentioned resin composition, which includes a prepreg, a resin film, a laminate or a printed circuit board.

[0020] For example, in one embodiment, the aforementioned product has at least one, multiple or all of the following characteristics:

[0021] The glass transition temperature measured by the method described in IPC-TM-650 2.4.24.4 is greater than or equal to 221°C;

[0023] The copper foil tensile force measured by the method described in IPC-TM-650 2.4.8 is greater than or equal to 3.6 lb / in;

[0025] The dielectric loss measured at a frequency of 10 GHz according to the method described in JIS C2565 is less than or equal to 0.00215;

[0026] The Z-axis thermal expansion rate measured by the method described in IPC-TM-650 2.4.24.5 is less than or equal to 1.6%;

[0028] The dielectric loss thermal change rate calculated from the dielectric loss measured at a frequency of 10 GHz according to the method described in JIS C2565 after being allowed to stand at a constant temperature of 125° C. for 120 hours is less than or equal to 51.5%; and

[0030] After being left to stand for 176 hours at a constant temperature of 85° C. and a relative humidity of 85%, the dielectric loss calculated by measuring the dielectric loss at a frequency of 10 GHz according to the method described in JIS C2565 has a dielectric loss hygrothermal change rate of less than or equal to 36.0%. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text have the common meanings understood by those skilled in the art for the present invention. In case of conflict, the definitions in this specification shall prevail.

[0032] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0033] The use of "one", "a", "an" or similar expressions to describe the components and technical features of the present invention is merely for the convenience of expression and to provide a general meaning to the scope of the present invention. Therefore, such description should be understood to include one or at least one, and the singular also includes the plural, unless it is obvious that it refers to another meaning.

[0034] As used herein, the terms "comprises," "includes," "has," "contains," or any other similar terms are open-ended transitional phrases, which are intended to cover non-exclusive inclusions. For example, a composition or article comprising a plurality of elements encompasses any one or any one of the listed elements, and is not limited to the elements listed herein, but may also include other elements that are not explicitly listed but are generally inherent to the composition or article. In addition, unless expressly stated to the contrary, the term "or" refers to an inclusive "or" rather than an exclusive "or." For example, any of the following situations satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist), A is false (or does not exist) and B is true (or exists), and both A and B are true (or exist). In addition, in this article, the terms "comprising", "including", "having", and "containing" should be interpreted as being specifically disclosed and simultaneously covering closed conjunctions such as "consisting of", "consisting of", "the remainder of", and conjunctions such as "consisting essentially of", "mainly consisting of", "mainly consisting of", "basically containing", "essentially consisting of", "essentially consisting of", and "essentially containing".

[0035] As used herein, “or a combination thereof” means “or any combination thereof”, and covers any combination of more than two of the listed elements; “any one”, “any one”, “any one” means “any one”, “any one”, “any one”. For example, “a composition or its product includes A, B, C or a combination thereof”, or “a composition or its product includes any one or a combination of A, B, C”, when interpreted, covers the following situations: A is true (or exists) and B and C are false (or do not exist), B is true (or exists) and A and C are false (or do not exist), C is true (or exists) and A and B are false (or do not exist), A and B are true (or exist) and C is false (or do not exist), A and C are true (or exist) and B is false (or do not exist), B and C are true (or exist) and A is false (or do not exist), A and C are true (or exist) and B is false (or do not exist), B and C are true (or exist) and A is false (or do not exist), A, B and C are all true (or exist), and other elements not explicitly listed but generally inherent to the composition or its product.

[0036] In this article, the terms "and", "with", "and", "as well as" or other similar terms are used to connect parallel sentence components, and there is no distinction between the previous and subsequent components. The meaning of the parallel sentence components does not change after the positions of the parallel sentence components are exchanged in grammatical sense.

[0037] In this article, all features or conditions such as numerical values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for simplicity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be deemed to have covered and specifically disclosed all possible sub-ranges and individual values ​​within the range (including integers and fractions), especially integer values. For example, the range description of "1.0 to 8.0", "between 1.0 and 8.0" or "between 1.0 to 8.0" should be deemed to have specifically disclosed all sub-ranges such as 1.0 to 8.0, 1.0 to 7.0, 2.0 to 8.0, 2.0 to 6.0, 3.0 to 6.0, 4.0 to 8.0, 3.0 to 8.0, etc., and should be deemed to cover endpoint values, especially sub-ranges defined by integer values, and should be deemed to have specifically disclosed individual values ​​such as 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, etc. Unless otherwise indicated, the above explanation method applies to all contents of the entire text of the present invention, regardless of whether the scope is broad or not.

[0038] If the quantity, concentration or other numerical value or parameter is expressed as a range, a preferred range (or a better range) or a series of upper and lower limits, it should be understood that all ranges consisting of any pair of the upper limit or preferred value (or a better value) of the range and the lower limit or preferred value (or a better value) of the range have been specifically disclosed herein, regardless of whether these ranges are disclosed separately. In addition, if a numerical range is mentioned herein, unless otherwise specified, the range should include its endpoints and all integers and fractions within the range.

[0039] In this document, numerical values ​​should be understood to have the accuracy of the number of significant digits of the numerical value, provided that the purpose of the invention can be achieved. For example, the number 40.0 should be understood to cover the range of 39.50 to 40.49.

[0040] In this article, for the use of Markush groups or optional terms to describe the features or examples of the present invention, those skilled in the art should understand that all subgroups or any individual elements in the Markush group or option list can also be used to describe the present invention. For example, if X is described as "selected from the group consisting of X1, X2 and X3", it also means that the claim that X is X1 and the claim that X is X1 and / or X2 and / or X3 have been fully described. Furthermore, for the use of Markush groups or optional terms to describe the features or examples of the present invention, those skilled in the art should understand that any combination of subgroups or individual members of all elements in the Markush group or option list can also be used to describe the present invention. Accordingly, for example, if X is described as "selected from the group consisting of X1, X2 and X3", and Y is described as "selected from the group consisting of Y1, Y2 and Y3", it means that the claim that X is X1 and / or X2 and / or X3 and Y is Y1 and / or Y2 and / or Y3 has been fully described.

[0041] Unless otherwise specified, in the present invention, a compound refers to a chemical substance formed by two or more elements connected by chemical bonds, including small molecule compounds and polymer compounds, but not limited thereto. The compound herein is not limited to a single chemical substance when interpreted, but can also be interpreted as the same type of chemical substances with the same composition or the same properties.

[0042] If not otherwise specified, in the present invention, polymer refers to the product formed by the polymerization reaction of monomers, often including many polymer aggregates, each polymer is composed of many simple structural units repeatedly connected by covalent bonds, and the monomer is a compound of the synthetic polymer. Polymers can include homopolymers, copolymers, prepolymers, etc., and are not limited to this. Homopolymers refer to polymers polymerized from one monomer. Copolymers refer to polymers polymerized from two or more monomers. Copolymers include random copolymers (structures such as -AABABBBAAABBA-), alternating copolymers (structures such as -ABABABAB-), graft copolymers (structures such as -AA(A-BBBB)AA(A-BBBB)AAA-) and block copolymers (structures such as -AAAAA-BBBBBB-AAAAA-), etc. For example, the styrene-butadiene copolymer in the present invention can include styrene-butadiene random copolymers, styrene-butadiene alternating copolymers, styrene-butadiene graft copolymers or styrene-butadiene block copolymers when interpreted. Prepolymer refers to a polymer with a lower molecular weight between the monomer and the final polymer, and the prepolymer contains reactive functional groups that can further undergo polymerization to obtain a fully cross-linked or hardened product with a higher molecular weight. Polymers of course include oligomers, but are not limited to them. Oligomers, also known as low polymers, are polymers composed of 2 to 20 repeating units, usually 2 to 5 repeating units.

[0043] For those skilled in the art, a resin composition containing two or more compounds and a resin composition containing a prepolymer formed by two or more compounds are different resin compositions. For example, for those skilled in the art, a resin composition containing three compounds A, B and C and an additive (comprising four components in total) and a resin composition containing a prepolymer formed by three compounds A, B and C and an additive (comprising two components in total) are different resin compositions, and the two are completely different in many aspects such as the preparation method, the physical and chemical properties of the compounds themselves, and the properties of the products thereof. For example, the former is to mix A, B, C and the additive to form a resin composition, while the latter is to first prepolymerize the mixture including A, B and C under appropriate conditions to form a prepolymer, and then mix the prepolymer with the additive to obtain the resin composition. For example, for those skilled in the art, the above two resin compositions have completely different compositions, and because the function of the prepolymer formed by the three compounds A, B and C in the resin composition is completely different from the function of A, B and C individually or together in the resin composition, the two resin compositions should be regarded as completely different chemical substances with completely different chemical positions. For example, for those skilled in the art, since the two resin compositions are completely different chemical substances, their products will not have the same properties. For example, in a resin composition including a prepolymer formed by three compounds A, B and C and a crosslinking agent, since A, B and C have partially reacted or converted to form a prepolymer during the prepolymerization reaction, when the resin composition is subsequently heated at a high temperature to form a semi-cured state, a partial crosslinking reaction occurs between the prepolymer and the crosslinking agent, rather than a partial crosslinking reaction between A, B and C and the crosslinking agent, so the products formed by the two resin compositions will also be completely different and have completely different properties.

