Dual modified adhesive, preparation method and application thereof, and putty paste for interior wall

By oxidizing, gelatinizing, and cross-linking starch-based adhesives, and combining this with the Schiff base reaction of polyvinyl alcohol and soy protein isolate, the problems of poor water resistance, low bonding strength, and poor flowability of starch-based adhesives have been solved, resulting in a high-performance adhesive with no formaldehyde pollution, suitable for interior wall putty.

CN118994962AInactive Publication Date: 2024-11-22SOUTHWEST UNIV

Patent Information

Application Number
CN202411279720.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional starch-based adhesives suffer from poor water resistance, low bonding strength, poor flowability, and instability, and contain harmful substances such as formaldehyde, which limits their widespread use in building decoration.

Method used

A dual-modified adhesive preparation method is adopted, which involves oxidizing, gelatinizing and cross-linking starch, and introducing polyvinyl alcohol and soy protein isolate for Schiff base reaction to form a tight network structure, thereby improving the bonding strength and water resistance.

Benefits of technology

The prepared adhesive is free of formaldehyde pollution, has good bonding strength, water resistance and fluidity, and excellent stability. It is suitable for interior wall putty, improving human health safety and construction performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118994962A_ABST
    Figure CN118994962A_ABST
Patent Text Reader

Abstract

The invention relates to a dual-modified adhesive, a preparation method and application thereof, and putty paste for an inner wall. The double-modified adhesive is prepared from starch, a cross-linking agent, an oxidizing agent, a catalyst, a gelatinizing agent, an initiator, a reinforcing agent, lauryl sodium sulfate, silica sol and water. The invention also provides a preparation method of the double modified adhesive. The preparation method comprises the following steps: pretreating starch to obtain oxidized starch; carrying out gelatinization-crosslinking treatment on the oxidized starch to obtain a gelatinized-crosslinked-oxidized starch adhesive; and carrying out Schiff base reaction on the gelatinized-cross-linked-oxidized starch adhesive to obtain the starch oxidation / cross-linked dual modified adhesive suitable for the interior wall putty. The invention also provides application of the dual modified adhesive in interior wall putty. The invention also provides the interior wall putty paste containing the double modified adhesive, talcum powder and water. According to the invention, the defects of the traditional starch adhesive in the aspects of water resistance, bonding strength, fluidity, stability and the like are effectively overcome.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of composite polymer materials, and in particular to a double-modified adhesive and a preparation method and application thereof, as well as a putty paste for interior walls. Background Art

[0002] Adhesives are an important component of building putty pastes. Currently, the adhesives widely used in the market are mainly based on petrochemical raw materials, especially formaldehyde-based synthetic resins. However, such adhesives have the risk of releasing harmful substances such as formaldehyde and rely on non-renewable resources such as petroleum, which poses a potential threat to the sustainable development of society. Therefore, the development of bio-based adhesives based on renewable resources such as starch, bioprotein, tannin and lignin to replace traditional formaldehyde-based synthetic resins is gradually becoming the focus of industry attention.

[0003] In the preparation process of traditional starch-based adhesives for interior walls, hydrogen bonds are easily formed between starch and water, giving it extremely high hydrophilicity, which leads to poor water resistance. There are a large number of hydrogen bonds within and between starch molecules, which limit the flexibility and mobility of the molecules, making it difficult to contact and infiltrate the surface of the adherend during the bonding process, ultimately resulting in low bonding strength of the adhesive. In addition, traditional starch-based adhesives have poor fluidity, making it difficult to distribute evenly during application, thus affecting the quality of the final product. In addition, starch-based adhesives are also easily affected by environmental factors such as temperature and humidity, resulting in performance fluctuations and even failure during storage and use. These problems limit the widespread use of starch-based adhesives in industrial applications, and therefore urgently need to be solved by improving the formula or developing new alternatives. Summary of the invention

[0004] The purpose of the present invention is to provide a double-modified adhesive and a preparation method and application thereof, as well as a putty paste for interior walls, so as to solve the problems of poor water resistance, low bonding strength, poor fluidity and instability of traditional starch adhesives, and also solve the problem that the existing putty glue for interior decoration of buildings contains formaldehyde that harms human health.

[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0006] A double-modified adhesive comprises the following raw materials: starch, a cross-linking agent, an oxidant, a catalyst, a gelatinizer, an initiator, a reinforcing agent, sodium dodecyl sulfate, silica sol and water.

[0007] Preferably, the double modified adhesive comprises the following raw materials, by weight: 40 to 60 parts by weight of starch, 60 to 70 parts by weight of a cross-linking agent, 6 to 10 parts by weight of an oxidant, 0.01 to 0.02 parts by weight of a catalyst, 2 to 5 parts by weight of a gelatinizer, 6 to 10 parts by weight of an initiator, 15 to 25 parts by weight of a reinforcing agent, 2 to 6 parts by weight of sodium dodecyl sulfate, 10 to 20 parts by weight of silica sol and 1500 to 2500 parts by weight of water.

[0008] The double-modified adhesive comprises the following raw materials, measured in parts by weight: 60-70 parts by weight of starch, 50-60 parts by weight of a cross-linking agent, 6-10 parts by weight of an oxidant, 0.01-0.02 parts by weight of a catalyst, 2-5 parts by weight of a gelatinizer, 6-10 parts by weight of an initiator, 15-25 parts by weight of a reinforcing agent, 2-6 parts by weight of sodium dodecyl sulfate, 10-20 parts by weight of silica sol and 1500-2500 parts by weight of water.

[0009] Preferably, the starch is selected from hydroxypropyl distarch phosphate.

[0010] Preferably, the cross-linking agent is selected from polyvinyl alcohol solution.

[0011] Preferably, the oxidant is selected from at least one of sodium hypochlorite, hydrogen peroxide, sodium periodate and potassium permanganate.

[0012] Preferably, the catalyst is selected from nickel sulfate.

[0013] Preferably, the gelling agent is selected from sodium hydroxide.

[0014] Preferably, the initiator is selected from urea.

[0015] Preferably, the enhancer is selected from soy protein isolate.

[0016] Preferably, the solid content of the silica sol is 20-30 wt %.

[0017] Preferably, the pH value of the silica sol is 7-9.

[0018] Preferably, the available chlorine content in the sodium hypochlorite is 20%.

[0019] Preferably, the purity of the sodium hypochlorite is 99%.

[0020] The present invention also provides a method for preparing the dual-modified adhesive according to the present invention, comprising the following steps:

[0021] S1. pretreating starch to obtain oxidized starch (OST);

[0022] S2, gelatinizing and cross-linking the oxidized starch to obtain a gelatinized-cross-linked-oxidized starch adhesive (OST-PVA);

[0023] S3. The gelatinized-crosslinked-oxidized starch adhesive is subjected to a Schiff base reaction to obtain a starch oxidation / crosslinked double-modified adhesive (OST-PVA-SPI-U) for interior wall putty.

