Thick-wall high-acid-resistance pipeline steel and production method thereof
Through low carbon combined with fine crystal reinforced alloy design and clean steel smelting technology, the problem of insufficient corrosion resistance of subsea acid-resistant pipelines in extremely cold environments is solved, high resistance to HIC and SSCC, and the horizontal and vertical stretching and low temperature are met. Requirements for impact performance.
Patent Information
- Application Number
- CN202411105907.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-13
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-13
AI Technical Summary
Subsea acid-resistant pipelines need to have high corrosion resistance in extremely cold environments and meet HIC and SSCC detection standards. It is difficult for the prior art to maintain the toughness and strength of the material under low temperature conditions.
The design of low-carbon combined with fine crystal reinforced alloy is adopted. Through clean steel smelting and fast-rolling post-frozen technology, a structure mainly based on bainite is achieved. Combined with two-stage rolling technology and calcium treatment, the material's resistance to HIC and SSCC is improved. performance.
High concentration HIC and 90% actual yield stress SSCC detection are achieved, which meets the requirements of transverse and longitudinal tensile performance and -40℃ low-temperature impact toughness, and improves the overall performance stability of the pipeline.
Smart Images

Figure CN118996275A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of iron and steel metallurgy, and in particular to a thick-walled high-acid-resistant pipeline steel and a production method thereof. Background Art
[0002] The marine environment is extremely complex and changeable, and has long been under the test of extreme climatic conditions, including continuous low temperatures, turbulent waves, and occasional strong typhoons. At the same time, the ocean current movement and water pressure have put forward extremely high requirements on the horizontal and vertical mechanical bearing capacity of submarine pipelines. In particular, the straight seam submerged arc welding technology and the welding quality of the pipeline end are directly related to the overall performance of the product.
[0003] In a high-acid-resistant and low-temperature crack-arresting submarine acid-resistant pipeline project, the hydrogen sulfide content in the transport medium is extremely high, which puts forward extremely high requirements on the corrosion resistance of the steel material for the pipeline. It is necessary to maintain the toughness and strength of the material under extremely cold conditions and meet strict HIC and SSCC resistance testing standards. Based on this, the present invention proposes a thick-walled high-acid-resistant pipeline steel and a production method thereof. Through a reasonable component ratio and production process, the material's HIC and SSCC resistance performance is improved to ensure that the material meets the project requirements. Summary of the invention
[0004] The present invention aims at the above-mentioned technical problems, overcomes the shortcomings of the prior art, and provides a thick-walled, highly acid-resistant pipeline steel and a production method thereof. The present invention adopts a low-carbon combined with fine-grained strengthening alloy design, and through clean steel smelting and post-rolling rapid cooling technology, realizes a bainite-based organizational morphology, meets the product's transverse and longitudinal tensile performance requirements, -40°C low-temperature impact toughness, and -40°C DWTT performance requirements, and realizes high-concentration HIC and 90% actual yield stress SSCC detection.
[0005] In the first aspect, the present invention provides a thick-walled, highly acid-resistant pipeline steel, whose chemical composition and mass percentage are as follows: C: 0.02%~0.05%, Si: 0.15%~0.35%, Mn: 1.00%~1.20%, P:≤0.015%, S:≤0.0010%, Nb: 0.030~0.050%, V: 0.060~0.070%, Ti: 0.008~0.030%, Cr: 0.10~0.30%, Ni: 0.50%~0.60%, Mo:≤0.050%, Cu: 0.10~0.30%, Al: 0.015%~0.055%, B≤0.00050%, Ca: 0.0006%~0.0030%, N≤0.0060%, H≤0.0002%, and the balance is Fe and unavoidable impurities.
