Emulsion type self-crosslinking bio-based itaconate pressure-sensitive adhesive and preparation method thereof
By using bio-itaconic acid ester and functional monomers in the pressure-sensitive adhesive for esterification, a high bio-based content emulsion self-crosslinked pressure-sensitive adhesive was prepared, which solved the problem of acrylate pressure-sensitive adhesive for petrochemical resources. Dependence and environmental pollution problems have achieved high bonding performance and low carbon emissions.
Patent Information
- Application Number
- CN202410565659.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-17
- Filing Date
- 2024-05-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-05-09
AI Technical Summary
The existing acrylate-based pressure-sensitive adhesives are highly dependent on non-renewable petrochemical resources, resulting in environmental pollution and carbon emission problems, and their preparation process has volatile organic emissions and high costs.
Using semi-continuous emulsion polymerization process, bio-itaconic acid ester monomer is used to replace acrylate monomers, combining functional monomers and self-crosslinked monomers, and emulsion-type self-crosslinked bio-itaconic ester pressure is prepared through esterification reaction. Sensitive adhesives improve their bio-based content and adhesive properties.
It significantly improves the 180° peel strength and viscosity of bio-based pressure-sensitive adhesive, reduces the use of petroleum-based monomers, reduces carbon emissions and environmental pollution, and has a simple process and low cost, which is suitable for sustainable development.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of pressure-sensitive adhesives, and in particular to an emulsion-type self-crosslinking bio-based itaconate pressure-sensitive adhesive and a preparation method thereof. Background Art
[0002] Pressure sensitive adhesive (PSA for short) is a pressure-responsive adhesive that can quickly bond to smooth surfaces under low pressure to generate bonding force.
[0003] Acrylate-based pressure-sensitive adhesive is the most widely used pressure-sensitive adhesive with the largest output. However, the preparation of acrylate-based pressure-sensitive adhesive is highly dependent on non-renewable petrochemical resources. It is of great significance to use renewable bio-based monomers to partially replace non-renewable petroleum-based monomers to prepare pressure-sensitive adhesive.
[0004] Acrylic pressure-sensitive adhesives are divided into emulsion type and solvent type. Emulsion type acrylic pressure-sensitive adhesives use emulsion polymerization technology to avoid the use of a large amount of solvents, thereby reducing the emission of volatile organic compounds (VOCs), and have more environmental advantages. At the same time, emulsion type pressure-sensitive adhesives have higher molecular weight, simple process and low cost. The market share of emulsion type acrylic pressure-sensitive adhesives has increased year by year, and has broad development prospects.
[0005] Therefore, there is an urgent need for an emulsion-type acrylic pressure-sensitive adhesive that can partially replace non-renewable petroleum-based monomers. Summary of the invention
[0006] In order to solve the problems existing in the prior art, alleviate the dependence of pressure-sensitive adhesives on non-renewable petroleum resources, reduce the pollution of VOC to the environment during the production process and reduce carbon emissions, the present invention provides an emulsion-type self-crosslinking bio-based itaconate pressure-sensitive adhesive and a preparation method thereof. Itaconate can be synthesized by esterification reaction of itaconate obtained by biological fermentation and bio-alcohol. The present invention adopts a semi-continuous emulsion polymerization process to partially replace acrylate monomers with itaconate monomers to prepare bio-based pressure-sensitive adhesives, which provides a solution for the sustainable development of the industry. The present invention partially replaces acrylate-based monomers derived from non-renewable petrochemical resources with renewable monomers, and the prepared pressure-sensitive adhesive has a higher bio-based content, higher 180° peel strength and sustained adhesion, simple process, excellent comprehensive bonding performance, and good application prospects.
[0007] One of the purposes of the present invention is to provide an emulsion-type self-crosslinking bio-based itaconate pressure-sensitive adhesive, which is prepared from raw materials including the following components: water, itaconate monomers, acrylate monomers, functional monomers, self-crosslinking monomers, initiators, pH buffers and emulsifiers.
[0008] In a preferred embodiment of the present invention,
[0009] Each component is calculated based on 100 parts by weight of water.