[0044] If not otherwise specified, the "resin" in the present invention is a customary name for a synthetic polymer, which may include monomers, polymers thereof, combinations of monomers, combinations of polymers thereof, or combinations of monomers and polymers thereof, etc., and is not limited thereto.

[0045] If not otherwise specified, in the present invention, modified products include products after modification of reactive functional groups of each resin, products after prepolymerization of each resin with other resins, products after crosslinking of each resin with other resins, products after copolymerization of each resin with other resins, and the like.

[0046] If not otherwise specified, the unsaturated bond described in the present invention refers to a reactive unsaturated bond, such as but not limited to an unsaturated double bond that can undergo a cross-linking reaction with other functional groups, such as but not limited to an unsaturated carbon-carbon double bond that can undergo a cross-linking reaction with other functional groups.

[0047] The unsaturated carbon-carbon double bonds described in the present invention preferably include, but are not limited to, vinyl, vinylbenzyl, (meth)acryloyl, allyl or a combination thereof. Vinyl should be interpreted to include vinyl and vinylidene (also known as vinylidene), and (meth)acryloyl should be interpreted to include acryloyl and methacryloyl. Therefore, unless otherwise specified, the polyphenylene ether resin containing unsaturated carbon-carbon double bonds described in the present invention includes, but is not limited to, a polyphenylene ether resin having any one of the functional groups of vinyl, vinylbenzyl, (meth)acryloyl, allyl, etc., and is not limited thereto.

[0048] Unless otherwise specified, the alkyl, alkenyl, and monomer described in the present invention include their various isomers when interpreted. For example, propyl should be interpreted as including n-propyl and isopropyl.

[0049] Unless otherwise specified, in the present invention, parts by weight represent relative parts by weight in the composition, which may be any weight unit, such as but not limited to kilograms, kilograms, grams, pounds, etc. For example, 100 parts by weight of polyphenylene ether resin containing unsaturated carbon-carbon double bonds may represent 100 kilograms of polyphenylene ether resin containing unsaturated carbon-carbon double bonds or 100 pounds of polyphenylene ether resin containing unsaturated carbon-carbon double bonds.

[0050] It should be understood that the features disclosed in the various embodiments herein may be arbitrarily combined to form the technical solution of the present invention, as long as there is no contradiction in the combination of these features.

[0051] The present invention will be described below with specific embodiments and examples. It should be understood that these specific embodiments and examples are merely exemplary and are not intended to limit the scope of the present invention and its use. The methods, reagents and conditions used in the examples are, unless otherwise stated, methods, reagents and conditions conventional in the art.

[0052] As mentioned above, the present invention mainly discloses a resin composition, comprising the following components or prepolymers thereof:

[0053] (A) 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds; and

[0054] (B) 10 to 50 parts by weight of a compound of formula (1);

[0055]

[0056] In formula (1), n ​​represents the average number of repeating units, and n is a value of 0 to 4; when n is 0, R is a hydrogen atom or a vinyl group; when n is not 0, R is a vinyl group;

[0057] The prepolymer is obtained by prepolymerization of a mixture, and the mixture at least includes the component (A) and the component (B).

[0058] For example, in one embodiment, the resin composition of the present invention may include 100 parts by weight of a polyphenylene ether resin containing an unsaturated carbon-carbon double bond and 10 to 50 parts by weight of a compound of formula (1). For example, in another embodiment, the resin composition of the present invention may include a prepolymer obtained by prepolymerizing 100 parts by weight of a polyphenylene ether resin containing an unsaturated carbon-carbon double bond and 10 to 50 parts by weight of a compound of formula (1).

[0059] In the resin composition of the present invention, unless otherwise specified, the amount of each component added is based on 100 parts by weight of the total amount of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds. For example, but not limited to, the amount of the compound of formula (1) is 10 to 50 parts by weight, for example, but not limited to, 10 parts by weight, 20 parts by weight, 35 parts by weight, 40 parts by weight or 50 parts by weight, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds.

[0060] The polyphenylene ether resin containing unsaturated carbon-carbon double bonds suitable for use in the present invention is not particularly limited, and may be any one or more polyphenylene ether resins containing unsaturated carbon-carbon double bonds suitable for preparing prepregs, resin films, laminates or printed circuit boards, and may be any one or more commercially available products, homemade products or combinations thereof, for example including but not limited to any one or combinations thereof of vinylbenzyl polyphenylene ether resin, (meth)acryl polyphenylene ether resin, vinyl polyphenylene ether resin, and allyl polyphenylene ether resin.

[0061] The polyphenylene ether resin containing unsaturated carbon-carbon double bonds of the present invention all have unsaturated carbon-carbon double bonds and a phenylene ether skeleton, wherein the unsaturated carbon-carbon double bonds are reactive functional groups, which can self-polymerize after being heated, and can also undergo free radical polymerization reaction with other components having unsaturated bonds in the resin composition and finally cross-link and cure. The cured product has the characteristics of high heat resistance and low dielectric. Preferably, the polyphenylene ether resin containing unsaturated carbon-carbon double bonds includes a polyphenylene ether resin containing unsaturated carbon-carbon double bonds substituted with 2,6-dimethyl on the phenylene ether skeleton, and the methyl groups after substitution form a steric hindrance so that the oxygen atoms on the ether are not easy to produce hydrogen bonds or van der Waals forces and absorb moisture, thereby having lower dielectric properties.

[0062] For example, in one embodiment, the polyphenylene ether resin containing unsaturated carbon-carbon double bonds includes, but is not limited to, vinylbenzyl polyphenylene ether resin having a number average molecular weight of about 1200 (e.g., OPE-2st 1200, available from Mitsubishi Gas Chemical Co., Ltd.), vinylbenzyl polyphenylene ether resin having a number average molecular weight of about 2200 (e.g., OPE-2st 2200, available from Mitsubishi Gas Chemical Co., Ltd.), vinylbenzyl polyphenylene ether resin having a number average molecular weight of about 2400 to 2800 (e.g., vinylbenzyl bisphenol A polyphenylene ether resin), (meth)acryl polyphenylene ether resin having a number average molecular weight of about 1900 to 2300 (e.g., SA9000, available from Sabic), vinyl polyphenylene ether resin having a number average molecular weight of about 2200 to 3000, or a combination thereof. The vinyl polyphenylene ether resin may include various types of polyphenylene ether resins disclosed in U.S. Patent Application US20160185904A1, all of which are incorporated herein by reference. For example, in one embodiment, the vinylbenzyl polyphenylene ether resin includes, but is not limited to, vinylbenzyl biphenyl polyphenylene ether resin, vinylbenzyl bisphenol A polyphenylene ether resin, or a combination thereof.

[0063] On the other hand, in the structure represented by formula (1), n ​​represents the average number of repeating units, and n is a value of 0 to 4 (for example, n is 0, 1, 2, 3 or 4). When n is 0, R is a hydrogen atom or a vinyl group; when n is not 0 (for example, n is 1, 2, 3 or 4), R is a vinyl group.

[0064] For example, the compound of formula (1) may include a structure in which n is 0 and R is a hydrogen atom, and / or the compound of formula (1) may include a structure in which n is 0 and R is a vinyl group, and / or the compound of formula (1) may include a structure in which n is not 0 and R is a vinyl group.

[0065] For example, in one embodiment, the resin composition of the present invention includes a prepolymer, which is obtained by prepolymerization of a mixture, and the mixture includes at least 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds and 10 to 50 parts by weight of a compound of formula (1).

[0066] The prepolymer of the present invention contains residual unsaturated carbon-carbon double bonds, and the conversion rate of the reaction raw materials and the molecular weight of the prepolymer can be adjusted as needed. For example, in one embodiment, the residual unsaturated carbon-carbon double bonds in the prepolymer can react with other components, such as polymerization reaction or cross-linking reaction. In the present invention, by controlling the conversion rate of the compound of formula (1) and the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the presence and content of the residual unsaturated carbon-carbon double bonds in the prepolymer can be controlled. The conversion rate of the compound of formula (1) and the polyphenylene ether resin containing unsaturated carbon-carbon double bonds can be controlled by means known in the art, such as hardening accelerators and / or molecular weight regulators, as well as reaction temperature and reaction time. For example, the conversion rate of the compound of formula (1) can be between 10% and 99%, preferably between 30% and 95%, between 50% and 95%, between 50% and 90%, or between 75% and 90%. For example, when the conversion rate of the compound of formula (1) is 0%, it means that the compound of formula (1) is completely unreacted and the prepolymer of the present invention cannot be formed. When the conversion rate of the compound of formula (1) is 100%, it means that the compound of formula (1) is completely reacted and the prepolymer of the present invention cannot be formed.