[0024] Preferably, the S1 includes:

[0025] Starch, an oxidant and a catalyst are added into water, fully stirred at room temperature, and allowed to stand for a period of time to obtain a mixed starch liquid containing oxidized starch.

[0026] Preferably, S2 includes:

[0027] S21, adding a crosslinking agent into water, and heating until completely dissolved to obtain a crosslinking agent solution;

[0028] S22, adding a gelatinizer to the cross-linking agent solution, adjusting the pH value to 9-11, then adding oxidized starch, heating to perform gelatinization-cross-linking reaction, and obtaining a gelatinization-cross-linking-oxidized starch adhesive.

[0029] Preferably, the standing time is 10 h to 14 h.

[0030] Preferably, the temperature for heating to complete dissolution is 95°C.

[0031] Preferably, the heating temperature of the gelatinization-crosslinking reaction is 80°C to 90°C.

[0032] Preferably, the gelatinization-crosslinking reaction time is 30 min to 40 min, so that the gelatinization-crosslinking reaction can be fully carried out.

[0033] Preferably, S3 includes:

[0034] S31, adding the enhancer into water, then adding sodium lauryl sulfate, stirring evenly to obtain a first mixed material;

[0035] S32, adding the mixed material to the gelatinized-crosslinked-oxidized starch adhesive, heating and stirring to react, to obtain a second mixed material;

[0036] S33, cooling the second mixed material, adding silica sol, stirring and mixing evenly, mixing and reacting, cooling the discharged material to room temperature, and obtaining a double-modified adhesive.

[0037] Preferably, the temperature of the heating and stirring reaction is 80°C to 90°C.

[0038] Preferably, the heating and stirring reaction time is 2h to 3h.

[0039] Preferably, the second mixed material is cooled to 60°C.

[0040] Preferably, the mixing reaction time is 15 min to 20 min.

[0041] The present invention also provides an application of the double-modified adhesive prepared by the preparation method of the present invention as a starch adhesive for interior wall putty.

[0042] The invention also provides a putty paste for interior walls, comprising the double-modified adhesive prepared by the preparation method of the invention, talcum powder and water.

[0043] Preferably, the particle size of the talc is 10 to 60 microns.

[0044] Preferably, the weight proportion of the double modified adhesive is 15-20, the weight proportion of talc is 180-200, and the weight proportion of water is 60-80.

[0045] Preferably, the mass ratio of the double-modified adhesive, talcum powder and water is 15:200:80.

[0046] Beneficial effects of the present invention:

[0047] The double modified adhesive of the present invention uses starch and polyvinyl alcohol as main raw materials, and the adhesive does not contain pollutants such as formaldehyde, and no toxic and harmful substances are added to the raw materials, thereby effectively preventing the generation and release of toxic and harmful substances, significantly reducing pollution to the environment, and improving human health and safety. After experimental testing, the double modified adhesive exhibits the advantages of no agglomeration, uniform mixing, excellent low-temperature storage stability, strong workability, no cracks in the initial drying stage, easy grinding, good water resistance and high bonding strength.

[0048] The invention provides a method for preparing a double modified adhesive. The method effectively improves the bonding strength and water resistance of the adhesive by oxidizing, gelatinizing and cross-linking starch, and introducing a primary amine compound to perform a Schiff base reaction. Specifically, firstly, sodium hypochlorite is used as an oxidant to cause the hydroxypropyl distarch phosphate to undergo a glucosidic bond breakage under its action, resulting in the oxidation of some secondary hydroxyl groups at the C2 and C3 positions in the molecule to aldehyde groups. At the same time, phosphoric acid also has an acidolysis effect on starch molecules, promoting the formation of a cross-linked structure, which is beneficial to the reaction. The oxidized starch contains aldehyde groups and carboxyl groups, showing good anti-corrosion and anti-mildew capabilities, as well as excellent cooking stability, dispersibility, cold flow and bonding properties. Secondly, polyvinyl alcohol is selected as a cross-linking agent because of its non-toxicity, non-irritation, water solubility, good adhesion and biocompatibility. A large number of secondary hydroxyl groups and a small amount of acetoxy groups in the polyvinyl alcohol molecule react with the starch molecular chain to form free radicals, which are combined with the polymer monomer to form a polymer molecular chain. This process makes the adhesive have significant advantages in terms of adhesion, fluidity and anti-freezing properties. Finally, urea is used as an initiator and soy protein isolate is used as a reinforcing agent. The aldehyde groups formed by starch during the oxidation process react with the amino groups rich in urea and soy protein molecules to form a tight network structure, which further effectively improves the bonding strength of the adhesive. This preparation method has the advantages of simple process, mild reaction conditions, no by-products, abundant raw material sources, biodegradability, no pollution and low price. It provides favorable guarantees for the industrial production of bio-based adhesives and has important application value in the field of composite polymer material technology.

[0049] Secondly, polyvinyl alcohol is used as a cross-linking agent because of its non-toxic, non-irritating, water-soluble, excellent adhesion and biocompatibility. The secondary hydroxyl group and a small amount of acetoxy group in its molecular structure react with the starch molecular chain to form free radicals, which combine with the polymer monomer to form a polymer molecular chain, thereby giving the adhesive better adhesion, fluidity and anti-freezing properties. In addition, urea is used as an initiator and soy protein isolate is used as a reinforcing agent. The aldehyde group formed in the starch reacts with the amino group in urea and soy protein to form a tight network structure, further improving the bonding strength of the adhesive. The preparation method has the advantages of simple process operation, mild reaction conditions, no by-products, a wide range of raw material sources, biodegradability, no plastic pollution and low cost, etc., which provides strong support for the industrial production of bio-based adhesives, has significant industrial production potential, and shows potential application prospects in the field of composite polymer material technology. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] Figure 1 Flow chart for the preparation of dual modified adhesive;

[0051] Figure 2Fourier transform infrared spectra (FTIR) of oxidized starch (OST), polyvinyl alcohol (PVA) and gelatinized-cross-linked-oxidized starch adhesive (OST-PVA);

[0052] Figure 3 FTIR spectra of soy protein isolate (SPI), gelatinized-cross-linked-oxidized starch adhesive (OST-PVA) and double modified adhesive (OST-PVA-SPI-U). DETAILED DESCRIPTION

[0053] The following will describe the embodiments of the present invention with reference to the accompanying drawings and preferred embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be understood that the preferred embodiments are only for illustrating the present invention, not for limiting the scope of protection of the present invention.

