Preparation method of bimetallic ATP complex composite graphene fireproof coating
Through the preparation of bimetallic ATP complex composite graphene fire-retardant coating, the hydrothermal method of RGO@ACC nanocomposite flame retardant was used to solve the problems of organic solvent pollution and poor flame retardant performance of traditional coatings, achieving efficient The flame retardant effects of gas phase and condensed phase improve the strength and thermal insulation performance of the carbon layer.
Patent Information
- Application Number
- CN202410654384.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-24
- Publication Date
- 2024-11-22
AI Technical Summary
Traditional steel structure fire-retardant coatings have problems such as organic solvent pollution, toxic gas release and poor flame retardant performance, and the water-based fire-retardant coatings are not of uniform quality, and the fire-retardant performance and the structural strength of the expanded carbon layer are low.
The preparation method of bimetallic ATP complex composite graphene fire-retardant coating is prepared by the hydrothermal method of RGO@ACC nanocomposite flame retardant, combined with metal ions catalyzed to form carbon and ATP to promote the expansion and carbonization of the carbon layer, forming a gas phase and Coating phase flame retardant dual function coating.
It improves the flame retardant performance of the coating, extends the escape path of combustible gases, reduces the release of toxic gases, and enhances the flame retardant performance and thermal insulation effect of the carbon layer, which is in line with the development trend of green and environmental protection.
Smart Images

Figure CN118994998A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparation of graphene-based water-based ultra-thin epoxy intumescent fire-retardant coatings, and specifically relates to a method for preparing a bimetallic ATP complex composite graphene fire-retardant coating. Background Art
[0002] With the acceleration of economic construction and urbanization, super-high-rise and large-span steel structures have been vigorously developed. However, due to the good thermal conductivity of the steel substrate itself, when it encounters a flame, the surface temperature of the steel will quickly rise to more than 600°C, which will destroy the strength of the steel substrate and cause the rapid collapse of the steel structure, resulting in serious safety accidents and property losses. Fire-retardant coatings are important fire prevention measures for steel structures. The strength and quality of the residual carbon layer after the resin matrix is burned is the basis and key to the flame retardant performance of the coating. Traditional steel structure fire-retardant coatings are organic solvent-based products, and organic volatiles (VOCs, such as diacetone alcohol, The content of xylene, etc. is high, which will pollute the air and cause harm to the human body during the coating manufacturing and spraying process. If it is not handled properly, it will also pollute the soil or groundwater. At present, most flame retardants of intumescent steel structure fire retardant coatings adopt CNP system. The raw materials contain a large amount of film-forming agents, foaming agents and carbon-forming agents, which will decompose and release toxic gases such as CO, HCN, NOX during the heating process. Therefore, in the process of green and environmentally friendly sustainable development, water-based fire retardant coatings have made great progress. However, the quality of current water-based fire retardant coatings is uneven, and there are generally problems such as poor fire resistance, low expansion ratio and low structural strength of the expanded carbon layer.
[0003] With the continuous emergence of new nanomaterials and the mature development of nanotechnology, many researchers have used nanomaterials to enhance the flame retardant properties of water-based fire retardant coatings. Among the many nanomaterials, graphene (Gr) and its derivatives can change the pyrolysis behavior, thermal conductivity, heat absorption, viscosity and anti-dripping of polymers during combustion due to their high chemical stability, significant thermodynamic properties and excellent barrier properties. They can improve the thermal stability of polymers, delay the ignition point, inhibit flame propagation and reduce the heat release rate by suppressing heat. Summary of the invention
[0004] Adenosine triphosphate (ATP), as a nucleotide, is composed of phosphate groups, ribose and adenine. Its structure is rich in P (18.3%), N (13.8%) and C (23.7%) elements, which can provide N, O and P sites for the interaction of metal ions to form coordination compounds. Here, ATP contains structural components of acid source, carbon source and nitrogen-containing gas source at the same time. The phosphoric acid released by decomposition when heated can undergo esterification reaction with the carbon source hydroxyl group to generate viscous deposition products, which is beneficial to the carbon source replenishment in the high temperature stage. Moreover, the nitrogen-containing group is used as a gas source, and the nitrogen / ammonia generated by thermal decomposition is beneficial to further promote the catalysis of carbon deposition. In addition, transition metals can cause the polymer to be pyrolyzed and deposited in the condensed phase, and catalytically cracked into small molecules, further dehydrogenated (or dehydrated), aromatized, and then cross-linked into carbon, so as to inhibit the production of organic matter and catalyze its carbonization, promote the polymer to form amorphous carbon, and improve the quality and strength of the residual carbon layer.