[0067] For example, the prepolymer disclosed in the present invention can be prepared by the following method: a mixture of at least 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds and 10 to 50 parts by weight of a compound of formula (1) is subjected to a prepolymerization reaction under appropriate conditions. For example, the prepolymerization reaction can be carried out in the presence of a hardening accelerator and / or a molecular weight regulator. The types of hardening accelerators are described in detail later. In one or more embodiments, the molecular weight regulator includes: n-butyl mercaptan, dodecyl mercaptan, thioglycolic acid, mercaptopropionic acid, mercaptoethanol, 2,4-diphenyl-4-methyl-1-pentene, 4,4'-butylenebis(6-tert-butyl-3-methylphenol), 2,2'-methylenebis(4-ethyl-6-tert-butylphenol) or a combination thereof. The amount of the hardening accelerator and / or molecular weight regulator used in the present invention is not particularly limited. Relative to 100 parts by weight of the total amount of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds and 10 to 50 parts by weight of the compound of formula (1), the amount can be 0.01 to 5 parts by weight, for example, 0.1 to 3 parts by weight, and the amount is not limited thereto. Usually, the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the compound of formula (1) and the optional hardening accelerator and / or molecular weight regulator are dissolved in a solvent for prepolymerization. The solvent can be a solvent conventionally used in the art for the polymerization reaction between a monomer or oligomer containing unsaturated carbon-carbon double bonds (such as the compound of formula (1)) and a polyphenylene ether resin containing unsaturated carbon-carbon double bonds, including but not limited to toluene. The temperature of the prepolymerization reaction is usually higher than room temperature, for example, between 50°C and 140°C, preferably between 80°C and 130°C. The reaction time is usually 0.5 to 6 hours, preferably 1 to 4 hours. The reaction is usually carried out under stirring conditions. Usually, before the reaction starts, the reaction temperature is first raised to above room temperature. After a period of reaction, the temperature is lowered to room temperature (about 25° C.) to obtain a solution, and a filter is used to filter out impurities in the solution. After the solution is purified, a prepolymer product is obtained, i.e., a prepolymer obtained by prepolymerizing the compound of formula (1) with a polyphenylene ether resin containing unsaturated carbon-carbon double bonds.

[0068] For example, in one embodiment, the resin composition of the present invention preferably does not use epoxy resin as the main resin. More preferably, the resin composition of the present invention does not contain epoxy resin, which is beneficial for further reducing the dielectric constant and dielectric loss of the resin composition and its products.

[0069] For example, in one embodiment, in addition to the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the compound of formula (1) or the prepolymer of the above two components, the resin composition of the present invention may further include other components. For example, in one embodiment, the resin composition of the present invention may also include polyolefin, a cross-linking agent containing unsaturated carbon-carbon double bonds other than the compound of formula (1), a silicone resin, a benzoxazine resin, a polyester resin, a phenol resin, an amine curing agent, a polyamide, a polyimide, styrene maleic anhydride, a maleimide resin, a cyanate resin, a maleimide triazine resin or a combination thereof as needed.

[0070] If not otherwise specified, in the resin composition of the present invention, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the amount of polyolefin, crosslinking agent containing unsaturated carbon-carbon double bonds different from the compound of formula (1), silicone resin, benzoxazine resin, polyester resin, phenolic resin, polyamide, polyimide, styrene maleic anhydride, maleimide resin, cyanate resin or maleimide triazine resin is not particularly limited, and can be adjusted as required. For example, each component can be independently 1 part by weight to 100 parts by weight, such as but not limited to 1 part by weight, 5 parts by weight, 10 parts by weight, 15 parts by weight, 20 parts by weight, 25 parts by weight, 50 parts by weight or 100 parts by weight. If not otherwise specified, in the resin composition of the present invention, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the amount of amine curing agent is not particularly limited, and can be adjusted as required. For example, the amount of amine curing agent can be 1 part by weight to 30 parts by weight.

[0071] The polyolefin applicable to the present invention is not particularly limited, and may be any one or more polyolefins applicable to the preparation of prepregs, resin films, laminates or printed circuit boards, and may be any one or more commercially available products, homemade products or combinations thereof. For example, the polyolefin applicable to the present invention includes but is not limited to diene polymers, monoene polymers, hydrogenated diene polymers or combinations thereof. The diene is a hydrocarbon compound containing two unsaturated carbon-carbon double bonds in the molecule, and the monoene is a hydrocarbon compound containing one unsaturated carbon-carbon double bond in the molecule. The polyolefins suitable for use in the present invention include, but are not limited to, any one of polybutadiene, polyisoprene, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-butadiene-divinylbenzene polymer, maleic anhydride added styrene-butadiene polymer, vinyl-polybutadiene-urea polymer, maleic anhydride added polybutadiene, polymethylstyrene, hydrogenated polybutadiene, hydrogenated polyisoprene, hydrogenated styrene-butadiene-divinylbenzene polymer, hydrogenated maleic anhydride added styrene-butadiene polymer, hydrogenated styrene-butadiene copolymer, hydrogenated styrene-isoprene copolymer, and multifunctional vinyl aromatic copolymers or a combination thereof.

[0072] For example, if not specifically stated, the multifunctional vinyl aromatic copolymer used in the present invention may include various types of multifunctional vinyl aromatic copolymers disclosed in US Pat. No. 20070129502A1, which are all incorporated herein by reference.

[0073] Cross-linking agents containing unsaturated carbon-carbon double bonds other than the compound of formula (1) suitable for use in the resin composition of the present invention include, but are not limited to, divinylbenzene (DVB), divinylnaphthalene, divinylbiphenyl, triallyl isocyanurate (TAIC), triallyl cyanurate (TAC), vinylbenzocyclobutene (VBCB), di(vinylbenzyl) ether (bis(vinylbenzyl) ether, BVBE), trivinylcyclohexane (TVCH), diallyl bisphenol A (DABPA), diallyl isophthalate (DAIP), butadiene, decadiene, octadiene, or any one or a combination thereof.

[0074] In the present invention, for example, the silicone resin may be any type of silicone resin known in the art. Specific examples include, but are not limited to, polyalkyl silicone resins, polyaryl silicone resins, polyalkylaryl silicone resins, modified silicone resins, or combinations thereof. Modified silicone resins include, but are not limited to, amino-modified silicone resins, epoxy-modified silicone resins, methacryloyl-modified silicone resins, hydroxyl-modified silicone resins, carboxyl-modified silicone resins, or combinations thereof. Preferably, the amino-modified silicone resin suitable for the present application includes, for example, amino-modified silicone resins produced by Shin-Etsu Chemical Co., Ltd. under the trade names KF-8010, X-22-161A, X-22-161B, KF-8012, KF-8008, X-22-9409, X-22-1660B-3, etc., amino-modified silicone resins produced by Toray-Dowcorning Co., Ltd. under the trade names BY-16-853U, BY-16-853, BY-16-853B, etc., amino-modified silicone resins produced by Momentive Performance Materials JAPAN under the trade names XF42-C5742, XF42-C6252, XF42-C5379, etc., or combinations thereof. The epoxy-modified silicone resin applicable to the present application is, for example, the product name X-22-163 series produced by Shin-Etsu Chemical Co., Ltd. The methacryloyl-modified silicone resin applicable to the present application is, for example, the product name X-22-164 series produced by Shin-Etsu Chemical Co., Ltd.

[0075] In the present invention, for example, the benzoxazine resin may be any type of benzoxazine resin known in the art. Specific examples include, but are not limited to, bisphenol A benzoxazine resin, bisphenol F benzoxazine resin, phenolphthalein benzoxazine resin, dicyclopentadiene benzoxazine resin, phosphorus-containing benzoxazine resin, diamino benzoxazine resin, and phenyl, vinyl or allyl modified benzoxazine resin. Suitable commercially available products include, for example, Huntsman sold under the trade names LZ-8270 (phenolphthalein benzoxazine resin), LZ-8298 (phenolphthalein benzoxazine resin), LZ-8280 (bisphenol F benzoxazine resin), LZ-8290 (bisphenol A benzoxazine resin), or sold under the trade names KZH-5031 (vinyl modified benzoxazine resin), KZH-5032 (phenyl modified benzoxazine resin) by Kolon Industries of Korea. The diaminobenzoxazine resin may be diaminodiphenylmethane benzoxazine resin, diaminodiphenyl ether benzoxazine resin, diaminodiphenyl sulfone benzoxazine resin, diaminodiphenyl sulfide benzoxazine resin or a combination thereof, and is not limited thereto.

[0076] In the present invention, for example, the polyester resin may be any polyester resin known in the art. Specific examples include, but are not limited to, polyester resins containing a dicyclopentadiene structure and polyester resins containing a naphthalene ring structure. Specific examples include, but are not limited to, the trade names HPC-8000 or HPC-8150 sold by Dainippon Ink Chemicals.