[0010]
[0011] In a preferred embodiment of the present invention,
[0012] The itaconate monomer is one or more of dimethyl itaconate, diethyl itaconate, dibutyl itaconate, diisooctyl itaconate, preferably dibutyl itaconate; and / or,
[0013] The acrylic acid ester monomer is one or more of butyl acrylate, n-octyl acrylate, isooctyl acrylate, ethyl acrylate, methyl acrylate, methyl methacrylate, isooctyl methacrylate, isobornyl acrylate, and isobornyl methacrylate, preferably butyl acrylate and / or isooctyl acrylate; and / or,
[0014] The functional monomer is a copolymerizable monomer containing a carboxylic acid group, preferably one or more of acrylic acid, methacrylic acid, itaconic acid, monomethyl itaconate, and monobutyl itaconate, preferably acrylic acid and / or methacrylic acid; the functional monomer can undergo a cross-linking reaction in the colloidal particles to form a three-dimensional network structure, thereby enhancing the mechanical properties and stability of the pressure-sensitive adhesive, and can also adjust the adhesion properties of the pressure-sensitive adhesive, and can also enhance the solvent resistance of the pressure-sensitive adhesive, so that it is not easy to soften or dissolve when it comes into contact with a solvent, thereby improving the stability and durability of the pressure-sensitive adhesive; specific functional monomers can also enhance the antioxidant properties of the pressure-sensitive adhesive, extend its life during storage and use, and reduce the performance degradation caused by oxidation; in addition, the introduction of functional monomers can also adjust the rheological properties of the pressure-sensitive adhesive, including viscosity, fluidity, and deformation behavior, so as to adapt to different application requirements; and / or,
[0015] The self-crosslinking monomer is one or both of glycidyl methacrylate and glycidyl acrylate; and / or,
[0016] The initiator is a water-soluble thermal initiator, preferably potassium persulfate and / or ammonium persulfate, more preferably ammonium persulfate; and / or,
[0017] The pH buffer is sodium bicarbonate and / or disodium hydrogen phosphate, preferably sodium bicarbonate; and / or,
[0018] The emulsifier is one or more of anionic emulsifiers and nonionic emulsifiers, preferably one or more of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, 1-allyloxy-3-(4-nonylphenol)-2-propanol polyoxyethylene (10) ether ammonium sulfate, and polyoxyethylene octylphenol ether-10, more preferably sodium dodecylbenzene sulfonate and 1-allyloxy-3-(4-nonylphenol)-2-propanol polyoxyethylene (10) ether ammonium sulfate, and more preferably, the ratio of the two is 1:2.
[0019] In a preferred embodiment of the present invention,
[0020] The raw materials for preparing the emulsion type self-crosslinking bio-based itaconate pressure-sensitive adhesive also include a molecular weight regulator; preferably,
[0021] The molecular weight regulator is one or both of n-dodecyl mercaptan and tert-dodecyl mercaptan; and / or,
[0022] Based on 100 parts by weight of water, the amount of the molecular weight regulator is 0-0.15 parts by weight; preferably 0-0.03 parts by weight; more preferably 0.001-0.03 parts by weight.
[0023] The second object of the present invention is to provide a method for preparing the emulsion type self-crosslinking bio-based itaconate pressure-sensitive adhesive of one of the objects of the present invention, comprising semi-continuous emulsion polymerization of components including water, itaconate monomers, acrylate monomers, functional monomers, self-crosslinking monomers, initiators, pH buffers, emulsifiers and optional molecular weight regulators to obtain the emulsion type self-crosslinking bio-based itaconate pressure-sensitive adhesive.
[0024] In a preferred embodiment of the present invention,
[0025] The method comprises:
[0026] (a) using water as a solvent, mixing itaconate monomers, acrylate monomers, functional monomers, self-crosslinking monomers, a pH buffer, an optional molecular weight regulator and 60-95% of an emulsifier to obtain a pre-emulsion;
[0027] (b) reacting 3-20% of the pre-emulsion obtained in step (a), water, 1-80% of the initiator and the remaining emulsifier until the emulsion turns blue;
[0028] (c) adding the remaining pre-emulsion and the initiator to the reaction system of step (b) at a uniform rate, raising the temperature for reaction, and adding a weak base to adjust the pH to a weak alkaline state after the reaction, thereby obtaining the emulsion-type self-crosslinking bio-based itaconate pressure-sensitive adhesive.
[0029] In a preferred embodiment of the present invention,
[0030] The mass ratio of the amount of water used in step (a) to the total amount of water used in step (b) is in the range of 1:(0.1-10).
[0031] In a preferred embodiment of the present invention,
[0032] In step (b),
[0033] The reaction temperature is 70-80°C, preferably 75-80°C.