[0054] Example 1

[0055] like Figure 1 As shown, a method for preparing a double-modified adhesive comprises the following steps:

[0056] S1. Pretreating starch to obtain oxidized starch, specifically comprising:

[0057] 60 g of hydroxypropyl distarch phosphate, 8 g of sodium hypochlorite and 0.0125 g of nickel sulfate were dissolved in 100 g of water, stirred at a speed of 125 rad / min for 20 min, and then allowed to stand for 12 h to obtain oxidized starch;

[0058] S2, gelatinizing and cross-linking the oxidized starch to obtain a gelatinized-cross-linked-oxidized starch adhesive, specifically comprising:

[0059] Dissolve 50 g of polyvinyl alcohol in 2 kg of water, heat to 95°C, add 3 g of sodium hydroxide, and adjust the pH value to 11 to obtain a crosslinking agent;

[0060] The oxidized starch and the cross-linking agent were mixed and stirred at a temperature of 85°C and a rotation speed of 90 rad / min for 30 min to obtain a gelatinized

[0061] - Cross-linked-oxidized starch adhesive;

[0062] S3, performing Schiff base reaction on the gelatinized-crosslinked-oxidized starch adhesive to obtain a double-modified adhesive, specifically comprising:

[0063] To the gelatinized-cross-linked-oxidized starch adhesive prepared in S2, add 20 g of soy protein isolate, 8 g of urea, and 5 g of sodium dodecyl sulfate, then stir for 2 h at a temperature of 80 ° C and a rotation speed of 90 rad / min, cool to 60 ° C, add 15 g of silica sol, stir for 15 min to 20 min, and cool to room temperature to obtain a starch oxidation / cross-linking dual-modified adhesive for interior wall putty.

[0064] Example 2

[0065] like Figure 1 As shown, a method for preparing a double-modified adhesive comprises the following steps:

[0066] S1. Pretreating starch to obtain oxidized starch, specifically comprising:

[0067] 70 g of hydroxypropyl distarch phosphate, 10 g of sodium hypochlorite and 0.0125 g of nickel sulfate were dissolved in 100 g of water, stirred at a speed of 125 rad / min for 20 min, and then allowed to stand for 12 h to obtain oxidized starch;

[0068] S2, gelatinizing and cross-linking the oxidized starch to obtain a gelatinized-cross-linked-oxidized starch adhesive, specifically comprising:

[0069] Dissolve 50 g of polyvinyl alcohol in 2 kg of water, heat to 95°C, add 3 g of sodium hydroxide, and adjust the pH value to 11 to obtain a crosslinking agent;

[0070] The oxidized starch and the cross-linking agent were mixed, and stirred at a temperature of 85° C. and a rotation speed of 90 rad / min for 30 minutes to prepare a gelatinized-cross-linked-oxidized starch adhesive;

[0071] S3, performing Schiff base reaction on the gelatinized-crosslinked-oxidized starch adhesive to obtain a double-modified adhesive, specifically comprising:

[0072] To the gelatinized-cross-linked-oxidized starch adhesive prepared in S2, add 20 g of soy protein isolate, 8 g of urea, and 5 g of sodium dodecyl sulfate, then stir for 2 h at a temperature of 80 ° C and a rotation speed of 90 rad / min, cool to 60 ° C, add 15 g of silica sol, stir for 15 min to 20 min, and cool to room temperature to obtain a starch oxidation / cross-linking dual-modified adhesive for interior wall putty.

[0073] Example 3

[0074] like Figure 1 As shown, a method for preparing a double-modified adhesive comprises the following steps:

[0075] S1. Pretreating starch to obtain oxidized starch, specifically comprising:

[0076] 60 g of hydroxypropyl distarch phosphate, 8 g of sodium hypochlorite and 0.0125 g of nickel sulfate were dissolved in 100 g of water, stirred at a speed of 125 rad / min for 20 min, and then allowed to stand for 12 h to obtain oxidized starch;

[0077] S2, gelatinizing and cross-linking the oxidized starch to obtain a gelatinized-cross-linked-oxidized starch adhesive, specifically comprising:

[0078] Dissolve 60 g of polyvinyl alcohol in 2 kg of water, heat to 95° C., add 3 g of sodium hydroxide, and adjust the pH value to 11 to obtain a crosslinking agent;

[0079] The oxidized starch and the cross-linking agent were mixed, and stirred at a temperature of 85° C. and a rotation speed of 90 rad / min for 30 minutes to prepare a gelatinized-cross-linked-oxidized starch adhesive;

[0080] S3, performing Schiff base reaction on the gelatinized-crosslinked-oxidized starch adhesive to obtain a double-modified adhesive, specifically comprising:

[0081] To the gelatinized-cross-linked-oxidized starch adhesive prepared in S2, add 20 g of soy protein isolate, 8 g of urea, and 5 g of sodium dodecyl sulfate, then stir for 2 h at a temperature of 80 ° C and a rotation speed of 90 rad / min, cool to 60 ° C, add 15 g of silica sol, stir for 15 min to 20 min, and cool to room temperature to obtain a starch oxidation / cross-linking dual-modified adhesive for interior wall putty.

[0082] Example 4

[0083] like Figure 1 As shown, a method for preparing a double-modified adhesive comprises the following steps:

[0084] S1. Pretreating starch to obtain oxidized starch, specifically comprising:

[0085] 70 g of hydroxypropyl distarch phosphate, 10 g of sodium hypochlorite and 0.0125 g of nickel sulfate were dissolved in 100 g of water, stirred at a speed of 125 rad / min for 20 min, and then allowed to stand for 12 h to obtain oxidized starch;

[0086] S2, gelatinizing and cross-linking the oxidized starch to obtain a gelatinized-cross-linked-oxidized starch adhesive, specifically comprising:

[0087] Dissolve 60 g of polyvinyl alcohol in 2 kg of water, heat to 95° C., add 3 g of sodium hydroxide, and adjust the pH value to 11 to obtain a crosslinking agent;

[0088] The oxidized starch and the cross-linking agent were mixed, and stirred at a temperature of 85° C. and a rotation speed of 90 rad / min for 30 minutes to prepare a gelatinized-cross-linked-oxidized starch adhesive;

[0089] S3, performing Schiff base reaction on the gelatinized-crosslinked-oxidized starch adhesive to obtain a double-modified adhesive, specifically comprising:

[0090] To the gelatinized-cross-linked-oxidized starch adhesive prepared in S2, add 20 g of soy protein isolate, 8 g of urea, and 5 g of sodium dodecyl sulfate, then stir for 2 h at a temperature of 80 ° C and a rotation speed of 90 rad / min, cool to 60 ° C, add 15 g of silica sol, stir for 15 min to 20 min, and cool to room temperature to obtain a starch oxidation / cross-linking dual-modified adhesive for interior wall putty.