[0077] In the present invention, for example, the phenolic resin may be any phenolic resin known in the art. Specific examples include, but are not limited to, phenolic resin or phenoxy resin, wherein the phenolic resin includes phenolic resin, o-methylphenolic resin, bisphenol A resin, naphthol resin, biphenyl phenolic resin and dicyclopentadiene phenol resin, but is not limited thereto.

[0078] In the present invention, for example, the amine curing agent may be any amine curing agent known in the art, and specific examples include but are not limited to at least one of diaminodiphenyl sulfone, diaminodiphenylmethane, diaminodiphenyl ether, diaminodiphenyl sulfide and dicyandiamide, or a combination thereof.

[0079] In the present invention, for example, the polyamide may be any of various polyamides known in the art, and specific examples include but are not limited to various commercially available polyamide resin products.

[0080] In the present invention, for example, the polyimide may be any polyimide known in the art, and specific examples include but are not limited to various commercially available polyimide resin products.

[0081] In the present invention, for example, styrene maleic anhydride can be various styrene maleic anhydride known in the art, wherein the ratio of styrene (St) to maleic anhydride (MA) can be 1 / 1, 2 / 1, 3 / 1, 4 / 1, 6 / 1, 8 / 1 or 12 / 1. Specific examples include, but are not limited to, styrene maleic anhydride copolymers sold by Cray Valley under the trade names SMA-1000, SMA-2000, SMA-3000, EF-30, EF-40, EF-60 and EF-80, or styrene maleic anhydride copolymers sold by Polyscope under the trade names C400, C500, C700, C900, etc.

[0082] In the present invention, for example, the maleimide resin may be any of various maleimide resins known in the art. Specific examples include, but are not limited to: 4,4'-diphenylmethanebismaleimide, polyphenylmethane maleimide (or oligomer of phenylmethane maleimide), bisphenol Adiphenyl ether bismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethanebismaleimide, 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethanebismaleimide, 3,3'-dimethyl-5,5'-dipropyl-4,4'-diphenylmethane bismaleimide), m-phenylene bismaleimide, 4-methyl-1,3-phenylene bismaleimide

[0083] (4-methyl-1,3-phenylene bismaleimide), 1,6-bismaleimide-(2,2,4-trimethyl)hexane, n-2,3-dimethylphenylmaleimide

[0084] (N-2,3-xylylmaleimide), n-2,6-dimethylphenylmaleimide (N-2,6-xylylmaleimide), n-phenylmaleimide (N-phenylmaleimide), vinylbenzyl maleimide (VBM), maleimide containing biphenyl structure, maleimide containing isopropyl and meta-arylene structure, maleimide containing indane structure, maleimide resin containing aliphatic structure with carbon number of 10 to 50, prepolymer of diallyl compound and maleimide resin, prepolymer of diamine and maleimide resin, prepolymer of polyfunctional amine and maleimide resin, prepolymer of acidic phenol compound and maleimide resin or combination thereof. Modified products of these components are also included in the interpretation.

[0085] For example, the maleimide resin includes, but is not limited to, maleimide resins produced by Daiwakasei Industry with trade names such as BMI-1000, BMI-1000H, BMI-1100, BMI-1100H, BMI-2000, BMI-2300, BMI-3000, BMI-3000H, BMI-4000, BMI-5000, BMI-5100, BMI-TMH, BMI-7000 and BMI-7000H, or maleimide resins produced by KI Chemical Co., Ltd. with trade names such as BMI-70 and BMI-80, or maleimide resins produced by Nippon Kayaku Co., Ltd. with trade names such as MIR-3000 or MIR-5000, or maleimide resins containing indane structures produced by DIC.

[0086] For example, the maleimide resin containing an aliphatic structure with 10 to 50 carbon atoms, or the maleimide resin extended by imide, may include various maleimide resins extended by imide disclosed in the patent application publication number TW200508284A, which is incorporated herein by reference in its entirety. The maleimide resin containing an aliphatic structure with 10 to 50 carbon atoms suitable for the present invention may include, for example, but not limited to, maleimide resins produced by designer molecules under the trade names of BMI-689, BMI-1400, BMI-1500, BMI-1700, BMI-2500, BMI-3000, BMI-5000 and BMI-6000.

[0087] In the present invention, for example, the cyanate ester may be various cyanate resins known in the art, such as compounds having an Ar-OC≡N structure, wherein Ar may be a substituted or unsubstituted aromatic group. From the perspective of improving the heat resistance of the resin composition, specific examples include, but are not limited to, phenolic cyanate resins, bisphenol A cyanate resins, bisphenol F cyanate resins, cyanate resins containing dicyclopentadiene structures, cyanate resins containing naphthalene ring structures, phenolphthalein cyanate resins, adamantane cyanate resins, fluorene cyanate resins, or combinations thereof. Among them, the phenolic cyanate resin may be a bisphenol A phenolic cyanate resin, a bisphenol F phenolic cyanate resin, or a combination thereof. For example, the cyanate resin may be a cyanate resin produced by Lonza under the trade names of Primaset PT-15, PT-30S, PT-60S, BA-200, BA-230S, BA-3000S, BTP-2500, BTP-6020S, DT-4000, DT-7000, ULL950S, HTL-300, CE-320, LVT-50, LeCy, etc.

[0088] In the present invention, for example, the maleimide triazine resin may be various maleimide triazine resins known in the art. Specific examples include, but are not limited to: maleimide triazine resin obtained by polymerizing maleimide resin with bisphenol A type cyanate resin, maleimide triazine resin obtained by polymerizing maleimide resin with bisphenol F type cyanate resin, maleimide triazine resin obtained by polymerizing maleimide resin with phenol novolac type cyanate resin, maleimide triazine resin obtained by polymerizing maleimide resin with cyanate resin containing dicyclopentadiene structure. In one embodiment, the maleimide triazine resin may be obtained by polymerizing the aforementioned maleimide resin with the aforementioned cyanate resin in any molar ratio; for example, the molar ratio of maleimide resin to cyanate resin may be 1:1 to 10, such as but not limited to 1:1, 1:2, 1:4, 1:6, 1:8, 1:10.

[0089] For example, in one embodiment, the resin composition further comprises a hardening accelerator, an inhibitor, a flame retardant, an inorganic filler, a surface treatment agent, a colorant, a toughening agent, a solvent or a combination thereof.

[0090] In the present invention, for example, the hardening accelerator (including the hardening initiator) may include a catalyst such as a Lewis base or a Lewis acid. The Lewis base may include one or more of imidazole, boron trifluoride amine complex, ethyltriphenyl phosphonium chloride, 2-methylimidazole (2MI), 2-phenyl-1H-imidazole (2PZ), 2-ethyl-4-methylimidazole (2E4MZ), triphenylphosphine (TPP) and 4-dimethylaminopyridine (DMAP). The Lewis acid may include a metal salt compound, such as a metal salt compound of manganese, iron, cobalt, nickel, copper, zinc, etc., such as a metal catalyst such as zinc octoate and cobalt octoate. The hardening accelerator also includes a hardening initiator, such as a peroxide that can generate free radicals, and the hardening initiator includes but is not limited to: diisopropylbenzene peroxide (DCP), tert-butyl peroxybenzoate, dibenzoyl peroxide (BPO), 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne (25B) and bis(tert-butylperoxyisopropyl)benzene or a combination thereof. For example, in one embodiment, compared to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 0.01 to 5.0 parts by weight of the hardening accelerator, preferably 0.01 to 4.0 parts by weight of the hardening accelerator, and more preferably 0.1 to 2.0 parts by weight of the hardening accelerator, but is not limited thereto.

[0091] In the present invention, for example, the inhibitor may include but is not limited to 1,1-diphenyl-2-trinitrophenylhydrazine, methacrylonitrile, nitrogen oxide stable free radicals, triphenylmethyl free radicals, metal ion free radicals, sulfur free radicals (for example, including but not limited to dithioesters), hydroquinone, p-methoxyphenol, p-benzoquinone, phenothiazine, β-phenylnaphthylamine, p-tert-butylcatechol, methylene blue, 4,4'-butylenebis(6-tert-butyl-3-methylphenol) and 2,2'-methylenebis(4-ethyl-6-tert-butylphenol) or a combination thereof. For example, the above-mentioned nitrogen oxide stable free radicals may include but are not limited to nitrogen oxide free radicals from cyclic hydroxylamines such as 2,2,6,6-substituted-1-piperidinyloxy free radicals or 2,2,5,5-substituted-1-pyrrolidinyloxy free radicals. As a substituent, an alkyl group with a carbon number of less than four, such as a methyl group or an ethyl group, is preferred. Specific nitrogen oxide free radical compounds are not limited, and examples include but are not limited to 2,2,6,6-tetramethyl-1-piperidinyloxy free radicals, 2,2,6,6-tetraethyl-1-piperidinyloxy free radicals, 2,2,6,6-tetramethyl-4-oxo-1-piperidinyloxy free radicals, 2,2,5,5-tetramethyl-1-pyrrolidinyloxy free radicals, 1,1,3,3-tetramethyl-2-isoindolinyloxy free radicals, N,N-di-tert-butylamineoxy free radicals, etc. Stable free radicals such as galvinoxyl free radicals can also be used to replace nitrogen oxide free radicals. The inhibitor suitable for the resin composition of the present invention can also be a product derived from the hydrogen atom or atomic group in the inhibitor being replaced by other atoms or atomic groups. For example, the hydrogen atom in the inhibitor is replaced by an atomic group such as an amino group, a hydroxyl group, a ketocarbonyl group, etc. For example, in one embodiment, based on 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 0.001 to 20 parts by weight of a polymerization inhibitor, preferably 0.01 to 10 parts by weight of a polymerization inhibitor, but is not limited thereto.