[0005] To achieve the above purpose, the technical solution adopted by the present invention to solve its technical problem is.
[0006] A method for preparing a bimetallic ATP complex composite graphene fire retardant coating comprises the following steps.
[0007] 1. Preparation of RGO@ACC nanocomposite flame retardant.
[0008] First, 0.25 g of copper nitrate trihydrate (Cu(NO3)2·3H2O) and 0.15 g of cobalt nitrate hexahydrate (Co(NO3)2·6H2O) were weighed and dissolved in 10 mL of deionized water, recorded as solution A; 0.4 g of adenosine triphosphate (ATP) was dissolved in 30 mL of deionized water, recorded as solution B; secondly, the above solution A was slowly added dropwise to a three-necked flask containing 0.025 g of graphene oxide (GO) dispersion, and the GO mixed solution was stirred at room temperature for 60 min, and then the prepared solution B was added, and continued to stir at 80°C for 2 h; the obtained GO mixed slurry was transferred to a polytetrafluoroethylene autoclave, and a hydrothermal reaction was carried out at 120°C for 16 h; finally, the precipitate was repeatedly washed with deionized water to remove excess metal ions and ATP, and the RGO@ATP-Cu-Co (RGO@ACC) nanocomposite flame retardant sample was obtained by freeze drying. The specific preparation scheme is as follows: Figure 1 shown.
[0009] 2. Preparation of bimetallic ATP complex composite graphene fire retardant coating.
[0010] Firstly, polyphosphate (MPP), pentaerythritol (PER) and melamine (MEL) were weighed and dispersed in an appropriate amount of water and stirred to obtain a uniform expansion system mixture for standby use; secondly, water-based epoxy resin emulsion (EP) and curing agent were added to the expansion system mixture, and stirring was continued for 20 minutes to obtain an expandable epoxy resin mixture; then, RGO@ACC nanocomposite flame retardant was ultrasonically dispersed in 10 mL of deionized water, and the RGO@ACC suspension was added to the expandable epoxy resin mixture and stirred for 30 minutes to obtain a uniformly mixed RGO@ACC expandable epoxy resin slurry; finally, the RGO@ACC expandable epoxy resin slurry was brushed on the surface of a steel sheet with a sandblasting grade of Sa2, and after brushing, it was cured at room temperature for 7 days to obtain a bimetallic ATP complex composite graphene fire retardant coating.
[0011] Furthermore, in step 1, the molar ratio of cobalt nitrate hexahydrate to copper nitrate trihydrate is 1:1-1.5.
[0012] Furthermore, in step 1, the mass ratio of copper nitrate trihydrate to adenosine triphosphate is 1:1-2.
[0013] Furthermore, in step 1, the mass ratio of graphene oxide to copper nitrate trihydrate is 1:5-15.
[0014] Furthermore, the graphene oxide in step 1 can be hexagonal boron nitride, carbon nitride, or two-dimensional MXene.
[0015] Furthermore, in step 2, the mass ratio of epoxy resin to expansion system is 1:1-1.2.
[0016] Furthermore, in step 2, the mass ratio of epoxy resin to curing agent is 2:1-1.2.
[0017] Furthermore, in step 2, the curing agent can be ethylenediamine, diethylenetriamine, or triethylenetetramine.