[0034] In a preferred embodiment of the present invention,
[0035] In step (c),
[0036] The reaction temperature is 85-90°C, preferably 85-88°C, and the reaction time is 30-120 min, preferably 50-100 min; and / or,
[0037] The weak base comprises aqueous ammonia; and / or,
[0038] The weak alkalinity refers to a pH of 7-9, preferably 7-8.
[0039] In a preferred embodiment of the present invention,
[0040] Step (c) also includes the step of filtering the emulsion after adjusting the pH to weak alkalinity.
[0041] The present invention can adopt the following specific technical solutions:
[0042] The method for preparing the bio-based pressure-sensitive adhesive of the present invention comprises the following steps:
[0043] (a) using water as solvent, mixing itaconate monomer, acrylate monomer, functional monomer, self-crosslinking monomer, 50-100% of pH buffer, optional molecular weight regulator and 60-95% of emulsifier to prepare pre-emulsion; wherein the stirring rate is 200-500 r / min, and the stirring time is 30-60 min;
[0044] (b) reacting 3-20% of the pre-emulsion obtained in step (a), water, 1-80% of the initiator, the remaining pH buffer and the remaining emulsifier at 70-80° C. until the emulsion turns blue; wherein the stirring rate is 150-300 r / min;
[0045] (c) uniformly adding the remaining pre-emulsion and initiator to the reaction system of step (b) at a certain time; wherein the stirring rate is 150-300 r / min and the dropping time is 2h-4h; after the dropping is completed, the stirring rate is maintained to increase the reaction temperature to 85-90°C and react for 30-120min, then the reaction is shut down and cooled, and a weak base is added to adjust the pH value to between 7-9; the emulsion is filtered to obtain the emulsion-type self-crosslinking bio-based itaconate pressure-sensitive adhesive.
[0046] Compared with the prior art, the present invention has the following beneficial effects:
[0047] The increase in the content of bio-based itaconate (preferably dibutyl itaconate) increases the loss modulus of the pressure-sensitive adhesive at a shear frequency of 50Hz, reduces the storage modulus at a shear frequency of 0.1Hz, and increases the energy loss in the peeling process under 1% strain conditions, thereby increasing the 180° peel strength; on the other hand, the molecular weight and gel content of the pressure-sensitive adhesive will decrease after the copolymerization of the acrylate monomer with the itaconate monomer, which will significantly reduce its holding force. Therefore, the present invention introduces a self-crosslinking monomer to increase its crosslinking degree, and at the same time explores the appropriate range of the amount of the self-crosslinking monomer, so as to ensure a high initial adhesion and 180° peel strength while significantly improving the holding force. In the present invention, a proper amount of carboxyl groups and epoxy groups undergo crosslinking reactions to effectively increase the crosslinking density of the pressure-sensitive adhesive, thereby improving the holding force.
[0048] The present invention preferably uses 30-50wt% (accounting for the total weight of monomers) of bio-based itaconate monomers to reduce the use of petroleum-based acrylate monomers, which can reduce the dependence of the pressure-sensitive adhesive preparation industry on petrochemical resources and reduce carbon emissions. Compared with the solvent-based pressure-sensitive adhesive preparation process, the emulsion polymerization process is used to further reduce the emission of volatile organic compounds (VOC) and reduce environmental pollution. The increase in the itaconate content improves the 180° peel strength of the pressure-sensitive adhesive. The self-crosslinking reaction improves the long-term adhesion and heat resistance of the pressure-sensitive adhesive. The bio-based pressure-sensitive adhesive of the present invention has a holding force of preferably more than 10 hours, more preferably more than 40 hours, an initial adhesion of preferably more than 5 (representing the ball number of the rolling ball), more preferably more than 10, and a 180° peel strength of preferably more than 5N / 25mm, more preferably more than 10N / 25mm. DETAILED DESCRIPTION
[0049] The present invention is described in detail below in conjunction with specific embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the contents of the present invention still fall within the scope of protection of the present invention.
[0050] Unless otherwise specified, the raw materials in the following examples and comparative examples are commercially available.
[0051] Initial adhesion is measured according to GB / T 4852-2002; sustained adhesion is measured according to GB / T 4851-1998; 180° peel strength is measured according to GB / T 2792-2014 using a microcomputer-controlled annular peel tester. The test is stopped when the sustained adhesion exceeds 168h.