[0092] In the present invention, for example, the flame retardant may be any one or more flame retardants suitable for preparing prepregs, resin films, laminates or printed circuit boards, such as but not limited to phosphorus-containing flame retardants or bromine-containing flame retardants. The bromine-containing flame retardant preferably includes decabromodiphenylethane. Phosphorus-containing flame retardants preferably include: hydroquinone bis-(diphenyl phosphate), bisphenol A bis-(diphenyl phosphate), tri(2-carboxyethyl)phosphine (TCEP), tri(chloroisopropyl) phosphate, trimethyl phosphate (TMP), dimethyl methylphosphonate (DMMP), resorcinol bis(dixylenyl phosphate), RDXP (such as commercial products such as PX-200, PX-201, PX-202), ammonium polyphosphate, melamine polyphosphate, etc. polyphosphate), phosphazene compounds (such as commercially available products such as SPB-100, SPH-100, and SPV-100), 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide, DOPO) compounds and their derivatives or resins (such as bis-DOPO compounds), diphenylphosphine oxide (DPPO) compounds and their derivatives or resins (such as bis-DPPO compounds), melamine cyanurate and tri-hydroxy ethyl isocyanurate, aluminum phosphinate (such as products such as OP-930 and OP-935), or combinations thereof.

[0093] For example, in one embodiment, the flame retardant can be a flame retardant sold by Katayama Chemical Industry Co., Ltd., such as but not limited to V1, V2, V3, V4, V5, V7, S-2, S-4, E-4c, E-7c, E-8g, E-9g, E-10g, E-100, B-3, W-1o, W-2h, W-2o, W-3o, W-4o, OX-1, OX-2, OX-4, OX-6, OX-6+, OX-7, OX-7+, OX-13, BPE-1, BPE-3, HyP-2, API-9, CMPO, ME-20, C-1R, C-1S, C-3R, C-3S or C-11R. The flame retardant of the present invention can include one or more of the above.

[0094] For example, in one embodiment, relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 1 to 100 parts by weight of a flame retardant, preferably 5 to 50 parts by weight of a flame retardant.

[0095] In the present invention, for example, the inorganic filler can be any one or more inorganic fillers suitable for preparing prepregs, resin films, laminates or printed circuit boards, and specific examples thereof include, but are not limited to, silicon dioxide (molten, non-molten, porous or hollow), aluminum oxide, aluminum hydroxide, magnesium oxide, magnesium hydroxide, calcium carbonate, aluminum nitride, boron nitride, aluminum silicon carbide, silicon carbide, titanium dioxide, barium titanate, lead titanate, strontium titanate, calcium titanate, magnesium titanate, barium zirconate, lead zirconate, magnesium zirconate, lead zirconate titanate, zinc molybdate, calcium molybdate, magnesium molybdate, ammonium molybdate, zinc molybdate-modified talc, zinc oxide, zirconium oxide, mica, boehmite (AlOOH), calcined talc, talc, silicon nitride, zirconium tungstate, petalite, calcined kaolin or a combination thereof. In addition, the inorganic filler can be spherical (including solid sphere or hollow sphere), fibrous, plate-like, granular, flaky or needle-like, and can be selectively pretreated with a silane coupling agent. In addition, the inorganic filler can be prepared by a variety of methods, such as a melting method, a deflagration method, and a chemical synthesis method. For example, in one embodiment, relative to 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention can further include 10 to 300 parts by weight of an inorganic filler, preferably 50 to 300 parts by weight of an inorganic filler, more preferably 80 to 200 parts by weight of an inorganic filler, but is not limited thereto.

[0096] In the present invention, for example, the type of surface treatment agent is not particularly limited, and may include but is not limited to silane compounds (silane, such as siloxane compounds), which can be divided into aminosilane compounds (amino silane), epoxysilane compounds (epoxide silane), vinylsilane compounds, hydroxylsilane compounds, isocyanate silane compounds, methacryloxysilane compounds and acryloxysilane compounds according to the type of functional group. The main function of adding a surface treatment agent in the present invention is to allow the inorganic filler to be uniformly dispersed in the resin composition. For example, in one embodiment, relative to 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 0.001 to 20 parts by weight of a surface treatment agent, preferably 0.01 to 10 parts by weight of a surface treatment agent, but is not limited thereto.

[0097] In the present invention, for example, the coloring agent may include but is not limited to a dye or a pigment. For example, in one embodiment, based on 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 0.001 to 10 parts by weight of the coloring agent, preferably 0.01 to 5 parts by weight of the coloring agent, but is not limited thereto.

[0098] The main function of adding a toughening agent in the present invention is to improve the toughness of the resin composition. In the present invention, for example, the toughening agent may include, but is not limited to, carboxyl-terminated butadieneacrylonitrile rubber (CTBN), core-shell rubber, ethylene-propylene rubber and other compounds or combinations thereof. For example, in one embodiment, based on 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the resin composition of the present invention may further include 1 to 20 parts by weight of a toughening agent, preferably 3 to 10 parts by weight of a toughening agent, but is not limited thereto.

[0099] In the present invention, for example, the solvent can be any solvent suitable for dissolving the resin composition of the present invention, including but not limited to: methanol, ethanol, ethylene glycol monomethyl ether, acetone, butanone (also known as methyl ethyl ketone), methyl isobutyl ketone, cyclohexanone, nitrogen methyl pyrrolidone, toluene, xylene, methoxyethyl acetate, ethoxyethyl acetate, propoxyethyl acetate, ethyl acetate, dimethylformamide, dimethylacetamide, propylene glycol methyl ether acetate and the like solvents or mixed solvents thereof. The amount of solvent added is to be able to completely dissolve the resin and adjust to a specific total solid content of the resin composition. For example, in one embodiment, the amount of solvent added is to adjust the total solid content of the resin composition to 50% to 85% (weight percentage) for addition, but is not limited thereto.

[0100] In addition to the aforementioned resin composition, the present invention also provides a product made from the aforementioned resin composition, such as a component suitable for use in various electronic products, including but not limited to: a prepreg, a resin film, a laminate or a printed circuit board.

[0101] For example, the resin composition of the present invention can be made into a semi-cured sheet, which includes a reinforcing material and a layered object arranged on the reinforcing material. The layered object is obtained by heating the aforementioned resin composition at a high temperature to form a semi-cured state (B-stage). The baking temperature for making the semi-cured sheet is between 120°C and 180°C, preferably between 120°C and 160°C. The reinforcing material can be any one of a fiber material, a woven fabric, and a non-woven fabric, and the woven fabric preferably includes a glass fiber cloth. The type of glass fiber cloth is not particularly limited, and can be various glass fiber cloths that can be used for printed circuit boards, such as E-type glass cloth, D-type glass cloth, S-type glass cloth, T-type glass cloth, L-type glass cloth, Q-type glass cloth or QL-type glass cloth (a glass cloth of a mixed structure made of Q glass and L glass); the types of glass fibers include yarns and rovings, etc., and the forms include open fiber or unopen fiber, and the end face shape includes a circular or flat shape. The aforementioned non-woven fabric preferably includes a liquid crystal resin non-woven fabric, such as a polyester non-woven fabric, a polyurethane non-woven fabric, etc., and is not limited thereto. The aforementioned fabric may also include a liquid crystal resin fabric, such as a polyester fabric or a polyurethane fabric, etc., and is not limited thereto. This reinforcing material can increase the mechanical strength of the prepreg. In a preferred embodiment, the reinforcing material can also be selectively pretreated with a silane coupling agent. The prepreg is subsequently heated and cured (C-stage) to form an insulating layer.

[0102] For example, the resin composition of the present invention can be made into a resin film, which is obtained by semi-curing the aforementioned resin composition after baking and heating. The resin composition can be selectively coated on a supporting material, the supporting material includes but is not limited to a liquid crystal resin film, a polytetrafluoroethylene film, a polyethylene terephthalate film (PET film), a polyimide film (PI film), a metal foil or a resin-coated copper foil (RCC), and then baked and heated to form a semi-cured state, so that the resin composition forms a resin film.