[0018] Furthermore, in step 2, the ratio of polyphosphate, pentaerythritol and melamine is 5.5-6.5:2.5-3.5:1-1.5.
[0019] Furthermore, in step 2, the RGO@ACC nanocomposite flame retardant accounts for 1.5-3.0 wt.% of the total mass of the polyphosphate, pentaerythritol, melamine, waterborne epoxy resin emulsion, curing agent and RGO@ACC nanocomposite flame retardant.
[0020] The preparation method of a bimetallic ATP complex composite graphene fire-retardant coating provided by the present invention combines the excellent barrier properties of RGO, the metal ion catalytic carbonization effect and the coupling effect of ATP promoting the expansion and carbonization of the carbon layer, synthesizes a new expandable / highly catalytic RGO@ACC nano-composite flame retardant by a simple hydrothermal method, and applies the flame retardant to a fire-retardant coating system to obtain an RGO@ACC / EP nano-composite fire-retardant coating with dual functions of gas phase flame retardancy and condensed phase flame retardancy. The development of the coating is in line with the development trend of high-efficiency fire prevention, energy saving and consumption reduction, economic savings, non-toxic and low pollution, and ecological environmental protection, as well as the mainstream trend of the coating industry, and is of great significance in protecting objects and winning rescue time.
[0021] In addition, the preparation method of a bimetallic ATP complex composite graphene fire retardant coating provided by the present invention has the following beneficial effects.
[0022] (1) Compared with single metal catalysts, bimetallic elements have more active site types than single element compositions, which is beneficial to improving the catalytic activity, selectivity and synergistic effect of the reaction.
[0023] (2) Adenosine triphosphate (ATP) as an organic ligand contains high content of N and P elements, which can provide acid and gas sources, promote the expansion and carbonization of the carbon layer, and enhance the flame retardant properties of the carbon layer.
[0024] (3) Reduced graphene oxide (RGO) as a two-dimensional nanosheet material has excellent physical barrier properties, which can extend the escape path of combustible gases and improve flame retardant properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 Schematic diagram of the preparation process of RGO@ACC nanocomposite flame retardant.
[0026] Figure 2 FT-IR images of GO, RGO, ATP-Cu / Co and RGO@ACC.
[0027] Figure 3 XRD spectra of GO, RGO, ATP-Cu / Co and RGO@ACC.
[0028] Figure 4 This is the XPS spectrum of RGO@ACC nanocomposite flame retardant.
[0029] Figure 5 For (a,b)EP, (c,d)RGO / EP, (e,f)ATP-Cu / Co / EP, (g,h)RGO@ACC 1.5% / EP、(i,j)RGO@ACC 2.0% / EP、(k,l)RGO@ACC 2.5% / Digital photos before and after EP burning test.
[0030] Figure 6 This is a curve diagram of the temperature change on the back of the steel sheet and the coating sample.
[0031] Figure 7 are the expansion height and expansion rate of different samples.
[0032] Figure 8 (a) Absorbance curve and (b) smoke density ratio of different samples.
[0033] Fig. 9 XRD spectra of the carbon layer after combustion of different coatings.
[0034] Fig.10 SEM morphology and EDS spectra of the remaining carbon layer after combustion test of different samples, including (a) EP, (b) RGO / EP, (c) ATP-Cu / Co / EP, (d) RGO@ACC 1.5% / EP、(e,g)RGO@ACC 2.0% / EP、(f)RGO@ACC 2.5% SEM images of carbon layer of / EP and (hl)RGO@ACC 2.0% / EP’s EDS-Mapping photos. DETAILED DESCRIPTION
[0035] Example 1.
[0036] A method for preparing a bimetallic ATP complex composite graphene fire retardant coating comprises the following steps.
[0037] 1. Preparation of RGO@ACC nanocomposite flame retardant.
