Preparation method of bipolar membrane for hydrogen production by electrolysis of water
By combining the proton exchange membrane and anion exchange membrane, and using porous metal thin metal material to prepare the electrolytic bipolar membrane, the problem of high catalyst demand and short life under high voltage in the prior art is solved, and low energy consumption and high Efficient process of electrolyzing hydrogen production.
Patent Information
- Application Number
- CN202411081283.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-22
AI Technical Summary
The existing proton exchange membrane electrolytic hydroforming hydrogen production and anion exchange membrane electrolytic water technology when used in combination have problems such as high catalyst demand, difficulty in water elimination and short life under high voltage, which limits its large-scale promotion.
Using the preparation method of electrolytic bipolar membrane combining proton exchange membrane and anion exchange membrane, by adding a thin metal material with a microporous structure to the intermediate layer, the cracking of water and the conversion of hydrogen are only completed at low voltage, eliminating external acids. Alkaline supply system, simplifying equipment.
It realizes the cracking of water and conversion of hydrogen at low voltage, reduces energy consumption, improves electrolytic efficiency, reduces the demand for external acid and alkali, and reduces the operating and maintenance costs of the system.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of hydrogen production by water electrolysis, and in particular to a method for preparing a bipolar membrane for hydrogen production by water electrolysis. Background Art
[0002] There is an unprecedented global consensus on producing green, low-carbon hydrogen through electrolysis of water using renewable energy. The hydrogen energy industry includes multiple links such as hydrogen production, storage, transportation, and utilization. Since the content of elemental hydrogen in nature is extremely low, it is necessary to first consider large-scale hydrogen production through reasonable technical means. According to the carbon emission intensity of the hydrogen production process, hydrogen can be divided into gray hydrogen, blue hydrogen, and green hydrogen. Among them, the process of preparing green hydrogen by electrolysis of water coupled with renewable energy power generation has extremely low carbon emissions and is regarded as an important direction for future industrial development. There are currently three main methods for producing hydrogen by electrolysis of water: alkaline water electrolysis, proton exchange membrane water electrolysis, and anion exchange membrane water electrolysis.
[0003] Alkaline water electrolysis hydrogen production technology has been domestically produced and scaled up. Thanks to its low manufacturing cost, it currently occupies most of the market share of water electrolysis hydrogen production; however, its cold start time is as long as 1 to 2 hours, and its dynamic regulation performance is poor when directly coupled with renewable energy power generation. Proton exchange membrane water electrolysis hydrogen production has been initially commercialized, and its operation is more flexible, with excellent dynamic load characteristics, and is more adaptable to the volatility of renewable energy, but the high equipment cost and use cost limit its large-scale promotion and use. Anion exchange membrane water electrolysis technology is a new water electrolysis hydrogen production technology developed on the basis of traditional alkaline water electrolysis and proton exchange membrane water electrolysis technology. It combines the low-cost material system of alkaline water electrolysis technology and the dynamic response characteristics of proton exchange membrane water electrolysis hydrogen production technology, and is expected to bring breakthrough changes to large-scale renewable energy electrolysis hydrogen production, but there is still the defect of short life of anion exchange membrane in alkaline environment and high voltage.
[0004] In the technology of hydrogen production by water electrolysis, in addition to inorganic precious metal catalysts, another key material component is the diaphragm material. Among the two new technologies for hydrogen production by water electrolysis, the proton exchange membrane used in the proton exchange membrane electrolysis technology plays the role of conducting protons and blocking gas reactants. It generally needs to have high proton conductivity, low electronic conductivity, low gas osmotic pressure, good chemical and electrochemical stability, and low dimensional change rate. At present, proton exchange membranes are mainly homogeneous membranes and composite membranes prepared from perfluorosulfonic acid resins. However, the high cost still restricts the large-scale promotion of proton exchange membrane water electrolysis technology. The anion exchange membrane used in the anion exchange membrane water electrolysis technology plays the role of conducting hydroxide ions, while isolating the anode and cathode and blocking the mixing of hydrogen and oxygen products. In the industrial application of anion exchange membrane water electrolysis to produce hydrogen, the anion exchange membrane must meet the requirements of high ion conductivity and low resistance; good chemical / electrochemical stability, and maintain long-term stability in pure water / low-concentration alkaline aqueous solution when the water electrolysis hydrogen production system is running; good barrier properties to prevent direct contact between the anode and cathode gases and ensure low permeability water and low electroosmotic water content; excellent mechanical strength and dimensional stability, and maintain good support, tensile strength, and swelling rate during operation.