[0091] Example 5

[0092] like Figure 1 As shown, a method for preparing a double-modified adhesive comprises the following steps:

[0093] S1. Pretreating starch to obtain oxidized starch, specifically comprising:

[0094] 70 g of hydroxypropyl distarch phosphate, 10 g of sodium hypochlorite and 0.0125 g of nickel sulfate were dissolved in 100 g of water, stirred at a speed of 125 rad / min for 20 min, and then allowed to stand for 12 h to obtain oxidized starch;

[0095] S2, gelatinizing and cross-linking the oxidized starch to obtain a gelatinized-cross-linked-oxidized starch adhesive, specifically comprising:

[0096] Dissolve 60 g of polyvinyl alcohol in 2 kg of water, heat to 95° C., add 3 g of sodium hydroxide, and adjust the pH value to 11 to obtain a crosslinking agent;

[0097] The oxidized starch and the cross-linking agent were mixed, and stirred at a temperature of 85° C. and a rotation speed of 90 rad / min for 30 minutes to prepare a gelatinized-cross-linked-oxidized starch adhesive;

[0098] S3, performing Schiff base reaction on the gelatinized-crosslinked-oxidized starch adhesive to obtain a double-modified adhesive, specifically comprising:

[0099] To the gelatinized-cross-linked-oxidized starch adhesive prepared in S2, add 25 g of soy protein isolate, 8 g of urea, and 5 g of sodium dodecyl sulfate, then stir for 2 h at a temperature of 80 ° C and a rotation speed of 90 rad / min, cool to 60 ° C, add 15 g of silica sol, stir for 15 min to 20 min, and cool to room temperature to obtain a starch oxidation / cross-linking dual-modified adhesive for interior wall putty.

[0100] Example 6

[0101] like Figure 1 As shown, a method for preparing a double-modified adhesive comprises the following steps:

[0102] S1. Pretreating starch to obtain oxidized starch, specifically comprising:

[0103] 60 g of hydroxypropyl distarch phosphate, 10 g of sodium hypochlorite and 0.0125 g of nickel sulfate were dissolved in 100 g of water, stirred at a speed of 125 rad / min for 20 min, and then allowed to stand for 12 h to obtain oxidized starch;

[0104] S2, gelatinizing and cross-linking the oxidized starch to obtain a gelatinized-cross-linked-oxidized starch adhesive, specifically comprising:

[0105] Dissolve 60 g of polyvinyl alcohol in 2 kg of water, heat to 95° C., add 3 g of sodium hydroxide, and adjust the pH value to 11 to obtain a crosslinking agent;

[0106] The oxidized starch and the cross-linking agent were mixed, and stirred at a temperature of 85° C. and a rotation speed of 90 rad / min for 30 minutes to prepare a gelatinized-cross-linked-oxidized starch adhesive;

[0107] S3, performing Schiff base reaction on the gelatinized-crosslinked-oxidized starch adhesive to obtain a double-modified adhesive, specifically comprising:

[0108] To the gelatinized-cross-linked-oxidized starch adhesive prepared in S2, add 25 g of soy protein isolate, 8 g of urea, and 5 g of sodium dodecyl sulfate, then stir for 2 h at a temperature of 80 ° C and a rotation speed of 90 rad / min, cool to 60 ° C, add 15 g of silica sol, stir for 15 min to 20 min, and cool to room temperature to obtain a starch oxidation / cross-linking dual-modified adhesive for interior wall putty.

[0109] Example 7

[0110] like Figure 1 As shown, a method for preparing a double-modified adhesive comprises the following steps:

[0111] S1. Pretreating starch to obtain oxidized starch, specifically comprising:

[0112] 60 g of hydroxypropyl distarch phosphate, 10 g of sodium hypochlorite and 0.0125 g of nickel sulfate were dissolved in 100 g of water, stirred at a speed of 125 rad / min for 20 min, and then allowed to stand for 12 h to obtain oxidized starch;

[0113] S2, gelatinizing and cross-linking the oxidized starch to obtain a gelatinized-cross-linked-oxidized starch adhesive, specifically comprising:

[0114] Dissolve 60 g of polyvinyl alcohol in 2 kg of water, heat to 95° C., add 3 g of sodium hydroxide, and adjust the pH value to 11 to obtain a crosslinking agent;

[0115] The oxidized starch and the cross-linking agent were mixed, and stirred at a temperature of 85° C. and a rotation speed of 90 rad / min for 30 minutes to prepare a gelatinized-cross-linked-oxidized starch adhesive;

[0116] S3, performing Schiff base reaction on the gelatinized-crosslinked-oxidized starch adhesive to obtain a double-modified adhesive, specifically comprising:

[0117] To the gelatinized-cross-linked-oxidized starch adhesive prepared in S2, add 25 g of soy protein isolate, 8 g of urea, and 5 g of sodium dodecyl sulfate, then stir for 2 h at a temperature of 80 ° C and a rotation speed of 90 rad / min, cool to 60 ° C, add 15 g of silica sol, stir for 15 min to 20 min, and cool to room temperature to obtain a starch oxidation / cross-linking dual-modified adhesive for interior wall putty.

[0118] Example 8

[0119] like Figure 1 As shown, a method for preparing a double-modified adhesive comprises the following steps:

[0120] S1. Pretreating starch to obtain oxidized starch, specifically comprising:

[0121] 60 g of hydroxypropyl distarch phosphate, 10 g of sodium hypochlorite and 0.0125 g of nickel sulfate were dissolved in 100 g of water, stirred at a speed of 125 rad / min for 20 min, and then allowed to stand for 12 h to obtain oxidized starch;

[0122] S2, gelatinizing and cross-linking the oxidized starch to obtain a gelatinized-cross-linked-oxidized starch adhesive, specifically comprising:

[0123] Dissolve 50 g of polyvinyl alcohol in 2 kg of water, heat to 95°C, add 3 g of sodium hydroxide, and adjust the pH value to 11 to obtain a crosslinking agent;

[0124] The oxidized starch and the cross-linking agent were mixed, and stirred at a temperature of 85° C. and a rotation speed of 90 rad / min for 30 minutes to prepare a gelatinized-cross-linked-oxidized starch adhesive;

[0125] S3, performing Schiff base reaction on the gelatinized-crosslinked-oxidized starch adhesive to obtain a double-modified adhesive, specifically comprising:

[0126] To the gelatinized-cross-linked-oxidized starch adhesive prepared in S2, add 25 g of soy protein isolate, 8 g of urea, and 5 g of sodium dodecyl sulfate, then stir for 2 h at a temperature of 80 ° C and a rotation speed of 90 rad / min, cool to 60 ° C, add 15 g of silica sol, stir for 15 min to 20 min, and cool to room temperature to obtain a starch oxidation / cross-linking dual-modified adhesive for interior wall putty.

[0127] Example 9

[0128] A method for preparing a putty paste for interior walls comprises the following steps:

[0129] 15 g of the double-modified adhesive prepared in Example 1, 200 g of talcum powder with a particle size of 10 to 60 μm, and 80 g of water were mixed evenly to obtain a putty paste for interior walls.

[0130] Example 10

[0131] A method for preparing a putty paste for interior walls comprises the following steps:

[0132] 15 g of the double-modified adhesive prepared in Example 2, 200 g of talcum powder with a particle size of 10 to 60 μm, and 80 g of water were mixed evenly to obtain a putty paste for interior walls.