[0103] For example, the resin composition described in the present invention can be made into various laminates, which include at least two metal foils and at least one insulating layer, wherein the insulating layer is disposed between the two metal foils, and the insulating layer can be cured by the aforementioned resin composition under high temperature and high pressure (C-stage), and the applicable curing temperature is, for example, between 190°C and 220°C, preferably between 200°C and 210°C, and the curing time is 90 to 180 minutes, preferably between 120 to 150 minutes, and the applicable pressing pressure is, for example, between 300psi and 550psi, preferably between 400psi and 500psi. The aforementioned insulating layer can be obtained by curing the aforementioned semi-cured sheet or resin film. The material of the aforementioned metal foil can be copper, aluminum, nickel, platinum, silver, gold or their alloys, such as copper foil. In a preferred embodiment, the laminate is a copper foil substrate.

[0104] In one embodiment, the aforementioned laminate can be further processed into a printed circuit board after circuit processing. One of the methods for making the printed circuit board of the present invention can be to use a double-sided copper-clad laminate (such as product EM-827, which can be purchased from Taiguang Electronic Materials (Kunshan) Co., Ltd.) with a thickness of 28 mils and 1 ounce of HTE (High Temperature Elongation) copper foil, and electroplating after drilling to form electrical conduction between the upper copper foil and the bottom copper foil. The upper copper foil and the bottom copper foil are then etched to form an inner layer circuit. The inner layer circuit is then browned and roughened to form a concave-convex structure on the surface to increase the roughness. Then, the copper foil, the aforementioned prepreg, the aforementioned inner layer circuit board, the aforementioned prepreg, and the copper foil are stacked in sequence, and then a vacuum laminating device is used to heat for 90 to 180 minutes at a temperature of 190°C to 220°C to cure the insulating layer material of the prepreg. Next, various circuit board processing techniques known in the art such as blackening, drilling, and copper plating are performed on the copper foil on the outermost surface to obtain a printed circuit board.

[0105] For example, in one embodiment, the product made of the resin composition of the aforementioned embodiments contains a reinforcing material or a supporting material and a semi-cured or cured product obtained by heating and chemically cross-linking the resin composition.

[0106] For example, in one embodiment, the resin composition disclosed in the present invention and various products prepared therefrom preferably have one, more or all of the following characteristics:

[0107] The glass transition temperature measured by the method described in IPC-TM-650 2.4.24.4 is greater than or equal to 221°C, for example, between 221°C and 265°C;

[0109] The copper foil tensile force measured by the method described in IPC-TM-650 2.4.8 is greater than or equal to 3.6 lb / in, such as between 3.6 lb / in and 3.9 lb / in;

[0111] The dielectric loss measured at a frequency of 10 GHz according to the method described in JIS C2565 is less than or equal to 0.00215, for example, between 0.00193 and 0.00215;

[0112] The Z-axis thermal expansion rate measured by the method described in IPC-TM-650 2.4.24.5 is less than or equal to 1.6%, such as between 1.0% and 1.6%;

[0114] The dielectric loss thermal change rate calculated from the dielectric loss measured at a frequency of 10 GHz according to the method described in JIS C2565 after standing at a constant temperature of 125° C. for 120 hours is less than or equal to 51.5%, such as between 39.1% and 51.5%, or such as between 39.1% and 44.3%;

[0116] And the dielectric loss hygrothermal change rate calculated by measuring the dielectric loss at a frequency of 10 GHz according to the method described in JIS C2565 after being allowed to stand for 176 hours at a constant temperature of 85°C and a relative humidity of 85% is less than or equal to 36.0%, for example, between 25.9% and 36.0%, or for example, between 25.9% and 28.5%.

[0119] The resin compositions of the embodiments of the present invention and the comparative examples of the present invention were prepared using various raw materials from the following sources according to the amounts shown in Tables 1 to 3, and were further prepared into various test samples.

[0120] The chemical raw materials used in the embodiments and comparative examples of the present invention are as follows:

[0121] SA9000: (meth)acryl polyphenylene ether resin, available from Sabic.

[0122] OPE-2st 1200: vinyl benzyl polyphenylene ether resin, purchased from Mitsubishi Gas Chemical.

[0123] OPE-2st 2200: vinyl benzyl polyphenylene ether resin, purchased from Mitsubishi Gas Chemical.

[0124] Compounds of formula (1): Compounds P1 to P5 were prepared in-house and described in detail below.

[0125] Prepolymer: Prepolymers Y1 to Y5 were self-made and described in detail below.

[0126] BVPE: bis(vinylphenyl)ethane, purchased from Linchuan Chemical.

[0127] Compound D1 has the following structural formula:

[0128]

[0129] Compound D2 has the following structural formula:

[0130]

[0131] Compound D3 has the following structural formula:

[0132]

[0133] Compound D4 has the following structural formula:

[0134] Here, m is a value from 1 to 4.

[0135] Compound D5 has the following structural formula:

[0136]

[0137] G1726: hydrogenated styrene-butadiene-styrene triblock copolymer, available from KRATON.

[0138] B-3000: polybutadiene, purchased from Nippon Soda.

[0139] Ricon 184MA6: maleic anhydride addition styrene-butadiene polymer, available from Cray Valley Company.

[0140] Spherical silica: The median particle size D50 is about 1.5±0.5 microns. It is a chemically synthesized spherical silica prepared by a microemulsification method and surface-treated with a silane coupling agent. It is commercially available.

[0141] 25B: 2,5-dimethyl-2,5-di(tert-butylperoxy)-3-hexyne, purchased from NOF Corporation.

[0142] Solvent: Toluene, purchased from Sinopec. The content of the solvent is expressed as "appropriate amount", which means that the content of the solvent is adjusted to the overall solid content of the resin composition of 60% to 68% (solid content, S / C = 60% to 68%).

[0143] Chemical Raw Materials Preparation Example

[0144] Preparation Example 1: Compound P1

[0145] In a 100 ml round-bottom flask, 10 mmol (2.03 g) of phthaloyl chloride was completely dissolved in 30 ml of dichloromethane. 22 mmol (2.5 g) of p-hydroxystyrene and 25 mmol (25 g) of triethylamine were weighed and diluted and dissolved with 10 ml of dichloromethane, and the completely dissolved mixed solution was placed in a 20 ml constant pressure dropping funnel. Under ice bath conditions, the above mixed solution was completely added dropwise to the dichloromethane solution of phthaloyl chloride within 1 hour. After the reaction system was stirred in an ice bath for 2 hours, it was heated to 50 ° C and refluxed and stirred for 4 hours, and the reaction was completed. After the system was cooled to room temperature, the ammonium salt in the system was filtered out, the filtrate was vacuum concentrated, the crude product was added to 100 ml of petroleum ether for recrystallization, and the compound P1 was obtained by filtration, which has the structure shown in formula (1-1).

[0146]

[0147] Preparation Example 2: Compound P2

[0148] Step 1: At room temperature, 4 mmol (97 mg) of magnesium powder was added to a 50 ml flask, sealed with a rubber septum, and purged with nitrogen. 6 ml of lithium chloride (3 mmol, 127 mg) in tetrahydrofuran was slowly added to the flask using a syringe, followed by the addition of 2.6 mmol (0.64 g) of 4-bromophthalic acid to the system, and the reaction mixture was cooled to 0°C after stirring at room temperature for 2 hours. 0.1 mmol (16.2 mg) of FeCl3 and 1 ml of tetramethylethylenediamine (60 μl) in tetrahydrofuran were added to the flask via a syringe, followed by the addition of 2 mmol (0.21 g) of vinyl bromide and stirred at low temperature for 3 hours to complete the reaction. The system was quenched with saturated aqueous Na2CO3 solution and extracted three times with ethyl acetate (5 ml each time). The combined organic phases were dried over Na2SO4, the mixture was concentrated in vacuo, and the crude product was purified by column chromatography (cyclohexane: ethyl acetate = 1:1) to obtain a first intermediate having the following structure.

[0149]

[0150] Step 2: Add 50 mmol (6.10 g) of the aforementioned first intermediate, 15 ml of dichloromethane and 0.6 ml of N,N-dimethylformamide to a 100 ml round-bottom flask equipped with a magnetic stirring bar. Cool the reaction mixture to 0°C and stir for 5 minutes. Add 65 mmol (0.56 ml) of COCl2 dropwise to the reaction mixture. Stir the reaction mixture at room temperature for 4 hours. Concentrate the resulting mixture under reduced pressure to obtain a second intermediate having the following structure.

[0151]

[0152] Step 3: In a 100 ml round-bottom flask, 10 mmol (2.28 g) of the second intermediate is completely dissolved in 30 ml of dichloromethane. Weigh 22 mmol (2.5 g) of p-hydroxystyrene and 25 mmol of triethylamine and dilute and dissolve them with 10 ml of dichloromethane. The completely dissolved mixed solution is placed in a 20 ml constant pressure dropping funnel. Under ice bath conditions, the mixed solution is completely added dropwise to the dichloromethane solution of the second intermediate within 1 hour. After stirring at low temperature for 2 hours, the reaction system is heated to 50 ° C and refluxed and stirred for 4 hours, and the reaction is completed. After the system is cooled to room temperature, the ammonium salt in the system is filtered out, and the filtrate is vacuum concentrated. The crude product is added to 100 ml of petroleum ether for recrystallization, and filtered to obtain compound P2, which has the structure shown in formula (1-2).