[0005] So far, proton exchange membrane water electrolysis and anion exchange membrane water electrolysis for hydrogen production have achieved great development and progress, but the technology that combines the advantages of the two is still scarce. The use of low-precious metal catalysts and low-pH cathodes can facilitate the conversion of hydrogen; on the other hand, high-pH anodes promote the splitting of water produced by oxygen. In the early technical development, anion exchange membranes and proton exchange membranes were combined, in which the proton exchange membrane was used as the anode and the anion exchange membrane was used as the cathode to prepare a composite water electrolysis hydrogen production equipment. It not only needs to add acid on the anode side to lower the pH of the anode for better proton conduction, but also needs to add alkaline solution on the cathode side to increase the pH of the cathode for the transmission of hydroxide ions; this technology not only requires a large amount of acid and alkali, but also makes it difficult to remove the water produced in the middle.
[0006] Therefore, in view of the technical shortcomings of the combination of proton exchange membrane water electrolysis and anion exchange membrane water electrolysis to produce hydrogen, it is urgent to propose a new composite bipolar membrane as the key technology for combining the two. Summary of the invention
[0007] In view of the above-mentioned defects of the prior art, the technical problem to be solved by the present invention is to combine the advantages of proton exchange membrane water electrolysis for hydrogen production and anion exchange membrane water electrolysis for hydrogen production, and propose a new composite bipolar membrane.
[0008] The purpose of the present invention is to propose a preparation method of a bipolar composite membrane for hydrogen production by electrolysis of water. By combining a proton exchange membrane and an anion exchange membrane, it is possible to complete the splitting of water and the conversion of hydrogen only at a low voltage without any catalyst in the middle, by combining a proton exchange membrane and an anion exchange membrane so that water only needs to be introduced in the middle during the hydrogen production by electrolysis of water. At the same time, the proton exchange membrane serves as the cathode and the anion exchange membrane serves as the anode.
[0009] To achieve the above object, the present invention provides a method for preparing a bipolar membrane for hydrogen production by water electrolysis, the method comprising the following steps:
[0010] S10, installing a proton exchange membrane with a single-sided protective membrane on a coating device, and spraying a perfluorosulfonic acid resin solution on a surface of the proton exchange membrane without the protective membrane to form a composite body 1;
[0011] S20, laminating a metal thin material on the surface of the first composite body to form a second composite body;
[0012] S30, coating the anion exchange resin solution on the surface of the second composite, and drying to obtain the third composite;
[0013] S40, laying a reinforced porous fiber membrane on the surface of the composite body 3 to form a composite body 4;
[0014] S50, coating the anion exchange resin solution on the surface of the composite body 4, and obtaining the composite body 5 after drying;
[0015] S60, rolling the composite five and then drying it to obtain a bipolar membrane.
[0016] Preferably, the concentration of the perfluorosulfonic acid resin solution is 5-25%, the solvent of the perfluorosulfonic acid resin solution is one or more of isopropanol, ethanol, n-propanol, and methanol; the spraying parameters of the perfluorosulfonic acid resin solution are a spraying speed of 100-400 mm / s and a spraying flow rate of 5-10 mL / min; the loading of the perfluorosulfonic acid resin is 1-4 mg / cm 2 .