[0038] Firstly, 0.25g of copper nitrate trihydrate (Cu(NO3)2·3H2O) and 0.15g of cobalt nitrate hexahydrate (Co(NO3)2·6H2O) were weighed and dissolved in 10mL of deionized water, recorded as solution A; 0.4g of adenosine triphosphate (ATP) was dissolved in 30mL of deionized water, recorded as solution B; secondly, the above solution A was slowly added dropwise into a three-necked flask containing 0.025g of graphene oxide (GO) dispersion, and the GO mixed solution was stirred at room temperature for 60min, and then the prepared solution B was added, and the stirring was continued at 80℃ for 2h; the obtained GO mixed slurry was transferred to a polytetrafluoroethylene autoclave, and a hydrothermal reaction was carried out at 120℃ for 16h; finally, the precipitate was repeatedly washed with deionized water to remove excess metal ions and ATP, and the RGO@ATP-Cu-Co (RGO@ACC) nanocomposite flame retardant sample was obtained by freeze drying.
[0039] 2. Preparation of bimetallic ATP complex composite graphene fire retardant coating.
[0040] Firstly, polyphosphate (MPP), pentaerythritol (PER) and melamine (MEL) were weighed and dispersed in an appropriate amount of water and stirred to obtain a uniform expansion system mixture for standby use; secondly, water-based epoxy resin emulsion (EP) and curing agent were added to the expansion system mixture, and stirring was continued for 20 minutes to obtain an expandable epoxy resin mixture; then, RGO@ACC nanocomposite flame retardant was ultrasonically dispersed in 10 mL of deionized water, and the RGO@ACC suspension was added to the expandable epoxy resin mixture and stirred for 30 minutes to obtain a uniformly mixed RGO@ACC expandable epoxy resin slurry; finally, the RGO@ACC expandable epoxy resin slurry was brushed on the surface of a steel sheet with a sandblasting grade of Sa2, and after brushing, it was cured at room temperature for 7 days to obtain a bimetallic ATP complex composite graphene fire retardant coating.
[0041] Table 1 Basic components of different intumescent fire retardant coatings
[0042]
[0043] Experimental example 1.
[0044] This experimental example demonstrates the relevant experimental analysis results of a method for preparing a bimetallic ATP complex composite graphene fire retardant coating.
[0045] 2.5wt.% of RGO, ATP-Cu / Co and 1.5wt.%, 2.0wt.%, and 2.5wt.% of RGO@ACC hybrids were uniformly mixed with the matrix coating system to prepare RGO / EP, ATP-Cu / Co / EP, RGO@ACC / EP (1.5wt.%), RGO@ACC / EP (2.0wt.%), and RGO@ACC / EP (2.5wt.%) coatings, respectively; then, the uniformly dispersed coating system was brushed on the surface of a steel sheet with a pretreatment grade of Sa2, and after brushing, it was cured at room temperature for 7 days to obtain a sample coating; in addition, the experiment used pure EP coating as a control.
[0046] (1) FT-IR spectra of pure GO, RGO, ATP-Cu / Co and RGO@ACC Figure 2 As shown; it can be seen that pure GO has a peak at 1731 cm -1 , 1633cm -1 , 1394cm -1 , 1106cm -1 , 1076cm -1 , 554cm -1There are obvious absorption peaks at 3500cm -1 A large absorption wave appears near 1731 cm, indicating that the GO surface contains a large number of -OH functional groups. For the RGO hybrid, the hydroxyl characteristic peak of pure GO is significantly weakened, accompanied by a -1 The C=O absorption peak disappears, indicating that GO is successfully reduced to RGO during the preparation process. For the ATP-Cu / Co sample, the C=O absorption peak at 3000-3500cm -1 In the range, a broad and large absorption peak can be observed, which is attributed to the stretching vibration of -OH; 1633cm -1 The peaks near 1402 cm are attributed to C=C aromatic stretching. -1 The peaks nearby are due to the vibration of the CN stretching peak, (PO4) 3- The absorption peak of the bond is also at 618 cm -1 and 479cm -1 Observed at 1195cm -1 and 1073cm -1 There are two obvious peaks at the center, corresponding to the P=O / POC and PO stretching vibrations of the functional phosphate groups in the ATP structure. For the RGO@ACC composite, the characteristic peaks of RGO and ATP-Cu / Co can be observed simultaneously, which preliminarily proves that RGO and ATP-Cu / Co are successfully combined.