[0133] Embodiment 11

[0134] A method for preparing a putty paste for interior walls comprises the following steps:

[0135] 15 g of the double-modified adhesive prepared in Example 3, 200 g of talcum powder with a particle size of 10 to 60 μm, and 80 g of water were mixed evenly to obtain a putty paste for interior walls.

[0136] Example 12

[0137] A method for preparing a putty paste for interior walls comprises the following steps:

[0138] 15 g of the double-modified adhesive prepared in Example 4, 200 g of talcum powder with a particle size of 10 to 60 μm, and 80 g of water were mixed evenly to obtain a putty paste for interior walls.

[0139] Example 13

[0140] A method for preparing a putty paste for interior walls comprises the following steps:

[0141] 15 g of the double-modified adhesive prepared in Example 5, 200 g of talcum powder with a particle size of 10 to 60 μm, and 80 g of water were mixed evenly to obtain a putty paste for interior walls.

[0142] Embodiment 14

[0143] A method for preparing a putty paste for interior walls comprises the following steps:

[0144] 15 g of the double-modified adhesive prepared in Example 6, 200 g of talcum powder with a particle size of 10 to 60 μm, and 80 g of water were mixed evenly to obtain a putty paste for interior walls.

[0145] Embodiment 15

[0146] A method for preparing a putty paste for interior walls comprises the following steps:

[0147] 15 g of the double-modified adhesive prepared in Example 7, 200 g of talcum powder with a particle size of 10 to 60 μm, and 80 g of water were mixed evenly to obtain a putty paste for interior walls.

[0148] Example 16

[0149] A method for preparing a putty paste for interior walls comprises the following steps:

[0150] 15 g of the double-modified adhesive prepared in Example 8, 200 g of talcum powder with a particle size of 10 to 60 μm, and 80 g of water were mixed evenly to obtain a putty paste for interior walls.

[0151] Comparative Example 1

[0152] A method for preparing a conventional interior wall putty paste comprises the following steps:

[0153] S1. Dissolve 70 g of hydroxypropyl distarch phosphate, 10 g of sodium hypochlorite and 0.0125 g of nickel sulfate in 100 g of water, stir for 20 min at a speed of 125 rad / min, and let stand for 12 h to obtain oxidized starch;

[0154] S2, dissolving 60g of polyvinyl alcohol in 2kg of water, heating to 95°C, adding 3g of sodium hydroxide, adjusting the pH value to 11, and obtaining a cross-linking agent;

[0155] The oxidized starch paste and the cross-linking agent were mixed, and stirred at a temperature of 85° C. and a rotation speed of 90 rad / min for 30 minutes to prepare a cross-linked-gelatinized-oxidized starch adhesive;

[0156] S3. Take 15 g of cross-linked-gelatinized-oxidized starch adhesive, 200 g of talcum powder with a particle size of 10 to 60 μm and 80 g of water and mix them evenly to obtain an interior wall putty paste.

[0157] Comparative Example 2

[0158] A method for preparing a conventional interior wall putty paste comprises the following steps:

[0159] S1. Dissolve 70 g of hydroxypropyl distarch phosphate, 10 g of sodium hypochlorite and 0.0125 g of nickel sulfate in 100 g of water, stir for 20 min at a speed of 125 rad / min, and let stand for 12 h to obtain oxidized starch;

[0160] S2, adding 3 g of sodium hydroxide to the oxidized starch, stirring for 30 min at a temperature of 85° C. and a rotation speed of 90 rad / min to obtain a gelatinized-oxidized starch adhesive;

[0161] S3, add 20g soy protein isolate, 8g urea, 5g sodium dodecyl sulfate to the gelatinized-oxidized starch adhesive, stir for 2h at a temperature of 80°C and a rotation speed of 90rad / min, cool to 60°C, add 15g silica sol, stir for 15min-20min, cool to room temperature, and obtain a starch oxidation modified adhesive for interior wall putty;

[0162] S4. Take 15 g of starch oxidation-modified adhesive for interior wall putty, 200 g of talcum powder with a particle size of 10 to 60 microns and 80 g of water and mix them evenly to obtain an interior wall putty paste.

[0163] Comparative Example 3

[0164] A method for preparing a conventional interior wall putty paste comprises the following steps:

[0165] S1, dissolving 60g of hydroxypropyl distarch phosphate in 100g of water, stirring at a speed of 125rad / min for 20min, stirring at a speed of 125rad / min for 20min, to obtain a starch solution;

[0166] Dissolve 50 g of polyvinyl alcohol in 2 kg of water, heat to 95°C, add 3 g of sodium hydroxide, and adjust the pH value to 11 to obtain a crosslinking agent;

[0167] The starch solution and the cross-linking agent were mixed, and stirred at a temperature of 85° C. and a rotation speed of 90 rad / min for 30 minutes to prepare a cross-linked-gelatinized starch adhesive;

[0168] S2, add 20g soy protein isolate, 8g urea, 5g sodium dodecyl sulfate to the cross-linked-gelatinized starch adhesive, stir for 2h at a temperature of 80°C and a rotation speed of 90rad / min, cool to 60°C, add 15g silica sol, stir for 15min-20min, cool to room temperature, and obtain a starch cross-linked modified adhesive for interior wall putty;

[0169] S3. Take 15 g of starch cross-linked modified adhesive for interior wall putty, 200 g of talcum powder with a particle size of 10 to 60 microns and 80 g of water and mix them evenly to obtain an interior wall putty paste.

[0170] Comparative Example 4

[0171] A method for preparing a conventional interior wall putty paste comprises the following steps:

[0172] S1. Dissolve 60 g of hydroxypropyl distarch phosphate, 8 g of sodium hypochlorite and 0.0125 g of nickel sulfate in 100 g of water, stir for 20 min at a speed of 125 rad / min, and let stand for 12 h to obtain oxidized starch;

[0173] S2, dissolving 60g of polyvinyl alcohol in 2kg of water, heating to 95°C, adding 3g of sodium hydroxide, adjusting the pH value to 11, and obtaining a cross-linking agent;

[0174] The oxidized starch and the cross-linking agent were mixed, and stirred at a temperature of 85° C. and a rotation speed of 90 rad / min for 30 minutes to prepare a cross-linked-gelatinized-oxidized starch adhesive;

[0175] S3, add 40g soy protein isolate, 8g urea, and 5g sodium dodecyl sulfate to the cross-linked-gelatinized-oxidized starch adhesive, stir for 2h at a temperature of 80°C and a rotation speed of 90rad / min, cool to 60°C, add 15g silica sol, stir for 15min-20min, and cool to room temperature to obtain a starch oxidation / cross-linking dual-modified adhesive for interior wall putty;

[0176] S4. Take 15 g of starch oxidation / cross-linking dual-modified adhesive for interior wall putty, 200 g of talcum powder with a particle size of 10 to 60 microns and 80 g of water and mix them evenly to obtain an interior wall putty paste.