[0153]

[0154] Preparation Example 3: Compound P3

[0155] In a 5-liter reactor, 2 liters of dichloromethane, 1 mol (189 g) of 2-bromohydroquinone, 2 mol (268 g) of potassium vinyl trifluoroborate, 3.1 mol (300 g) of triethylamine and 0.04 mol (10.5 g) of triphenylphosphine were added, the system was cooled to 0°C, 1.1 mol (400 g) of 4-bromophthaloyl chloride was added dropwise under nitrogen, the reaction was stirred for 2 hours, and then 1.1 mol (121 g) of p-hydroxystyrene was added dropwise, and the system was heated to 50°C. The molecular weight of the product was monitored by gas chromatography during the reaction. The reaction was terminated by refluxing for 10 hours, the precipitated solid was removed by filtration, the filtrate was retained, and the remaining raw materials and the reaction solvent were removed by distillation to obtain compound P3, which has the structure shown in formula (1), wherein n is about 1, R is vinyl, and the number average molecular weight is 670.

[0156] Preparation Example 4: Compound P4

[0157] In a 5-liter reactor, 2 liters of acetonitrile, 1 mol (189 g) of 2-bromohydroquinone, 2 mol (268 g) of potassium vinyl trifluoroborate, 3.1 mol (300 g) of triethylamine and 0.04 mol (10.5 g) of triphenylphosphine were added, the system was cooled to 0°C, 1.1 mol (400 g) of 4-bromophthaloyl chloride was added dropwise under nitrogen, the reaction was stirred for 2 hours, and then 1.1 mol (121 g) of p-hydroxystyrene was added dropwise, and the system was heated to 70°C. The molecular weight of the product was monitored by gas chromatography during the reaction. The reaction was refluxed for 15 hours. After the reaction was terminated, the remaining raw materials and the reaction solvent were removed by distillation to obtain compound P4, which has the structure shown in formula (1), wherein n is about 2, R is vinyl, and the number average molecular weight is 930.

[0158] Preparation Example 5: Compound P5

[0159] In a 5-liter reactor, 2 liters of toluene, 1 mol (189 g) of 2-bromohydroquinone, 2 mol (268 g) of potassium vinyl trifluoroborate, 3.1 mol (300 g) of triethylamine and 0.04 mol (10.5 g) of triphenylphosphine were added, the system was cooled to 0°C, 1.1 mol (400 g) of 4-bromophthaloyl chloride was added dropwise under nitrogen, the reaction was stirred for 2 hours, and then 1.1 mol (121 g) of p-hydroxystyrene was added dropwise, and the system was heated to 110°C. The molecular weight of the product was monitored by gas chromatography during the reaction. The reaction was terminated by reflux for 20 hours, the precipitated solid was removed by filtration, the filtrate was retained, and the remaining raw materials and the reaction solvent were removed by distillation to obtain compound P5, which has the structure shown in formula (1), wherein n is about 4, R is vinyl, and the number average molecular weight is 1460.

[0160] Preparation Example 6: Prepolymer Y1

[0161] 100 g of SA9000 and 10 g of compound P2 were added to a three-necked flask in sequence, and the temperature was raised to 100° C. until the reaction materials were molten. The mixture was mechanically stirred at a constant temperature for 2 hours to obtain prepolymer Y1, in which the conversion rate of the compound of formula (1) was between 10% and 99%.

[0162] Preparation Example 7: Prepolymer Y2

[0163] 100 g of SA9000 and 35 g of compound P2 were added to a three-necked flask in sequence, and the temperature was raised to 110° C. until the reaction materials were molten. The mixture was mechanically stirred at a constant temperature for 1.5 hours to obtain prepolymer Y2, in which the conversion rate of the compound of formula (1) was between 10% and 99%.

[0164] Preparation Example 8: Prepolymer Y3

[0165] 100 g of SA9000 and 50 g of compound P2 were added to a three-necked flask in sequence, and the temperature was raised to 130° C. until the reaction materials were molten. The mixture was mechanically stirred at constant temperature for 1 hour to obtain prepolymer Y3, in which the conversion rate of the compound of formula (1) was between 10% and 99%.

[0166] Preparation Example 9: Prepolymer Y4

[0167] Into a three-necked flask, 40 g of SA9000, 40 g of OPE-2st 1200, 20 g of OPE-2st 2200, 10 g of compound P1 and 10 g of compound P2 were added in sequence, the temperature was raised to 120° C. until the reaction materials were molten, and the mixture was mechanically stirred at a constant temperature for 2 hours to obtain a prepolymer Y4, wherein the conversion rate of the compound of formula (1) was between 10% and 99%.

[0168] Preparation Example 10: Prepolymer Y5

[0169] Into a three-necked flask, 60 g of SA9000, 30 g of OPE-2st 1200, 10 g of OPE-2st 2200, 10 g of compound P1, 15 g of compound P2, 5 g of compound P3, 5 g of compound P4 and 5 g of compound P5 were added in sequence, the temperature was raised to 130° C. until the reaction materials were in a molten state, and mechanical stirring was carried out at a constant temperature for 1.5 hours to obtain a prepolymer Y5, wherein the conversion rate of the compound of formula (1) was between 10% and 99%.

[0170] The compositions (all in parts by weight) of the resin compositions of the embodiments and comparative examples of the present invention and the test results of the sample properties are shown in Tables 1 to 3:

[0171] [Table 1] Composition and property test results of the resin composition of the embodiment (unit: weight parts)

[0172]

[0173]

[0174] [Table 2] Composition and property test results of the resin composition of the embodiment (unit: weight parts)

[0175]

[0176]

[0177] [Table 3] Composition and property test results of the resin composition of the comparative example (unit: parts by weight)

[0178]

[0179]

[0180] The characteristic tests of the embodiments and comparative examples of the present invention are performed by making the test objects (also called test specimens or samples) according to the following method and then performing the tests according to specific test conditions.

[0181] (1) Prepreg (PP): The resin composition of the embodiment or comparative example is selected and mixed uniformly to form a varnish, which is then injected into an impregnation tank, and a glass fiber cloth (e.g., L-glass fiber cloth with a specification of 2116 or 1080, both purchased from Asahi) is then immersed in the impregnation tank to allow the resin composition to adhere to the glass fiber cloth, and then heated at 150° C. to 170° C. to a semi-cured state (B-Stage), thereby obtaining a prepreg. The resin content of the prepreg made of the 1080 L-glass fiber cloth is about 70%; the resin content of the prepreg made of the 2116 L-glass fiber cloth is about 55%.

[0182] (2) Copper foil substrate (8-ply, 8 prepregs pressed together): 2 18 μm thick ultra-low surface roughness (HVLP) copper foils and 8 2116 L-glass cloths were prepared to impregnate the prepregs prepared from each sample to be tested (each set of examples or comparative examples), and the resin content of each prepreg was about 55%. One HVLP copper foil, eight prepregs, and one HVLP copper foil were stacked in this order, and pressed together under vacuum conditions, a pressure of 420 psi, and 200° C. for 2 hours to form a copper foil substrate.

[0183] (3) Copper-free substrate (8-ply, formed by pressing together 8 prepregs): The copper foil on both sides of the above copper foil substrate (8-ply) is etched to obtain a copper-free substrate (8-ply).

[0184] (4) Copper-free substrate (2-ply, formed by pressing two prepregs): Prepare two 18-micron-thick ultra-low surface roughness (HVLP) copper foils and two 1080 L-glass fiber cloths impregnated with the prepregs made from each sample to be tested (each set of examples or comparative examples), and the resin content of each prepreg is about 70%. Copper foil, two prepregs, and copper foil are stacked in order, and pressed for 2 hours under vacuum conditions, a pressure of 420 psi, and 200° C. to form a copper-containing substrate (2-ply, formed by pressing two prepregs). Next, the copper foil-containing substrate (2-ply) is etched to remove the copper foil on both sides to obtain a copper-free substrate.

[0185] The test methods and characteristic analysis items of the samples to be tested are as follows:

[0186] 1. Glass transition temperature (DMA-Tg)

[0187] The aforementioned copper-free substrate (8-ply) was selected as the sample to be tested, and the glass transition temperature of each sample to be tested was measured by a dynamic mechanical analyzer (DMA) with reference to the method described in IPC-TM-650 2.4.24.4, in degrees Celsius. The measuring temperature range was 50 to 400 degrees Celsius, and the temperature rise rate was 2 degrees Celsius per minute. The higher the glass transition temperature, the better.

[0188] 2. Copper foil pulling force (peeling strength, P / S)

[0189] The aforementioned copper foil substrate (8-ply) was cut into rectangular samples with a width of 24 mm and a length greater than 60 mm, and the surface copper foil was etched to leave only a long strip of copper foil with a width of 3.18 mm and a length greater than 60 mm. The strength required to pull the copper foil away from the surface of the substrate insulation layer was measured using a universal tensile strength tester at room temperature (about 25°C) according to the method described in IPC-TM-650 2.4.8, and the unit was lb / in.