[0047] (2) The crystal structures of pure GO, RGO, ATP-Cu / Co and RGO@ACC composites were tested by XRD. Figure 3 As shown in the figure, pure GO has a characteristic diffraction peak at 2θ=10.7°, which corresponds to the (001) plane of GO. For the RGO sample, two characteristic diffraction peaks at 2θ=26.2° and 43.4° can be clearly observed, which belong to the (002) and (100) crystal planes of RGO, respectively. The characteristic peak belonging to the GO (001) plane is significantly weakened, indicating that GO can be successfully reduced to RGO at high temperature by hydrothermal method. According to the Bragg equation, the interlayer spacing of RGO nanosheets is approximately equal to 0. .339nm; for ATP-Cu / Co, the sharp peak at 2θ=26.8° belongs to the characteristic diffraction of ATP-Cu / Co; for the RGO@ACC composite, all the characteristic diffraction peaks of ATP-Cu / Co and RGO can be detected; and the diffraction peak of the (002) crystal plane of RGO decreases from 26.2° to 25.9°, and the interlayer spacing of RGO increases from 0.339nm to 0.344nm; this directly proves that the ATP-Cu / Co nanosheets are successfully inserted into the RGO layer.
[0048] (3) The chemical bonding state and type of the ATP-Cu / Co complex were tested by XPS, such as Figure 4 shown; from Figure 4 As can be seen in (a), the high-resolution spectrum of C 1s can be decomposed into five peaks at 284.7, 285.4, 286.2, 287.1 and 288.4 electron volts, which are derived from CC, CN, CO, C=O and 0-C=O respectively; for the high-resolution spectrum of N1s ( Figure 4 (b)), the four peaks at 398.6, 399.5 and 400.2 eV correspond to NC, N=C / N=N and N(C)3 respectively; in the O1s high-resolution spectrum ( Figure 4 (c)), the peaks at 530.3, 531.4 and 532.6 eV are derived from O-Cu / O-Co, PO and P=O / CO; in Figure (4(d)), the Cu 2p high-resolution spectrum has two peaks at 932.7 and 952.7 eV, corresponding to Cu2P3 / 2 and Cu2P1 / 2, respectively; Figure 4 In (f), the high-resolution spectrum of Co 2P has four peaks at 781.6, 785.3, 797.6, and 803.2 electron volts, corresponding to Cu2P3 / 2 (Co 2+ ), cobalt salts and Cu2P1 / 2(Co 2+ ); P2P spectrum( Figure 4 (e)) can be decomposed into three peaks at 132.6, 133.9, and 134.8 eV, corresponding to PO 3- , POP / PO and P=O bonds.
[0049] (4) The surface morphology of the coating before and after the large plate combustion test is as follows Figure 5 shown; from Figure 5 From a, c, e, g, i, and k in the figure, it can be seen that all coatings have no cracks or holes on the surface before combustion, and are relatively smooth, which proves that the basic formula of the coating is reasonable; after the combustion of pure EP ( Figure 5 (b)), a large number of holes and cracks appeared on the surface of the carbon layer, and the residual carbon layer was almost completely separated from the matrix, indicating that the residual carbon formed was weak in strength, indicating that its protection effect was poor; for RGO / EP sample ( Figure 5 (d)), due to the superior mechanical strength and barrier properties of RGO nanosheets, only relatively small holes appeared on the surface of the carbon layer; as for the ATP-Cu / Co / EP sample ( Figure 5(f)), some cracks still exist on the surface of the carbon layer, while the huge and dense holes disappear, indicating that the introduction of ATP-Cu / Co can significantly improve the strength of the residual carbon, which is mainly attributed to the catalytic carbonization of Cu and Co during the thermal decomposition of the epoxy resin matrix and the flame retardant properties of the high content of N and P in the ATP ligand; Figure 5 As can be seen in h, j, and l, the carbon layer of the coatings with different amounts of RGO@ACC hybrids after combustion shows different characteristics; for RGO@ACC / EP (1.5wt.%) hybrid ( Figure 5 (h)), some cracks and micropores can still be observed on the surface of the carbon layer, which may be related to the low amount of filler added; Figure 5 As can be seen in (j), the RGO@ACC / EP (2.0wt.%) composite coating exhibits a relatively complete and dense carbon layer without holes and cracks, which is beneficial to improve its barrier effect against flames and heat; in addition, according to Figure 5 (l) It can be seen that obvious holes and narrow cracks appeared on the surface of the carbon layer of the RGO@ACC / EP (2.5wt.%) composite coating, which is mainly attributed to the fact that too much filler cannot be effectively and evenly dispersed in the resin matrix.