[0017] Preferably, the metal thin material has a microscopic porous cavity structure.
[0018] Preferably, the metal thin material is any one of a metal titanium plate with a porous double-sided papillary structure, a metal titanium woven mesh with a porous structure, and a metal thin plate with a porous double-sided flow channel structure.
[0019] Preferably, the metal titanium plate with a porous double-sided nipple structure has a hemispherical structure with a pore size of 0.3mm, a nipple diameter of 0.8mm, and a depth of 3mm; the metal titanium woven mesh with a porous structure has a pore size of 0.5mm, and a woven mesh wire diameter of 0.8mm; the metal titanium plate with a porous double-sided flow channel structure has a flow channel on the first side and a spine on the second side, with a pore size of 0.2mm, a flow channel depth of 1mm, and a flow channel width of 1mm.
[0020] Preferably, the anion exchange resin in the anion exchange resin solution is any one of functionalized polyresin, functionalized polystyrene, and functionalized polybenzimidazole; the concentration of the anion exchange resin solution is 10-25%; the solvent in the anion exchange resin solution is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and N-methylpyrrolidone.
[0021] Preferably, the coating parameters when the anion exchange resin solution is coated on the two surfaces of the composite are: a coating wet thickness of 100-160 μm, a coating speed of 0.2-0.6 m / min, and a drying temperature of 80-100°C.
[0022] Preferably, the reinforced porous fiber membrane is any one of polyolefin non-woven fabric, polyurethane fiber membrane, polyketone membrane, and polytetrafluoroethylene non-woven fabric.
[0023] Preferably, the coating parameters when the anion exchange resin solution is coated on the four surfaces of the composite are: a coating wet thickness of 220-380 μm, a coating speed of 0.4-0.9 m / min, and a drying temperature of 140-180°C.
[0024] Preferably, the temperature of the roller pressing treatment is 60-80°C, the pressure is 0.1-0.3 MPa; and the drying temperature is 130-150°C.
[0025] Beneficial technical effects of the present invention:
[0026] 1. In the process of preparing the bipolar composite membrane, the present invention adds a metal thin material with a microscopic porous cavity structure to the middle layer. On the one hand, the cavity structure can make water have better fluidity when passing into the middle of the bipolar composite membrane; on the other hand, the porous structure can make the hydrogen ions and hydroxide ions dissociated under the action of the electric field when water passes through pass through the middle metal thin plate, providing a transmission path for hydrogen ions to go to the proton exchange membrane and hydroxide ions to go to the anion exchange membrane; in addition, since the bipolar membrane can generate the required acidic and alkaline environment inside the membrane, the external acid and alkali supply system can be omitted, simplifying the overall equipment for electrolyzing water to produce hydrogen;
[0027] 2. The bipolar composite membrane prepared by the present invention only requires a very low electrolysis voltage to complete the splitting of water, thereby reducing the energy consumption in the electrolysis process, and directly generating H+ and 0H- ions inside the membrane, reducing energy loss and improving electrolysis efficiency. The bipolar composite membrane prepared by the present invention uses the proton exchange membrane side as the cathode and the anion exchange membrane side as the anode, and water is introduced in the middle for dissociation. The generated hydrogen ions move toward the cathode under the action of the electric field and pass through the proton exchange membrane to generate hydrogen at the cathode hydrogen evolution reaction potential, and the generated hydroxide ions move toward the anode under the potential drive and pass through the anion exchange membrane to generate oxygen at the anode oxygen evolution potential; therefore, the bipolar membrane prepared by the present invention has lower energy consumption in the process of electrolytic hydrogen production;
[0028] 3. In the process of preparing the bipolar membrane, the present invention sprays the perfluorosulfonic acid resin solution on the proton exchange membrane, on the one hand, to make the metal thin material more firmly attached and avoid the risk of movement and falling off; on the other hand, the metal thin material is better embedded in the perfluorosulfonic acid resin layer, shortening the transmission path of hydrogen ions without affecting water transmission;