[0190] 3. Dielectric loss (dissipation factor, Df@10GHz)

[0191] The aforementioned copper-free substrate (2-ply) was selected as the sample to be tested, and a microwave dielectric analyzer (microwave dielectric analyzer, purchased from AET Co., Ltd., Japan) was used to measure the dielectric loss of each sample to be tested at room temperature (about 25°C) and a frequency of 10 GHz according to the method described in JIS C2565. The lower the dielectric loss, the better the dielectric properties of the sample to be tested.

[0192] 4. Percent of thermal expansion, Z-axis, Z-PTE

[0193] The aforementioned copper-free substrate (8-ply) was used to prepare the test samples, and the thermal mechanical analysis (TMA) was performed according to the method of IPC-TM-650 2.4.24.5. The temperature was raised from 50°C to 260°C at a heating rate of 10°C / min, and the Z-axis thermal expansion coefficient (in %) of each test sample in the temperature range of 50°C to 260°C was measured.

[0194] 5. Dielectric loss thermal change rate (Df thermal change rate, ΔDf change rate 1)

[0195] The aforementioned copper-free substrate (2-ply) was selected as the sample to be tested, and a microwave dielectric analyzer (microwavedielectrometer, purchased from AET, Japan) was used to measure the dielectric loss of each sample to be tested at room temperature (about 25°C) and a frequency of 10 GHz, referring to the method of JIS C2565, and recorded as Df1. Each sample to be tested was cleaned with distilled water and placed in an environment of 125°C for 120 hours, and then its dielectric loss at a frequency of 10 GHz was tested, recorded as Df2, where Df thermal change rate =

[0196] [(Df2-Df1) / Df1]*100%. The lower the dielectric loss thermal change rate, the better the dielectric stability of the sample in a thermal environment.

[0197] 6. Dielectric loss hygrothermal change rate (Df hygrothermal change rate, ΔDf change rate 2)

[0198] The aforementioned copper-free substrate (2-ply) was selected as the sample to be tested, and a microwave dielectric analyzer (microwavedielectrometer, purchased from Japan AET Company) was used, referring to the method of JIS C2565, and the dielectric loss of each sample to be tested was measured at room temperature (about 25°C) and a frequency of 10GHz, which was recorded as Df3. After each sample to be tested was cleaned with distilled water, it was placed in an environment of 85°C and 85% relative humidity for 176 hours, and then its dielectric loss at a frequency of 10GHz was tested, which was recorded as Df4, wherein the Df wet-heat change rate = [(Df4-Df3) / Df3]*100%. The lower the wet-heat change rate of dielectric loss, the better the dielectric stability of the sample in a wet-heat environment.

[0199] By referring to the characteristic test results in Tables 1 to 3, the following phenomena can be clearly observed.

[0200] From Examples E1 to E14, it can be determined that the resin composition of the present invention and its products can be improved in one or more of the properties such as glass transition temperature, copper foil tension, dielectric loss, Z-axis thermal expansion coefficient, dielectric loss thermal change rate, and dielectric loss wet heat change rate.

[0201] Examples E1 to E9 use a polyphenylene ether resin containing unsaturated carbon-carbon double bonds and a compound of formula (1) without prepolymerization, and Examples E10 to E14 use a prepolymer of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds and a compound of formula (1). By observing the test results of Examples E1 to E9 and the test results of Examples E10 to E14, it can be found that the resin composition using the prepolymer of the present invention and its products have achieved significant improvements in at least two properties, namely, dielectric loss thermal change rate and dielectric loss wet heat change rate, compared with the resin composition containing a polyphenylene ether resin containing unsaturated carbon-carbon double bonds and a compound of formula (1) without prepolymerization and its products.

[0202] By comparing Examples E1 to E9 and Comparative Examples C1 to C2, it can be found that if the content of the compound of formula (1) is not within the range of 10 to 50 parts by weight relative to 100 parts by weight of the polyphenylene ether resin containing unsaturated carbon-carbon double bonds, the corresponding resin composition and its products cannot be improved in at least three properties: copper foil tensile force, dielectric loss thermal change rate, and dielectric loss wet-heat change rate.

[0203] By comparing Examples E1 to E9 and Comparative Examples C3 to C8, it can be found that the resin composition and its products using the compound of formula (1) of the present invention have achieved significant improvements in at least two properties, namely, dielectric loss thermal change rate and dielectric loss wet-heat change rate, compared with using BVPE or Compound D1 to Compound D5.

[0204] The above implementation modes and examples are essentially only for auxiliary explanation and are not intended to limit the embodiments of the present invention or the application or use of these embodiments. In the present invention, a term similar to "example" means "as an example, example or illustration". Any exemplary embodiment herein is not necessarily interpreted as being preferred or more advantageous relative to other embodiments, unless otherwise specified.

[0205] In addition, although at least one exemplary embodiment or comparative example has been proposed in the aforementioned embodiment, it should be understood that the present invention can still have a large number of variations. It should also be understood that the embodiments herein are not intended to limit the scope, use or configuration of the requested technical solution in any way. On the contrary, the aforementioned embodiment can provide a simple guide for those skilled in the art to implement one or more of the aforementioned embodiments and their equivalents. In addition, the claims include known equivalents and all foreseeable equivalents when the present patent application is filed.

Claims

1. A resin composition, It is characterized in that Comprising the following ingredients or their prepolymers: (A) 100 parts by weight of a polyphenylene ether resin containing unsaturated carbon-carbon double bonds; and (B) 10 to 50 parts by weight of a compound of formula (1); In formula (1), n ​​represents the average number of repeating units, and n is a value of 0 to 4; when n is 0, R is a hydrogen atom or a vinyl group; when n is not 0, R is a vinyl group; The prepolymer is obtained by prepolymerization of a mixture, and the mixture at least includes the component (A) and the component (B).

2. The resin composition according to claim 1, It is characterized in that The polyphenylene ether resin containing unsaturated carbon-carbon double bonds includes any one of vinylbenzyl polyphenylene ether resin, (meth)acryl polyphenylene ether resin, vinyl polyphenylene ether resin, and allyl polyphenylene ether resin, or a combination thereof.

3. The resin composition according to claim 1, It is characterized in that The compound of formula (1) includes a compound of formula (1-1), a compound of formula (1-2) or a combination thereof:

4. The resin composition according to claim 1, It is characterized in that The compound of formula (1) includes a structure in which n is not 0 and R is a vinyl group.

5. The resin composition according to claim 1, It is characterized in that The conversion rate of the prepolymerization reaction is between 10% and 99%.

6. The resin composition according to claim 1, It is characterized in that The resin composition does not contain epoxy resin.

7. The resin composition according to claim 1, It is characterized in that The resin composition further comprises polyolefin, a crosslinking agent containing unsaturated carbon-carbon double bonds which is different from the compound of formula (1), a silicone resin, a benzoxazine resin, a polyester resin, a phenolic resin, an amine curing agent, a polyamide, a polyimide, styrene maleic anhydride, a maleimide resin, a cyanate resin, a maleimide triazine resin or a combination thereof.

8. The resin composition according to claim 1, It is characterized in that The resin composition further includes a hardening accelerator, a polymerization inhibitor, a flame retardant, an inorganic filler, a surface treatment agent, a coloring agent, a toughening agent, a solvent or a combination thereof.

9. An article made from the resin composition according to claim 1, It is characterized in that The product includes a prepreg, a resin film, a laminate or a printed circuit board.

10. The product according to claim 9, It is characterized in that The product has one, more or all of the following characteristics: The glass transition temperature measured by the method described in IPC-TM-650 2.4.24.4 is greater than or equal to 221°C; The copper foil tensile force measured by the method described in IPC-TM-650 2.4.8 is greater than or equal to 3.6 lb / in; The dielectric loss measured at a frequency of 10 GHz according to the method described in JIS C2565 is less than or equal to 0.00215; The Z-axis thermal expansion rate measured by the method described in IPC-TM-650 2.4.24.5 is less than or equal to 1.6%; The dielectric loss thermal change rate calculated from the dielectric loss measured at a frequency of 10 GHz according to the method described in JIS C2565 after being allowed to stand at a constant temperature of 125° C. for 120 hours is less than or equal to 51.5%; and After being left to stand for 176 hours at a constant temperature of 85° C. and a relative humidity of 85%, the dielectric loss calculated by measuring the dielectric loss at a frequency of 10 GHz according to the method described in JIS C2565 has a dielectric loss hygrothermal change rate of less than or equal to 36.0%.

Citation Information

Patent Citations

  • Resin composition and article prepared from same

    CN109796745A

  • Composition containing polyser, poly (arylidene thio-ether), paraplex and compatilizer compound

    CN1135502A

  • Resin composition and product thereof

    CN115785647A

  • A polyphenylene ether resin and resin compositions and articles containing the same.

    TWI744031B

  • Modification method of polyphenylene ether resin, laminated film composite, laminated film, and substrate

    US20240052098A1