[0050] (5) Figure 6 The changes in the temperature of the back side of the steel plate during the combustion of the coated samples were recorded; it can be seen that the temperature of the back side of the uncoated bare steel plate rose sharply within 10 minutes, which would seriously reduce the strength of the substrate itself; the heating rate of the back side of the coated sample was significantly lower, indicating that this method of applying organic coatings is effective in extending the failure time of steel; for pure EP, the back side temperature still showed a rapid rising trend at the beginning of combustion, because the expansion components did not completely react to form insulating residual carbon, and therefore did not effectively prevent heat conduction; thereafter, the temperature gradually stabilized after 10 minutes of combustion, and finally stabilized at 268.4°C after 60 minutes of combustion; in the case of the addition of RGO / EP, the final temperature after 60 minutes of combustion remained at 224.5°C, which is a temperature of The further reduction is mainly due to the excellent barrier properties of RGO; for the ATP-Cu / Co / EP sample, the back temperature finally balances at 207.2℃, which is significantly lower than the temperature of the pure resin sample. This can be attributed to the release of water, nitrogen and ammonia during the combustion of ATP-Cu / Co, which reduces the surface temperature and the concentration of combustible gases, as well as the barrier effect of its flaky structure to external heat; in contrast, due to the synergistic effect of ATP-Cu / Co and RGO, the back temperature of the RGO@ACC composite coating after combustion is lower than that of other composite coatings; among them, the coating of the RGO@ACC (2.0wt.%) hybrid shows the lowest back temperature (164.6℃) after 60 minutes of combustion, indicating that it has the best thermal insulation performance.
[0051] (6) The expansion height and expansion rate of different samples after furnace storage test are as follows Figure 7 As shown; it can be seen that the expansion height and expansion rate of pure EP are only 8.1mm and 6.32, which determines that its barrier effect on heat and flame is very limited; after adding RGO nanosheets, the swelling height and swelling rate of the composite coating increase to 13.3mm and 10.15, which may be mainly related to the increase in the strength of the carbon layer caused by the flexibility of RGO; after adding ATP-Cu / Co / EP nanosheets, the swelling height and swelling rate of the composite coating increase to 15.2mm and 11.78, respectively, which may be related to the thermal decomposition of ATP to produce gases N2 and NH3; for RGO@ACC / EP (1.5wt.%), its The expansion height and expansion rate further increased to 17.3 mm and 13.62, respectively, which was mainly attributed to the release of N2 and NH3 and the barrier property of RGO, which further prolonged the gas escape path, thereby improving its expansion performance; in addition, for the RGO@ACC / EP (2.0wt.%) coating, the expansion height and expansion rate values at this time reached the maximum value (the expansion height was 25.4 mm and the expansion rate was 19.69); for the RGO@ACC / EP (2.5wt.%) coating, the expansion height and expansion rate decreased to 20.1 mm and 15.46, indicating that the excessive nano-additives were not conducive to the expansion process of the coating at high temperature.