[0177] Comparative Example 5

[0178] A method for preparing a conventional interior wall putty paste comprises the following steps:

[0179] S1, dissolving 60g of hydroxypropyl distarch phosphate, 8g of sodium hypochlorite and 0.0125g of nickel sulfate in 100g of water, stirring for 20min at a speed of 125rad / min, and standing for 12h to obtain oxidized starch;

[0180] S2, dissolving 100g of polyvinyl alcohol in 2kg of water, heating to 95°C, adding 3g of sodium hydroxide, adjusting the pH value to 11, and obtaining a cross-linking agent;

[0181] The oxidized starch and the cross-linking agent were mixed, and stirred at a temperature of 85° C. and a rotation speed of 90 rad / min for 30 minutes to prepare a cross-linked-gelatinized-oxidized starch adhesive;

[0182] S3, add 20g soy protein isolate, 8g urea, and 5g sodium dodecyl sulfate to the cross-linked-gelatinized-oxidized starch adhesive, stir for 2h at 80°C and a rotation speed of 90rad / min, cool to 60°C, add 15g silica sol, stir for 15min-20min, and cool to room temperature to obtain a starch oxidation / cross-linking dual modified adhesive for interior wall putty;

[0183] S4. Take 15 g of starch oxidation / cross-linking dual-modified adhesive for interior wall putty, 200 g of talcum powder with a particle size of 10 to 60 microns and 80 g of water and mix them evenly to obtain an interior wall putty paste.

[0184] Comparative Example 6

[0185] A method for preparing a conventional interior wall putty paste comprises the following steps:

[0186] S1, dissolving 60g of hydroxypropyl distarch phosphate, 8g of sodium hypochlorite and 0.0125g of nickel sulfate in 100g of water, stirring for 20min at a speed of 125rad / min, and standing for 12h to obtain oxidized starch;

[0187] S2, dissolving 100g of polyvinyl alcohol in 2kg of water, heating to 95°C, adding 3g of sodium hydroxide, adjusting the pH value to 11, and obtaining a cross-linking agent;

[0188] The oxidized starch and the cross-linking agent were mixed, and stirred at a temperature of 85° C. and a rotation speed of 90 rad / min for 30 minutes to prepare a cross-linked-gelatinized-oxidized starch adhesive;

[0189] S3, add 20g soy protein isolate, 8g urea, 5g sodium dodecyl sulfate to the cross-linked-gelatinized-oxidized starch adhesive, stir for 30min at a temperature of 80°C and a rotation speed of 90rad / min, cool to 60°C, add 15g silica sol, stir for 15min-20min, cool to room temperature, and obtain a starch oxidation / cross-linking dual modified adhesive for interior wall putty;

[0190] S4. Take 15 g of starch oxidation / cross-linking dual-modified adhesive for interior wall putty, 200 g of talcum powder with a particle size of 10 to 60 microns and 80 g of water and mix them evenly to obtain an interior wall putty paste.

[0191] Comparative Example 7

[0192] A method for preparing a conventional interior wall putty paste comprises the following steps:

[0193] S1, dissolving 60g of hydroxypropyl distarch phosphate, 8g of sodium hypochlorite and 0.0125g of nickel sulfate in 100g of water, stirring for 20min at a speed of 125rad / min, and standing for 12h to obtain oxidized starch;

[0194] S2, dissolving 100g of polyvinyl alcohol in 2kg of water, heating to 95°C, adding 3g of sodium hydroxide, adjusting the pH value to 11, and obtaining a cross-linking agent;

[0195] The oxidized starch and the cross-linking agent were mixed, and stirred at a temperature of 85° C. and a rotation speed of 90 rad / min for 30 minutes to prepare a cross-linked-gelatinized-oxidized starch adhesive;

[0196] S3, add 20g soy protein isolate, 8g urea, 5g sodium dodecyl sulfate to the cross-linked-gelatinized-oxidized starch adhesive, stir for 2h at a temperature of 60°C and a rotation speed of 90rad / min, cool to 60°C, add 15g silica sol, stir for 15min-20min, cool to room temperature, and obtain a starch oxidation / cross-linking dual modified adhesive for interior wall putty;

[0197] S4. Take 15 g of starch oxidation / cross-linking dual-modified adhesive for interior wall putty, 200 g of talcum powder with a particle size of 10 to 60 microns and 80 g of water and mix them evenly to obtain an interior wall putty paste.

[0198] Comparative Example 8

[0199] A method for preparing a conventional interior wall putty paste comprises the following steps:

[0200] S1, dissolving 60g of hydroxypropyl distarch phosphate, 8g of sodium hypochlorite and 0.0125g of nickel sulfate in 100g of water, stirring for 20min at a speed of 125rad / min, and standing for 6h to obtain oxidized starch;

[0201] S2, dissolving 100g of polyvinyl alcohol in 2kg of water, heating to 95°C, adding 3g of sodium hydroxide, adjusting the pH value to 11, and obtaining a cross-linking agent;

[0202] The oxidized starch and the cross-linking agent were mixed, and stirred at 85° C. and a rotation speed of 90 rad / min for 30 min to prepare a cross-linked-gelatinized-oxidized starch adhesive;

[0203] S3, add 20g soy protein isolate, 8g urea, 5g sodium dodecyl sulfate to the cross-linked-gelatinized-oxidized starch adhesive, stir for 2h at a temperature of 80°C and a rotation speed of 90rad / min, cool to 60°C, add 15g silica sol, stir for 15min-20min, and cool to room temperature to obtain a starch oxidation / cross-linking dual modified adhesive for interior wall putty;

[0204] S4. Take 15 g of starch oxidation / cross-linking dual-modified adhesive for interior wall putty, 200 g of talcum powder with a particle size of 10 to 60 microns and 80 g of water and mix them evenly to obtain an interior wall putty paste.

[0205] Detection and analysis

[0206] 1) The interior wall putty pastes prepared in Examples 5 to 8 and the conventional interior wall putty pastes prepared in Control Examples 1 to 8 were subjected to performance tests (the test method was performed in accordance with JG / T 298-2010 "Architectural Interior Putty"). The performance indicators of the obtained putties are shown in Table 1.

[0207] Table 1 Performance indicators of interior wall putty pastes prepared in Examples 5 to 8 and Comparative Examples 1 to 8

[0208]

[0209]

[0210]

[0211] Note: The row label in the table is: JG / T 298-2010 "Putty for Building Interior Use", and the listed indicators are the differential indicators that can be affected by changes in putty glue.