[0006] Furthermore, the chemical composition and mass percentage of the thick-walled, highly acid-resistant pipeline steel are as follows: C: 0.02% to 0.04%, Si: 0.15% to 0.25%, Mn: 1.00% to 1.10%, P: ≤0.013%, S: ≤0.0010%, Nb: 0.030 to 0.040%, V: 0.060 to 0.065%, Ti: 0.008 to 0.020%, Cr: 0.10 to 0.20%, Ni: 0.50% to 0.55%, Mo: ≤0.050%, Cu: 0.10 to 0.20%, Al: 0.015% to 0.050%, B≤0.00050%, Ca: 0.0006% to 0.0020%, N≤0.0060%, H≤0.0002%, and the balance is Fe and unavoidable impurities.
[0007] Furthermore, the chemical composition and mass percentage of the thick-walled, highly acid-resistant pipeline steel are as follows: C: 0.03% to 0.05%, Si: 0.25% to 0.35%, Mn: 1.10% to 1.20%, P: ≤0.015%, S: ≤0.0010%, Nb: 0.040 to 0.050%, V: 0.065 to 0.070%, Ti: 0.010 to 0.030%, Cr: 0.20 to 0.30%, Ni: 0.55% to 0.60%, Mo: ≤0.050%, Cu: 0.20 to 0.30%, Al: 0.020% to 0.055%, B≤0.00050%, Ca: 0.0008% to 0.0030%, N≤0.0060%, H≤0.0002%, and the balance is Fe and unavoidable impurities.
[0008] In a second aspect, the present invention also provides a method for producing thick-walled high acid-resistant pipeline steel, comprising the following steps:
[0009] S1. After desulfurization, smelting furnace is used for smelting. Nickel iron and copper plate are added to the smelting furnace along with scrap steel. After the molten steel is qualified, it is sent to LF / RH for refining;
[0010] S2. Add ferrovanadium in the later stage of alloying, and carry out calcium treatment after the ferrovanadium alloying is completed. After the calcium treatment, stir statically for 15-20 minutes;
[0011] S3, continuous casting adopts dynamic soft pressure and electromagnetic stirring technology, with a casting speed of 0.6-1.3m / min. After the casting, the billet is piled and cooled for 48 hours for surface inspection;
[0012] S4. The billet that has passed the surface inspection is austenitized and heated, and the tapping temperature is 1200-1260 degrees. Two-stage rolling is adopted, and the final rough rolling reduction rate is not less than 22%, and the reduction amount is not less than 26mm. The finishing rolling adopts even-pass rolling;
[0013] S5. The rolled steel plate is rapidly cooled, with a water entry temperature of 780-820 degrees, a cooling rate of 20-30 degrees Celsius / min, and a red-return temperature of 400-500 degrees;
[0014] S6. The cooled steel plates are piled, sheared, marked and stored.
[0015] Furthermore, the thickness of the steel plate in S6 is 20 to 50 mm.
[0016] Furthermore, the yield strength of the steel plate described in S6 is greater than 452 MPa, and the tensile strength is greater than 568 MPa.
[0017] Furthermore, the steel plate in S6 has an impact energy greater than 360 J at a low temperature of -40°C.
[0018] Furthermore, the SA% of the steel plate in S6 at DWTT at -40°C is ≥86.
[0019] The beneficial effects of the present invention are:
[0020] (1) The present invention adopts low-carbon design to effectively increase the ferrite content, reduce the potential difference formed by carbides inside the organization, and improve the HIC and SSCC pass rates. The low-manganese design can reduce the harm of manganese sulfide, ensure the core quality of thick-walled pipelines, and improve the performance stability of HIC and SSCC. The chromium element can improve the hardenability of thick-walled pipelines and improve the uniformity of the organization in the thickness direction of thick-walled pipelines; the nickel element can improve the adverse effects of low carbon and stabilize the strength of steel. The simultaneous use of nickel and chromium can improve the strength and toughness of thick-walled pipelines to a limited extent, and can improve the comprehensive mechanical properties after welding. The nickel element can promote the nucleation of austenite crystals to refine the grain size of the organization, strengthen the intergranular organization, and improve the low-temperature toughness of steel;
[0021] (2) The present invention adds ferrovanadium after refining and complete deoxidation, which can promote the production of vanadium nitrides and reduce the harm of nitrogen in steel. At the same time, the vanadium element in the solid solution steel improves the strength of the steel through precipitation strengthening. In the austenitization process, it can organize the growth of austenite grains, promote the nucleation of ferrite within the grain, and refine the ferrite grains, which can effectively improve the low-temperature toughness of the product and the stability of HIC and SSCC performance;
[0022] (3) The present invention produces solid inclusions mainly composed of CaS-CaO by performing calcium treatment after deoxidation. The solid inclusions are more conducive to floating on the molten steel, improving the purity of the molten steel. Clean molten steel smelting is conducive to the stability of HIC and SSCC performance;
[0023] (4) The present invention can improve the melting of the segregated structure in the core of the ingot into the austenite region by using an austenite temperature of 1200 to 1260 degrees, thereby reducing the adverse effects of the banded structure. At the same time, the high-temperature austenitization technology can enhance the precipitation strengthening of nickel, chromium, copper, niobium, vanadium, and titanium elements, enhance the metallurgical effect of the alloy elements, and improve the stability of the transverse and longitudinal mechanical properties.