[0029] 4. In the process of preparing the bipolar composite membrane of the present invention, a layer of anion exchange resin solution is first applied during the process of preparing the anion exchange membrane, and the solution is dried to a non-flowing state, in order to enhance the porous fiber membrane to better adhere to the surface, and then a layer of anion exchange resin is applied to prepare an anion exchange membrane with a reinforcement layer, which solves the defect of poor mechanical strength of the anion exchange membrane and improves its tolerance;
[0030] 5. In the process of preparing the bipolar composite membrane of the present invention, it needs to be rolled and pressed and dried at the end, so that the anion exchange membrane and the proton exchange membrane have a stronger bond with the intermediate metal thin layer, shorten the transmission path of hydrogen ions and hydroxide ions, improve the transmission efficiency, and thus improve the electrochemical efficiency;
[0031] 6. The bipolar membrane prepared by the present invention reduces the demand for external acid and alkali in actual use, thereby reducing the operation and maintenance costs of the system. DETAILED DESCRIPTION
[0032] The following introduces several preferred embodiments of the present invention to make its technical content clearer and easier to understand. The present invention can be embodied in many different forms of embodiments, and the protection scope of the present invention is not limited to the embodiments mentioned in the text.
[0033] The purpose of the present invention is to propose a preparation method of a bipolar composite membrane for hydrogen production by electrolysis of water. By combining a proton exchange membrane and an anion exchange membrane, it is possible to complete the splitting of water and the conversion of hydrogen only at a low voltage without any catalyst in the middle, by combining a proton exchange membrane and an anion exchange membrane so that water only needs to be introduced in the middle during the hydrogen production by electrolysis of water. At the same time, the proton exchange membrane serves as the cathode and the anion exchange membrane serves as the anode.
[0034] The present invention provides a method for preparing a bipolar membrane for hydrogen production by electrolysis of water, comprising the following steps:
[0035] S10, installing a proton exchange membrane with a single-sided protective membrane on a coating device, and spraying a perfluorosulfonic acid resin solution on a surface of the proton exchange membrane without the protective membrane to form a composite body 1;
[0036] The concentration of the perfluorosulfonic acid resin solution is 5-25%; the solvent of the perfluorosulfonic acid resin solution is one or more of isopropanol, ethanol, n-propanol, and methanol;
[0037] The spraying parameters of the perfluorosulfonic acid resin solution are spraying speed 100-400mm / s and spraying flow rate 5-10mL / min;
[0038] The loading of the perfluorosulfonic acid resin is 1-4 mg / cm 2 .
[0039] S20, laminating a metal thin material on the surface of the first composite body to form a second composite body;
[0040] The metal thin material has a microscopic porous cavity structure; the metal thin material is any one of a metal titanium plate with a porous double-sided papillary structure, a metal titanium woven mesh with a porous structure, and a metal thin plate with a porous double-sided flow channel structure;
[0041] The metal titanium plate with a porous double-sided mastoid structure has a hemispherical structure with a pore size of 0.3mm, a mastoid diameter of 0.8mm, and a depth of 3mm; the metal titanium woven mesh with a porous structure has a pore size of 0.5mm and a woven mesh wire diameter of 0.8mm; the metal titanium plate with a porous double-sided flow channel structure has a flow channel on the first side and a spine on the second side, with a pore size of 0.2mm, a flow channel depth of 1mm, and a flow channel width of 1mm.
[0042] S30, coating the anion exchange resin solution on the surface of the second composite, and drying to obtain the third composite;
[0043] The anion exchange resin in the anion exchange resin solution is any one of functionalized poly (aryl piperidine) resin, functionalized polystyrene (4-vinyl benzyl chloride-co-styrene), and functionalized polybenzimidazole; the concentration of the anion exchange resin solution is 10-25%; and the solvent in the anion exchange resin solution is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and N-methylpyrrolidone.