[0212] From the data analysis in Table 1 above, it can be seen that the putty paste for interior wall of the present invention obtained by using Examples 9 to 16 of the present invention has good properties, and the various difference indicators of putty performance have reached or exceeded the relevant technical indicators specified in the industry standard JG / T 298-2010 "Putty for Building Interiors". In comparative example 1, because the cross-linked-gelatinized-oxidized starch adhesive was not subjected to Schiff base reaction, the adhesive bonding strength was low, the coating surface curled and cracked during the scraping process, and the putty had slight powdering after film formation. In comparative example 2, because no cross-linking agent was introduced, the putty paste had poor construction and film-forming properties, the coating surface curled and pinholes during the scraping process, cracks, and serious powdering after the putty was formed. In comparative example 3, because the starch was not oxidized and pretreated, the starch and soy protein isolate did not react, the colloid was not fully polymerized, the low-temperature stability was poor, it was easy to deteriorate, and there was agglomeration. In control example 4, due to the excessive addition of soy protein isolate, the reaction was excessive, the crack resistance of the putty was poor in the initial stage of drying, there were cracks, and the putty film had powdering. In control example 5, due to the excessive amount of polyvinyl alcohol, the putty was too thick, there was agglomeration, and the surface drying time was long. In control example 6, due to the short reaction time of the Schiff base of the cross-linked-gelatinized-oxidized starch adhesive, the colloid polymerization effect was poor, and there were cracking and powdering. In control example 7, due to the low reaction temperature of the Schiff base of the cross-linked-gelatinized-oxidized starch adhesive, the colloid was not fully polymerized, and there were cracking and powdering. In control example 8, due to the short oxidation pretreatment time of the starch, the starch and the soy protein isolate did not react, the colloid was not fully polymerized, the low temperature stability was poor, it was easy to deteriorate, and there was agglomeration. This proves that in the preparation method of the starch oxidation / cross-linking dual-modified adhesive for interior wall putty of the present invention, starch pretreatment oxidation, gelatinization-cross-linking treatment of the pretreated oxidized starch, and Schiff base reaction of the gelatinized-cross-linked-oxidized starch are all important processes, and the ratio of polyvinyl alcohol and soy protein isolate, starch oxidation pretreatment time, colloidal Schiff base reaction time and temperature are all important parameters affecting the performance of putty glue.

[0213] 2) Infrared spectroscopy (FTIR) analysis

[0214] The specific steps are as follows:

[0215] S1. Pretreating starch to obtain oxidized starch, specifically comprising:

[0216] 70 g of hydroxypropyl distarch phosphate, 10 g of sodium hypochlorite and 0.0125 g of nickel sulfate were dissolved in 100 g of water, stirred at a speed of 125 rad / min for 20 min, and then allowed to stand for 12 h to prepare oxidized starch (OST);

[0217] S2, gelatinizing and cross-linking the oxidized starch to obtain a gelatinized-cross-linked-oxidized starch adhesive, specifically comprising:

[0218] 60 g of polyvinyl alcohol (PVA) was dissolved in 2 kg of water, heated to 95° C., 3 g of sodium hydroxide was added, and the pH value was adjusted to 11 to obtain a crosslinking agent;

[0219] The oxidized starch and the cross-linking agent were mixed and stirred at a temperature of 85°C and a rotation speed of 90 rad / min for 30 minutes to prepare a gelatinized-cross-linked-oxidized starch adhesive (OST-PVA);

[0220] S3, performing Schiff base reaction on the gelatinized-crosslinked-oxidized starch adhesive to obtain a double-modified adhesive, specifically comprising:

[0221] To the gelatinized-cross-linked-oxidized starch adhesive prepared in S2, add 20 g of soy protein isolate (SPI), 8 g of urea, and 5 g of sodium dodecyl sulfate, then stir for 2 h at a temperature of 80 ° C and a rotation speed of 90 rad / min, cool to 60 ° C, add 15 g of silica sol, stir for 15 min to 20 min, and cool to room temperature to obtain a starch oxidation / cross-linking dual-modified adhesive for interior wall putty (OST-PVA-SPI-U).

[0222] Fourier transform infrared (FTIR) spectroscopy (FTIR) analysis of all samples was performed on a Varian 1000 with a scanning range of 500–4000 cm -1 The measurement method is to spread the liquid sample evenly on the KBr sheet, and fully grind the dry solid sample and the solidified resin with the KBr solid for measurement.

[0223] The FTIR spectra of the above-mentioned oxidized starch (OST), polyvinyl alcohol (PVA), and gelatinized-crosslinked-oxidized starch adhesive (OST-PVA) are as follows: Figure 2 shown.

[0224] from Figure 2 The results show that in oxidized starch (OST) and gelatinized-cross-linked-oxidized starch adhesive (OST-PVA), 1660 and 1664 cm -1 The characteristic peak at 2886-2904cm belongs to the stretching vibration of C=O. -1 and 2935~2948cm -1 The characteristic peak of belongs to the stretching vibration of aldehyde protons. This proves that after starch is oxidized by NaClO, some of the secondary hydroxyl groups on C2 and C3 in its molecule are oxidized to aldehyde groups, and after cross-linking and gelatinization of oxidized starch using polyvinyl alcohol as a cross-linking agent, the gelatinization-cross-linking-oxidized starch adhesive has a peak at 1150cm -1 The stretching vibration of COC appeared at 1000-1250 cm -1The stretching vibration of CO and the range of 1010-1100cm -1 The stretching vibration peak intensity belonging to OH is significantly lower than that of oxidized starch and polyvinyl alcohol, which proves that after cross-linking and gelatinization, the hydroxyl content on the adhesive surface is reduced and the hydrophilicity of the colloid is greatly reduced, thereby effectively improving the water resistance of the adhesive.

[0225] The FTIR spectra of the above-mentioned soy protein isolate (SPI), gelatinized-crosslinked-oxidized starch adhesive (OST-PVA), and starch oxidation / crosslinked double modified adhesive for interior wall putty (OST-PVA-SPI-U) are as follows: Figure 3 shown.

[0226] from Figure 3 The analysis shows that in soy protein isolate (SPI), 3271 and 3061 cm -1 The characteristic peak at 1634cm belongs to the stretching vibration of NH -1 The characteristic peak belongs to the stretching vibration of C=O, 1226cm -1 The characteristic peaks belong to the stretching vibration of CN. In gelatinized-crosslinked-oxidized starch adhesive (OST-PVA), 1660 and 1664 cm -1 The characteristic peak at 2886-2904cm belongs to the stretching vibration of C=O. -1 and 2935~2948cm -1 The characteristic peaks belong to the stretching vibration of aldehyde protons. This indicates that there are free amino groups on the surface of soy protein isolate and free aldehyde groups on the surface of gelatinized-crosslinked-oxidized starch adhesive, which can provide reaction sites for Schiff base reaction. In the starch oxidation / crosslinking double modified adhesive for interior wall putty (OST-PVA-SPI-U), 1660cm -1 The characteristic peak at belongs to the stretching vibration of C=N, indicating that the Schiff base reaction is successful, thereby effectively improving the bonding strength of the adhesive.