[0052] (7) Light absorption rate and smoke density level during the combustion of composite coatings Figure 8 shown; from Figure 8 (a) It can be seen that, compared with other samples, pure EP always maintains the highest light absorption rate during the combustion process, indicating that it releases the largest amount of smoke during the combustion process; after adding RGO, the light absorption rate of the composite coating is reduced, indicating that the excellent barrier performance of RGO can effectively suppress the effect of smoke; after adding ATP-Cu / Co and RGO / ACC, the light absorption rate of the composite coating is further reduced, which is mainly attributed to the combined effect of the barrier property of RGO nanosheets, the bimetallic catalytic carbonization performance and the self-expansion of ATR, which increases the quality and strength of the carbon layer; among them, the composite coating with 2.0% RGO / ACC added maintains the lowest light absorption rate. When the content of RGO / ACC hybrid increases to 2.5%, the light absorption rate increases instead, indicating that too much addition will increase its dispersion difficulty in the resin matrix, thereby weakening the smoke suppression performance of the coating; Figure 8(b) shows the smoke density levels of different composite coatings. The smoke density levels of pure EP, RGO / EP, ATP-Cu / Co / EP, RGO@ACC / EP (1.5wt.%), RGO@ACC / EP (2.0wt.%) and RGO@ACC / EP (2.5wt.%) are 68.2%, 57.8%, 54.3%, 45.9%, 37.8% and 42.2%, respectively. Among them, the reduction of the smoke density level of RGO / ACC / EP is mainly due to the good dispersing effect of ATP on GO, which ensures the uniform dispersion of GO in the resin matrix, thereby hindering the outward diffusion of smoke. The lowest smoke density level of RGO@ACC / EP (1.5wt.%) is not only the effect of GO nanosheets, but more importantly, the effect of ATP and Cu 2+ / Co 2+ It can promote the conversion of more organic cracking products into coke, thereby reducing the amount of smoke generated; in comparison, the smoke density level of the RGO@ACC / EP (2.0wt.%) composite coating is the lowest (37.8%), indicating that it has the strongest smoke suppression effect.
[0053] (8) The crystal structure of the residual carbon was analyzed by XRD, such as Fig. 9 As shown in the figure, only the diffraction peak of amorphous carbon can be detected at 2θ=24.9° for the carbon layer after combustion of pure EP and RGO / EP; some new changes have occurred in the residual carbon of the RGO / ACC / EP composite coating, and characteristic diffraction peaks belonging to CuO (111), (202) and (220) crystal planes appear at 2θ=35.1°, 38.4°, 48.3°, 57.6°, 60.7° and 67.3°; while the peaks at 2θ=31.8°, 36.4° and 65.3° correspond to Co3 O4's (220), (311) and (440) crystal planes, while the diffraction peak at 2θ=25.6° is related to the characteristic diffraction peak of cobalt phosphate; the samples filled with RGO / ACC / EP compounds show similar diffraction peaks because the coating composition is not much different; in the combustion of the coating containing RGO / ACC / EP, ATP reacts with the expansion component to generate a small amount of cobalt phosphate, and the Co3O4 and CuO generated by the thermal decomposition of ATP-Cu-Co remain in the carbon layer, which is beneficial to blocking the penetration of external heat.
[0054] (9) SEM and EDS analysis were performed on the carbon layers of different samples after combustion, such as Fig.10 as shown; Fig.10 As shown in (a), the surface of the carbon layer of pure EP presents large cavities and cracks, which cannot block the heat outside, resulting in poor thermal insulation performance; after adding RGO nanosheets ( Fig.10(b)), the holes on the carbon layer surface become smaller, but obvious cracks can still be found, providing a path for thermal intrusion; for ATP-Cu / Co composite coating ( Fig.10 (c)), the cracks on the surface of the char layer after combustion are significantly reduced, indicating that its barrier effect on heat and flame is enhanced; Fig.10 (d, e, f) It can be seen that RGO@ACC / EP (2.0wt.%) has the best effect. There are no obvious cracks on the surface of the carbon layer, but it is covered by some small, uniformly sized, independent holes. These structures are very effective for heat insulation. The surface of the carbon layer is further improved, and the number and size of cracks are reduced. For RGO@ACC / EP (2.5wt.%), more obvious holes appear on the surface, and its heat insulation effect becomes worse. Fig.10 (hl) It can be seen that C, N, P, Cu, and Co are uniformly distributed in the carbon layer, indicating that the retained GO nanosheets and the formed Cu and Co oxides are uniformly dispersed throughout the residual carbon, thus contributing to its strength and thermal insulation properties.