[0024] (5) The present invention adopts a two-stage rolling technology and a post-rolling rapid cooling process, which can improve the adverse effects of the banded structure, refine the grain size of the structure and the stability of the structure transformation, and improve the stability of product performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is the metallographic structure diagram of the thick-walled, highly acid-resistant pipeline steel in Example 1 of the present invention. DETAILED DESCRIPTION
[0026] Example 1
[0027] The chemical composition and mass percentage of the thick-walled, highly acid-resistant pipeline steel in this embodiment are as follows: C: 0.03%, Si: 0.23%, Mn: 1.06%, P: 0.011%, S: 0.0009%, Nb: 0.037%, V: 0.063%, Ti: 0.009%, Cr: 0.17%, Ni: 0.53%, Mo: 0.030%, Cu: 0.17%, Al: 0.023%, B: 0.00030%, Ca: 0.00180%, N: 0.0051%, H: 0.00012%, and the remainder is Fe and unavoidable impurities.
[0028] The production method of thick-walled high acid-resistant pipeline steel in this embodiment specifically includes:
[0029] S1. After desulfurization, smelting furnace is used for smelting. Nickel iron and copper plate are added to the smelting furnace along with scrap steel. After the molten steel is qualified, it is sent to LF / RH for refining;
[0030] S2. Add ferrovanadium in the later stage of alloying, and carry out calcium treatment after the ferrovanadium alloying is completed. After the calcium treatment, stir statically for 15-20 minutes;
[0031] S3, continuous casting adopts dynamic soft pressure and electromagnetic stirring technology, with a casting speed of 0.6-1.3m / min. After the casting, the billet is piled and cooled for 48 hours for surface inspection;
[0032] S4. The billet that has passed the surface inspection is austenitized and heated, and the tapping temperature is 1200-1260 degrees. Two-stage rolling is adopted, and the final rough rolling reduction rate is not less than 22%, and the reduction amount is not less than 26mm. The finishing rolling adopts even-pass rolling;
[0033] S5. The rolled steel plate is rapidly cooled, with a water entry temperature of 780-820 degrees, a cooling rate of 20-30 degrees Celsius / min, and a red-return temperature of 400-500 degrees;
[0034] S6. The cooled steel plates are piled, sheared, marked and stored.
[0035] Example 2
[0036] The chemical composition and mass percentage of the thick-walled, highly acid-resistant pipeline steel in this embodiment are as follows: C: 0.041%, Si: 0.31%, Mn: 1.19%, P: 0.011%, S: 0.0008%, Nb: 0.043%, V: 0.069%, Ti: 0.017%, Cr: 0.26%, Ni: 0.57%, Mo: 0.020%, Cu: 0.27%, Al: 0.032%, B: 0.00030%, Ca: 0.0021%, N: 0.0046%, H: 0.00013%, and the balance is Fe and unavoidable impurities.