[0227] In summary, the double modified adhesive of the present invention uses starch and polyvinyl alcohol as main raw materials, so that the prepared adhesive does not contain pollutants such as formaldehyde, and no toxic and harmful substances are added to the raw materials, thereby preventing the generation and release of toxic and harmful substances, effectively avoiding environmental pollution, and improving human health and safety. And through test detection, the double modified adhesive has the advantages of no agglomeration, uniform mixing, excellent low-temperature storage stability, strong workability, no cracks in the initial drying stage, easy grinding, good water resistance and bonding strength.

[0228] The preparation method of the double-modified adhesive of the present invention effectively improves the bonding strength and water resistance of the adhesive by oxidizing starch, gelatinizing and cross-linking, and introducing a primary amine compound to carry out a Schiff base reaction. Specifically, first, sodium hypochlorite is used as an oxidant. The glucosidic bond of hydroxypropyl distarch phosphate is broken under the action of sodium hypochlorite, and some of the secondary hydroxyl groups on C2 and C3 in its molecule are oxidized to aldehyde groups. At the same time, phosphoric acid also has an acidolysis effect on the starch molecules, and the partial cross-linking structure of hydroxypropyl distarch phosphate is conducive to the reaction. The oxidized starch contains aldehyde groups and carboxyl groups, and has good anti-corrosion and anti-mildew capabilities as well as cooking stability, dispersibility, cold flow and bonding properties. Secondly, polyvinyl alcohol is used as a cross-linking agent. Polyvinyl alcohol is a non-toxic, non-irritating, water-soluble, high-molecular polymer with excellent adhesion and biocompatibility. A large number of secondary hydroxyl groups and a small amount of acetoxy starch molecular chains in its molecular structure generate free radicals, which meet high-molecular monomers to form high-molecular chains, so that the prepared adhesive has the advantages of better adhesion, fluidity and anti-freezing properties. In addition, urea is used as an initiator and soy protein isolate is used as a reinforcing agent. During the oxidation process, the aldehyde groups formed in starch and urea, and the rich amino groups in the soy protein molecules undergo Schiff base reaction to form a tight network structure, thereby effectively improving the bonding strength of the adhesive. The preparation method has the advantages of simple process operation, mild reaction conditions, no by-products, rich raw material sources, biodegradable, no plastic pollution and low price, etc., which provides favorable guarantees for the industrial production of bio-based glue, has more industrial production value, and has potential application value in the field of composite polymer material technology.

[0229] The above embodiments are only preferred embodiments for fully illustrating the present invention, and the protection scope of the present invention is not limited thereto. Any equivalent substitution or change made by a person skilled in the art based on the present invention is within the protection scope of the present invention.

Claims

1. A double modified adhesive, characterized in that: The invention comprises the following raw materials: starch, a cross-linking agent, an oxidant, a catalyst, a gelatinizer, an initiator, a reinforcing agent, sodium dodecyl sulfate, silica sol and water.

2. The double modified adhesive according to claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 60 to 70 parts by weight of starch, 50 to 60 parts by weight of a cross-linking agent, 6 to 10 parts by weight of an oxidant, 0.01 to 0.02 parts by weight of a catalyst, 2 to 5 parts by weight of a gelatinizer, 6 to 10 parts by weight of an initiator, 15 to 25 parts by weight of a reinforcing agent, 2 to 6 parts by weight of sodium dodecyl sulfate, 10 to 20 parts by weight of silica sol and 1500 to 2500 parts by weight of water.

3. The double modified adhesive according to claim 2, characterized in that: The starch is selected from hydroxypropyl distarch phosphate; and / or, the cross-linking agent is selected from polyvinyl alcohol solution; And / or, the oxidant is selected from at least one of sodium hypochlorite, hydrogen peroxide, sodium periodate and potassium permanganate; And / or, the catalyst is selected from nickel sulfate; And / or, the pasting agent is selected from sodium hydroxide; And / or, the initiator is selected from urea; And / or, the enhancer is selected from soy protein isolate; And / or, the solid content of the silica sol is 20-30wt%; And / or, the pH value of the silica sol is 7-9; And / or, the available chlorine content in the sodium hypochlorite is 20%; And / or, the purity of the sodium hypochlorite is 99%.

4. A method for preparing a dual-modified adhesive according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1. pretreating starch to obtain oxidized starch; S2, gelatinizing and cross-linking the oxidized starch to obtain a gelatinized-cross-linked-oxidized starch adhesive; S3. Performing a Schiff base reaction on the gelatinized-crosslinked-oxidized starch adhesive to obtain a double-modified adhesive.

5. The preparation method according to claim 4, characterized in that: The S1 includes: Adding starch, an oxidant and a catalyst into water, stirring and standing to obtain a mixed starch solution containing oxidized starch; And / or, S2 includes: S21, adding a crosslinking agent into water, heating and dissolving, to obtain a crosslinking agent solution; S22, adding a gelatinizer to the cross-linking agent solution, adjusting the pH value to 9-11, and then adding oxidized starch, heating to perform gelatinization-cross-linking reaction, to obtain a gelatinization-cross-linking-oxidized starch adhesive.

6. The preparation method according to claim 5, characterized in that: The standing time is 10h~14h; And / or, the temperature of heating and dissolving is 95°C; And / or, the heating temperature of the gelatinization-crosslinking reaction is 80° C. to 90° C.; And / or, the gelatinization-crosslinking reaction time is 30 min to 40 min.

7. The preparation method according to claim 4, characterized in that: The S3 includes: S31, adding a reinforcing agent into water, and then adding sodium lauryl sulfate to obtain a first mixed material; S32, adding the mixed material to the gelatinized-crosslinked-oxidized starch adhesive, heating and stirring to react, to obtain a second mixed material; S33, cooling the second mixed material, adding silica sol, mixing and reacting, and obtaining a double-modified adhesive.

8. The preparation method according to claim 7, characterized in that: The temperature of the heating and stirring reaction is 80°C to 90°C; And / or, the heating and stirring reaction time is 2h~3h; and / or, cooling the second mixed material to 60° C.; And / or, the mixing reaction time is 15 min to 20 min.

9. An application of a double-modified adhesive prepared by the preparation method according to any one of claims 4 to 8, characterized in that: The double-modified adhesive is used as a starch adhesive for interior wall putty.

10. A putty paste for interior walls, characterized in that: The invention comprises a double-modified adhesive prepared by the preparation method according to any one of claims 4 to 8, talcum powder and water.

Citation Information

Patent Citations

  • Environmental-friendly amylopectin composite adhesive for paper products and production method thereof

    CN101760149A

  • Oxidized starch adhesive and preparation method thereof

    CN104861892A

  • Preparation method of phosphate esterification starch adhesive based formaldehyde-free building inner wall putty

    CN106833087A

  • Preparation method for cassava oxidized starch based adhesive

    CN107603513A

  • Preparation method of mildew-proof wallpaper adhesive and product thereof

    CN112480844A

Cited By

  • Low-temperature starch type impregnating compound as well as preparation method and application thereof

    CN119390363A

  • Flame-retardant environment-friendly interior wall putty and preparation method thereof

    CN119529586A