[0044] The coating parameters when the anion exchange resin solution is coated on the two surfaces of the composite are as follows: a coating wet thickness of 100-160 μm, a coating speed of 0.2-0.6 m / min, and a drying temperature of 80-100° C.
[0045] S40, laying a reinforced porous fiber membrane on the surface of the composite body 3 to form a composite body 4;
[0046] The reinforced porous fiber membrane is any one of polyolefin non-woven fabric, polyurethane fiber membrane, polyketone membrane and polytetrafluoroethylene non-woven fabric.
[0047] S50, coating the anion exchange resin solution on the surface of the composite body 4, and obtaining the composite body 5 after drying;
[0048] The coating parameters of the anion exchange resin solution when coated on the four surfaces of the composite are as follows: a coating wet thickness of 220-380 μm, a coating speed of 0.4-0.9 m / min, and a drying temperature of 140-180°C.
[0049] S60, rolling the composite body 5 and then drying it to obtain a bipolar membrane. The obtained bipolar membrane is a water electrolysis diaphragm with water flowing in the middle.
[0050] The temperature of the roller pressing treatment is 60-80°C, the pressure is 0.1-0.3MPa, and the drying temperature is 130-150°C.
[0051] In the process of preparing the bipolar composite membrane of the present invention, a metal thin material with a microscopic porous cavity structure is added to the middle layer. On the one hand, the cavity structure can make water have better fluidity when passing into the middle of the bipolar composite membrane; on the other hand, the porous structure can make hydrogen ions and hydroxide ions dissociated under the action of the electric field when water passes through pass through the middle metal thin plate, providing a transmission path for hydrogen ions to go to the proton exchange membrane and hydroxide ions to go to the anion exchange membrane; in addition, since the bipolar membrane can generate the required acidic and alkaline environment inside the membrane, the external acid and alkali supply system can be omitted, simplifying the overall equipment for electrolyzing water to produce hydrogen;
[0052] The bipolar composite membrane prepared by the present invention only requires a very low electrolysis voltage to complete the splitting of water, thereby reducing the energy consumption in the electrolysis process, and directly generating H+ and 0H- ions inside the membrane, reducing energy loss and improving electrolysis efficiency. The bipolar composite membrane prepared by the present invention uses the proton exchange membrane side as the cathode and the anion exchange membrane side as the anode, and water is introduced in the middle for dissociation, and the generated hydrogen ions move toward the cathode under the action of the electric field and pass through the proton exchange membrane to generate hydrogen at the cathode hydrogen evolution reaction potential, and the generated hydroxide ions move toward the anode under the potential drive and pass through the anion exchange membrane to generate oxygen at the anode oxygen evolution potential; therefore, the bipolar membrane prepared by the present invention has lower energy consumption in the process of electrolytic hydrogen production;
[0053] In the process of preparing the bipolar membrane, the present invention sprays a perfluorosulfonic acid resin solution on the proton exchange membrane, on the one hand, to make the metal thin material more firmly attached and avoid the risk of movement and falling off; on the other hand, the metal thin material is better embedded in the perfluorosulfonic acid resin layer, shortening the transmission path of hydrogen ions without affecting water transmission;
[0054] In the process of preparing the bipolar composite membrane of the present invention, a layer of anion exchange resin solution is firstly applied during the process of preparing the anion exchange membrane, and the solution is dried to a non-flowing state, in order to enhance the porous fiber membrane to be better bonded to the surface, and then a layer of anion exchange resin is applied to prepare the anion exchange membrane with a reinforcement layer, thereby solving the defect of poor mechanical strength of the anion exchange membrane and improving its tolerance;
[0055] In the process of preparing the bipolar composite membrane of the present invention, rolling pressing and drying treatment are finally required to make the anion exchange membrane and the proton exchange membrane have a stronger combination with the intermediate metal thin layer, shorten the transmission path of hydrogen ions and hydroxide ions, improve the transmission efficiency, and thus improve the electrochemical efficiency; the bipolar membrane prepared by the present invention reduces the demand for external acid and alkali in actual use, and reduces the operation and maintenance costs of the system.