[0037] The production method of thick-walled high acid-resistant pipeline steel in this embodiment specifically includes:
[0038] S1. After desulfurization, smelting furnace is used for smelting. Nickel iron and copper plate are added to the smelting furnace along with scrap steel. After the molten steel is qualified, it is sent to LF / RH for refining;
[0039] S2. Add ferrovanadium in the later stage of alloying, and carry out calcium treatment after the ferrovanadium alloying is completed. After the calcium treatment, stir statically for 15-20 minutes;
[0040] S3, continuous casting adopts dynamic soft pressure and electromagnetic stirring technology, with a casting speed of 0.6-1.3m / min. After the casting, the billet is piled and cooled for 48 hours for surface inspection;
[0041] S4. The billet that has passed the surface inspection is austenitized and heated, and the tapping temperature is 1200-1260 degrees. Two-stage rolling is adopted, and the final rough rolling reduction rate is not less than 22%, and the reduction amount is not less than 26mm. The finishing rolling adopts even-pass rolling;
[0042] S5. The rolled steel plate is rapidly cooled, with a water entry temperature of 780-820 degrees, a cooling rate of 20-30 degrees Celsius / min, and a red-return temperature of 400-500 degrees;
[0043] S6. The cooled steel plates are piled, sheared, marked and stored.
[0044] in, Figure 1 The metallographic structure diagram of thick-walled high acid-resistant pipeline steel was obtained for Example 1. The performance test results of the aforementioned examples are shown in Tables 1 and 2.
[0045] Table 1 Transverse and longitudinal tensile properties of steel plates
[0046] Example direction Yield strength / MPa Tensile strength / MPa Elongation / % Yield strength ratio / % Example 1 Horizontal 460 570 45 81 Example 1 Vertical 455 569 42 80 Example 2 Horizontal 480 606 38 79 Example 2 Vertical 469 593 37 79
[0047] Table 2 Low temperature impact, DWTT performance, HIC and 90% actual yield stress SSCC test
[0048] Example Impact average (-40℃) / J DWTT(-40℃) / % HIC SSCC Example 1 363 88 qualified qualified Example 2 386 90 qualified qualified .
[0049] It can be seen from Tables 1 and 2 that the thick-walled high acid-resistant pipeline steel and the production method thereof provided by the present invention have successfully developed high acid-resistant pipeline steel, achieved a bainite-based organizational morphology, effectively improved the low-temperature toughness of the product and the stability of the HIC and SSCC performances, and the product meets the requirements of transverse and longitudinal tensile performance, -40°C low-temperature impact toughness, and DWTT performance at -40°C, and achieves high-concentration HIC and 90% actual yield stress SSCC detection, meeting the third-party detection approved by DNV.
[0050] In addition to the above embodiments, the present invention may also have other implementation modes. Any technical solution formed by equivalent replacement or equivalent transformation falls within the protection scope required by the present invention.
Claims
1. A thick-walled, highly acid-resistant pipeline steel, characterized in that: Its chemical composition and mass percentage are as follows: C: 0.02%~0.05%, Si: 0.15%~0.35%, Mn: 1.00%~1.20%, P:≤0.015%, S:≤0.0010%, Nb: 0.030~0.050%, V: 0.060~0.070%, Ti: 0.008~0.030%, Cr: 0.10~0.30%, Ni: 0.50%~0.60%, Mo:≤0.050%, Cu: 0.10~0.30%, Al: 0.015%~0.055%, B≤0.00050%, Ca: 0.0006%~0.0030%, N≤0.0060%, H≤0.0002%, and the balance is Fe and unavoidable impurities.
2. The thick-walled high acid-resistant pipeline steel according to claim 1 is characterized in that: Its chemical composition and mass percentage are as follows: C: 0.02% ~ 0.04%, Si: 0.15% ~ 0.25%, Mn: 1.00% ~ 1.10%, P: ≤ 0.013%, S: ≤ 0.0010%, Nb: 0.030 ~ 0.040%, V: 0.060 ~ 0.065%, Ti: 0.008 ~ 0.020%, Cr: 0.10 ~ 0.20%, Ni: 0.50% ~ 0.55%, Mo: ≤ 0.050%, Cu: 0.10 ~ 0.20%, Al: 0.015% ~ 0.050%, B ≤ 0.00050%, Ca: 0.0006% ~ 0.0020%, N ≤ 0.0060%, H ≤ 0.0002%, and the balance is Fe and unavoidable impurities.