[0052] Preparation of performance test samples: The emulsion self-crosslinking bio-based itaconate pressure-sensitive adhesive prepared in the examples and comparative examples was coated on a 50 μm PET film using an electric applicator, placed in a 105° C. forced air oven and dried for 8 minutes, then covered with release paper and cut into the required size for standby use.
[0053] Example 1
[0054] (a) Preparation of pre-emulsion: 23 parts by weight of dibutyl itaconate, 48 parts by weight of butyl acrylate, 1.53 parts by weight of acrylic acid, 0.38 parts by weight of glycidyl methacrylate, 1.15 parts by weight of 1-allyloxy-3-(4-nonylphenol)-2-propanol polyoxyethylene (10) ether ammonium sulfate, 0.57 parts by weight of sodium dodecylbenzene sulfonate, 0.153 parts by weight of sodium bicarbonate and 0 parts by weight of tert-dodecyl mercaptan were stirred in 46 parts by weight of deionized water at 50° C. and 350 r / min for 50 min to prepare a pre-emulsion.
[0055] (b) Semi-continuous emulsion polymerization: 5% of the pre-emulsion obtained in step (a) is placed in a four-necked flask, and then 31 parts by weight of deionized water, 0.38 parts by weight of 1-allyloxy-3-(4-nonylphenol)-2-propanol polyoxyethylene (10) ether ammonium sulfate, 0.19 parts by weight of sodium dodecylbenzene sulfonate, and 0.076 parts by weight of sodium bicarbonate are added into the four-necked flask, and stirred at 230 r / min for 20 min. The temperature is raised to 78° C., and an ammonium persulfate solution (0.15 parts by weight of ammonium persulfate dissolved in 4.6 parts by weight of deionized water) is added into the four-necked flask, and stirring is continued until the emulsion turns blue.
[0056] (c) Using a constant pressure dropping funnel, the remaining pre-emulsion and ammonium persulfate solution (0.23 parts by weight of ammonium persulfate dissolved in 18.4 parts by weight of deionized water) are added dropwise to the reaction system of step (b) at a constant speed, and the dropping time is 2 hours. After the dropping is completed, the stirring rate is maintained to increase the reaction temperature to 85°C and react for 90 minutes. After the reaction is shut down and the temperature is cooled to 40°C, ammonia water is added to make the pH value of the emulsion 7.5. The emulsion is filtered and discharged, which is the emulsion-type self-crosslinking bio-based itaconate pressure-sensitive adhesive.
[0057] Example 2
[0058] The formula and preparation method are the same as those in Example 1, except that: 30.5 parts by weight of dibutyl itaconate and 40.5 parts by weight of butyl acrylate.
[0059] Example 3
[0060] The formula and preparation method are the same as those in Example 1, except that: 38 parts by weight of dibutyl itaconate and 33 parts by weight of butyl acrylate.
[0061] Example 4
[0062] The formula and preparation method are the same as those in Example 1, except that: 0.765 parts by weight of glycidyl methacrylate.
[0063] Example 5
[0064] The formula and preparation method are the same as those in Example 1, except that: 1.15 parts by weight of glycidyl methacrylate.
[0065] Example 6
[0066] The formula and preparation method are the same as those in Example 1, except that: 1.53 parts by weight of glycidyl methacrylate.
[0067] Example 7
[0068] The formula and preparation method are the same as those in Example 1, except that 0.023 parts by weight of tert-dodecyl mercaptan is used.
[0069] Example 8
[0070] The formula and preparation method are the same as those in Example 1, except that 0.038 parts by weight of tert-dodecyl mercaptan is used.
[0071] Example 9
[0072] The formula and preparation method are the same as those in Example 1, except that: 0 weight parts of glycidyl methacrylate.
[0073] The test results of the pressure-sensitive adhesive properties of Examples 1-9 are shown in Table 1:
[0074] Table 1 Pressure sensitive adhesive adhesion test
[0075]
[0076]
[0077] Note: The initial adhesion value represents the ball number of the rolling ball.
[0078] It can be seen from Example 1 and Examples 2-3 that when the itaconate monomer in the present invention partially replaces the acrylate monomer to prepare the bio-based pressure-sensitive adhesive, the itaconate monomer content cannot be too high. Although adding too much bio-based itaconate monomer will significantly increase the 180° peel strength, it will reduce the initial adhesion and the lasting adhesion (as shown in Example 3). In order to ensure that the bio-based pressure-sensitive adhesive has both high lasting adhesion and high initial adhesion and 180° peel strength, it is preferred in the present invention that the itaconate monomer accounts for 30-50 wt% of the total monomer mass, more preferably 30-40 wt%, and further preferably 30-35 wt%.