Claims
1. A method for preparing a bimetallic ATP complex composite graphene fire retardant coating, comprising the following steps: (1) Preparation of RGO@ACC nanocomposite flame retardant First, 0.25 g of copper nitrate trihydrate (Cu(NO3)2·3H2O) and 0.15 g of cobalt nitrate hexahydrate (Co(NO3)2·6H2O) were weighed and dissolved in 10 mL of deionized water, recorded as solution A; 0.4 g of adenosine triphosphate (ATP) was dissolved in 30 mL of deionized water, recorded as solution B; secondly, the above solution A was slowly added dropwise to a three-necked flask containing 0.025 g of graphene oxide (GO) dispersion, and the GO mixed solution was stirred at room temperature for 60 min, and then the prepared solution B was added, and the stirring was continued at 80°C for 2 h; the obtained GO mixed slurry was transferred to a polytetrafluoroethylene autoclave, and a hydrothermal reaction was carried out at 120°C for 16 h; finally, the precipitate was repeatedly washed with deionized water to remove excess metal ions and ATP, and the RGO@ATP-Cu-Co (RGO@ACC) nanocomposite flame retardant sample was obtained by freeze drying; (2) Preparation of bimetallic ATP complex composite graphene fire retardant coating First, weigh polyphosphate (MPP), pentaerythritol (PER), and melamine (MEL), disperse them in an appropriate amount of water and stir to obtain a uniform expansion system mixture for standby use; secondly, add water-based epoxy resin emulsion (EP) and curing agent to the expansion system mixture, continue stirring for 20 minutes, and obtain an expandable epoxy resin mixture; then, ultrasonically disperse the RGO@ACC nanocomposite flame retardant in 10mL deionized water, and add the RGO@ACC suspension to the expandable epoxy resin mixture and continue stirring for 30 minutes to obtain a uniformly mixed RGO@ACC expandable epoxy resin slurry; finally, brush the RGO@ACC expandable epoxy resin slurry on the surface of a steel sheet with a sandblasting grade of Sa2, and after brushing, cure it at room temperature for 7 days to obtain a bimetallic ATP complex composite graphene fire retardant coating; In step (1), the molar ratio of cobalt nitrate hexahydrate to copper nitrate trihydrate is 1:1-1.5; the mass ratio of copper nitrate trihydrate to adenosine triphosphate is 1:1-2; the mass ratio of graphene oxide to copper nitrate trihydrate is 1:5-15; graphene oxide can be replaced by hexagonal boron nitride, carbon nitride, and two-dimensional MXene; in step (2), the RGO@ACC nanocomposite flame retardant accounts for 1.5-3.0wt.% of the total mass of polyphosphate, pentaerythritol, melamine, water-based epoxy resin emulsion, curing agent and RGO@ACC nanocomposite flame retardant.
2. A bimetallic ATP complex composite graphene fire retardant coating prepared by the method as claimed in claim 1.
Citation Information
Patent Citations
Preparation method of BN / PAP-coated Cu-MOF-based epoxy flame-retardant material
CN116376223A
Preparation method of organic solid acid modified boron nitride water-based expansion fireproof coating
CN116554757A
Preparation method of PAP activated carbon sphere-based waterborne epoxy intumescent fireproof coating
CN116814136A
Modified graphene flame-retardant floor paint and preparation method thereof
CN117844346A