3. The thick-walled high acid-resistant pipeline steel according to claim 1 is characterized in that: Its chemical composition and mass percentage are as follows: C: 0.03% ~ 0.05%, Si: 0.25% ~ 0.35%, Mn: 1.10% ~ 1.20%, P: ≤ 0.015%, S: ≤ 0.0010%, Nb: 0.040 ~ 0.050%, V: 0.065 ~ 0.070%, Ti: 0.010 ~ 0.030%, Cr: 0.20 ~ 0.30%, Ni: 0.55% ~ 0.60%, Mo: ≤ 0.050%, Cu: 0.20 ~ 0.30%, Al: 0.020% ~ 0.055%, B ≤ 0.00050%, Ca: 0.0008% ~ 0.0030%, N ≤ 0.0060%, H ≤ 0.0002%, and the balance is Fe and unavoidable impurities.
4. The method for producing thick-walled high acid-resistant pipeline steel according to any one of claims 1 to 3, characterized in that: The following steps are involved: S1. After desulfurization, smelting furnace is used for smelting. Nickel iron and copper plate are added to the smelting furnace along with scrap steel. After the molten steel is qualified, it is sent to LF / RH for refining; S2. Add ferrovanadium in the later stage of alloying, and carry out calcium treatment after the ferrovanadium alloying is completed. After the calcium treatment, stir statically for 15-20 minutes; S3, continuous casting adopts dynamic soft pressure and electromagnetic stirring technology, with a casting speed of 0.6-1.3m / min. After the casting, the billet is piled and cooled for 48 hours for surface inspection; S4. The billet that has passed the surface inspection is austenitized and heated, and the tapping temperature is 1200-1260 degrees. Two-stage rolling is adopted, and the final rough rolling reduction rate is not less than 22%, and the reduction amount is not less than 26mm. The finishing rolling adopts even-pass rolling; S5. The rolled steel plate is rapidly cooled, with a water entry temperature of 780-820 degrees, a cooling rate of 20-30 degrees Celsius / min, and a red-return temperature of 400-500 degrees; S6. The cooled steel plates are piled, sheared, marked and stored.
5. The production method according to claim 4, characterized in that: The thickness of the steel plate in S6 is 20 to 50 mm.
6. The production method according to claim 4, characterized in that: The yield strength of the steel plate described in S6 is greater than 452 MPa, and the tensile strength is greater than 568 MPa.
7. The production method according to claim 4, characterized in that: The steel plate in S6 has an impact energy greater than 360 J at a low temperature of -40°C.
8. The production method according to claim 4, characterized in that: The steel plate in S6 has a SA% of ≥ 86 at DWTT at -40°C.
Citation Information
Patent Citations
Medium plate for large-wall thick submerged pipeline steel and production method of medium plate
CN103993240A
Ultra-thick anti-HIC and anti-SSCC X65 pipeline steel plate and manufacturing method thereof
CN104789887A
Low yield-to-strength ratio anti-HIC and anti-SSCCX70 pipeline steel plate and making method thereof
CN104831182A
Method for producing thick-wall large-caliber acid-corrosion-resistant pipeline steel with high-phosphorus molten iron
CN107557683A
Acidic environment service pipeline steel plate with yield strength of 450MPa and production method thereof
CN108103407A
Cited By
Acid-resistant pipeline steel plate and rolling process thereof
CN120099401A
Production method of heat treatment type thick anti-acid pipe fitting steel X65MS
CN120290980A
Production method of thick-wall pipeline steel X65MS for polar region
CN121183233A
Wide and thick steel plate for high-strength anti-fatigue corrosion-resistant deep sea subsea pipeline and production method of wide and thick steel plate
CN121451055A
High-strength, fatigue-resistant, corrosion-resistant, thick steel plate for deep-sea subsea pipelines and method for producing the same
CN121451055B