[0079] It can be seen from Example 1 and Example 9 that if only the acrylate monomer is partially replaced by the itaconate monomer to prepare the bio-based pressure-sensitive adhesive without adding the self-crosslinking monomer, its holding force will be significantly reduced (Example 9). Therefore, the self-crosslinking monomer is specifically introduced in the present invention to ensure the initial adhesion and 180° peel strength while significantly improving the holding force (Example 1); further, it can be seen from Example 1 and Examples 4-6 that although the introduction of the self-crosslinking monomer can improve the holding force, if the self-crosslinking monomer is introduced in excess, it will cause the initial adhesion and 180° peel strength to decrease. Therefore, in order to ensure that the bio-based pressure-sensitive adhesive has both high holding force and high initial adhesion and 180° peel strength, the preferred amount of the self-crosslinking monomer in the present invention is 0.1-3 parts by weight, and more preferably 0.16-0.38 parts by weight.
[0080] It should be noted that the embodiments described above are only used to explain the present invention and do not constitute any limitation to the present invention. The present invention has been described with reference to typical embodiments, but it should be understood that the words used therein are descriptive and explanatory words, rather than restrictive words. The present invention may be modified as specified within the scope of the claims of the present invention, and the present invention may be revised without departing from the scope and spirit of the present invention. Although the present invention described therein relates to specific methods, materials and embodiments, it does not mean that the present invention is limited to the specific examples disclosed therein, on the contrary, the present invention can be extended to all other methods and applications with the same functions.
[0081] All publications, patent applications, patents and other references mentioned in this specification are incorporated herein by reference. Unless otherwise defined, all technical and scientific terms used in this specification have the meanings conventionally understood by those skilled in the art. In the event of a conflict, the definition in this specification shall prevail.
[0082] When this specification uses the prefix "well-known to those skilled in the art", "prior art" or similar terms to introduce materials, substances, methods, steps, devices or components, etc., the objects introduced by the prefix cover those commonly used in the art when this application is filed, but also include those that are not commonly used at present but will become recognized in the art as being suitable for similar purposes.
[0083] The endpoints and any values of the scope disclosed in the present application document are not limited to the precise scope or value, and these scopes or values should be understood to include values close to these scopes or values. For numerical ranges, between the endpoint values of each scope, between the endpoint values of each scope and a separate point value, and between separate point values, one or more new numerical ranges can be combined with each other, and these numerical ranges should be considered as specifically disclosed in this article. Hereinafter, in principle, each technical solution can be combined with each other to obtain a new technical solution, which should also be considered as specifically disclosed in this article.
[0084] In the context of the present specification, any matters or items not mentioned are directly applicable to those known in the art without any changes except those explicitly stated.
[0085] Moreover, any embodiment described in this document may be freely combined with one or more other embodiments described in this document, and the technical solutions or technical ideas formed thereby are deemed to be part of the original disclosure or original record of the present invention, and should not be regarded as new content that has not been disclosed or anticipated in this document, unless a person skilled in the art considers that the combination is obviously unreasonable.
Claims
1. An emulsion-type self-crosslinking bio-based itaconate pressure-sensitive adhesive is prepared from raw materials including the following components: water, itaconate monomer, acrylate monomer, functional monomer, self-crosslinking monomer, initiator, pH buffer and emulsifier.
2. The emulsion type self-crosslinking bio-based itaconate pressure-sensitive adhesive according to claim 1, characterized in that: Each component is calculated based on 100 parts by weight of water. Itaconate monomer 5-50 parts by weight; preferably 23-38 parts by weight; Acrylate monomer 20-70 parts by weight; preferably 38-53 parts by weight; Functional monomer 0.1-4 parts by weight; preferably 1.5-2.3 parts by weight; Initiator 0.01-1 parts by weight; preferably 0.24-0.4 parts by weight; 0.1-3 parts by weight of self-crosslinking monomer; preferably 0.16-0.38 parts by weight; pH buffer 0.01-0.4 parts by weight; preferably 0.24-0.32 parts by weight; Emulsifier 0.1-15 parts by weight; preferably 1.5-4.6 parts by weight.
3. The emulsion type self-crosslinking bio-based itaconate pressure-sensitive adhesive according to claim 1, characterized in that: The itaconate monomer is one or more of dimethyl itaconate, diethyl itaconate, dibutyl itaconate, and diisooctyl itaconate; and / or, The acrylic acid ester monomer is one or more of butyl acrylate, n-octyl acrylate, isooctyl acrylate, ethyl acrylate, methyl acrylate, methyl methacrylate, isooctyl methacrylate, isobornyl acrylate, and isobornyl methacrylate; and / or, The functional monomer is a copolymerizable monomer containing a carboxylic acid group, preferably one or more of acrylic acid, methacrylic acid, itaconic acid, monomethyl itaconate, and monobutyl itaconate; and / or, The self-crosslinking monomer is one or both of glycidyl methacrylate and glycidyl acrylate; and / or, The initiator is a water-soluble thermal initiator, preferably potassium persulfate and / or ammonium persulfate; and / or, The pH buffer is sodium bicarbonate and / or disodium hydrogen phosphate; and / or, The emulsifier is one or more of anionic emulsifiers and nonionic emulsifiers, preferably one or more of sodium dodecyl sulfonate, sodium dodecylbenzene sulfonate, sodium dodecyl sulfate, 1-allyloxy-3-(4-nonylphenol)-2-propanol polyoxyethylene (10) ether ammonium sulfate, and polyoxyethylene octylphenol ether-10.
4. The emulsion type self-crosslinking bio-based itaconate pressure-sensitive adhesive according to claim 1, characterized in that: The raw materials for preparing the emulsion type self-crosslinking bio-based itaconate pressure-sensitive adhesive also include a molecular weight regulator; preferably, The molecular weight regulator is one or both of n-dodecyl mercaptan and tert-dodecyl mercaptan; and / or, Based on 100 parts by weight of water, the amount of the molecular weight regulator is 0-0.15 parts by weight, preferably 0-0.03 parts by weight.
5. A method for preparing an emulsion-type self-crosslinking bio-based itaconate pressure-sensitive adhesive as described in any one of claims 1 to 4, comprising subjecting components including water, itaconate monomers, acrylate monomers, functional monomers, self-crosslinking monomers, initiators, pH buffers, emulsifiers and optional molecular weight regulators to semi-continuous emulsion polymerization to obtain the emulsion-type self-crosslinking bio-based itaconate pressure-sensitive adhesive.
6. The preparation method according to claim 5, characterized in that The method comprises: (a) using water as a solvent, mixing itaconate monomers, acrylate monomers, functional monomers, self-crosslinking monomers, a pH buffer, an optional molecular weight regulator and 60-95% of an emulsifier to obtain a pre-emulsion; (b) reacting 3-20% of the pre-emulsion obtained in step (a), water, 1-80% of the initiator and the remaining emulsifier until the emulsion turns blue; (c) adding the remaining pre-emulsion and the initiator to the reaction system of step (b) at a uniform rate, raising the temperature for reaction, and adding a weak base to adjust the pH to a weak alkaline state after the reaction, thereby obtaining the emulsion-type self-crosslinking bio-based itaconate pressure-sensitive adhesive.
7. The preparation method according to claim 6, characterized in that: The mass ratio of the amount of water used in step (a) to the total amount of water used in step (b) is in the range of 1:(0.1-10).
8. The preparation method according to claim 6, characterized in that: In step (b), The reaction temperature is 70-80°C.
9. The preparation method according to claim 6, characterized in that: In step (c), The reaction temperature is 85-90°C and the reaction time is 30-120 min; and / or, The weak base comprises aqueous ammonia; and / or, The weak alkalinity refers to a pH of 7-9.
10. The preparation method according to claim 6, characterized in that: Step (c) also includes the step of filtering the emulsion after adjusting the pH to weak alkalinity.
Citation Information
Patent Citations
Itaconate monomer modified acrylate copolymer and preparation method thereof, and rubber composition and preparation method thereof
CN115677910A
Adhesive strips on the basis of bio-based monomers
EP2626397A1
Production method for water dispersion for pressure-sensitive adhesive and water dispersion type pressure-sensitive adhesive composition using the water dispersion
JP2012121987A
Acryl-emulsion adhesvie compositoin
KR1019980009412A
Resin mixture based on vinyl ester resin, reactive resin mortar comprising same and use thereof
US20150232595A1