[0056] Below, the specific contents of the present invention are described by specific embodiments and comparative examples:
[0057] Example 1
[0058] (1) Weigh 100 g of perfluorosulfonic acid resin and dissolve it in 1900 g of isopropanol to form a 5% perfluorosulfonic acid resin solution;
[0059] (2) The proton exchange membrane with a single-sided protective membrane is mounted on a coating device, and the 5% perfluorosulfonic acid resin solution prepared in step (1) is sprayed on the surface of the side without the protective membrane using spraying parameters of 100 mm / s and 5 mL / min to form a composite body, wherein the loading amount of the perfluorosulfonic acid resin is 1 mg / cm 2;
[0060] (3) Laying a metal titanium plate with a double-sided mastoid structure having a pore size of 0.3 mm, a mastoid diameter of 0.8 mm, and a depth of 3 mm on the surface of the composite body 1 prepared in step (2) to form a composite body 2;
[0061] (4) weighing 100 g of functionalized poly(arylpiperidine) resin and dissolving it in 900 g of N,N-dimethylacetamide to form a 10% anion exchange resin solution;
[0062] (5) coating the anion exchange membrane resin solution prepared in step (4) on the surface of composite body 2 in step (3) using coating parameters 1 with a coating wet thickness of 100 μm and a coating speed of 0.2 m / min, and drying at 80° C. to obtain composite body 3;
[0063] (6) Laying the porous polyolefin nonwoven fabric on the surface of the composite body 3 obtained in step (5) to obtain composite body 4; continuing to use coating parameter 2 of coating wet thickness of 220 μm and coating speed of 0.4 m / min to coat the anion exchange resin solution prepared in step (4) on the surface of the porous polyolefin nonwoven fabric, and drying at 140° C. to obtain composite body 5;
[0064] (7) The temperature of the roller press was set to 60° C. and the pressure was set to 0.1 MPa. The composite 5 prepared in step (6) was passed through the roller press and then thoroughly dried at 130° C. to obtain a water electrolysis bipolar membrane with water flowing in the middle.
[0065] Example 2
[0066] (1) Weigh 250 g of perfluorosulfonic acid resin and dissolve it in 750 g of n-propanol to form a 25% perfluorosulfonic acid resin solution;
[0067] (2) The proton exchange membrane with a single-sided protective membrane is installed on a coating device, and the 25% perfluorosulfonic acid resin solution prepared in step (1) is sprayed on the side without the protective membrane using spraying parameters of 400 mm / s and 1 mL / min to form a composite body, wherein the perfluorosulfonic acid resin loading is 4 mg / cm 2 ;
[0068] (3) laying a titanium braided mesh with a pore size of 0.5 mm and a braided mesh wire diameter of 0.8 mm on the surface of the composite body 1 prepared in step (2) to form a composite body 2;
[0069] (4) weighing 250 g of functionalized poly (4-vinylbenzyl chloride-co-styrene) and dissolving it in 750 g of N,N-dimethylformamide to form a 25% anion exchange resin solution;
[0070] (5) coating the anion exchange membrane resin solution prepared in step (4) on the surface of composite body 2 in step (3) using coating parameters 1 of coating wet thickness of 160 μm and coating speed of 0.6 m / min, and drying at 100° C. to obtain composite body 3;
[0071] (6) Laying the porous polyurethane fiber membrane on the surface of the composite body 3 obtained in step (5) to obtain composite body 4; continuing to use coating parameters 2 of coating wet thickness of 380 μm and coating speed of 0.9 m / min to coat the anion exchange resin solution prepared in step (4) on the surface of the porous polyurethane fiber membrane, and drying at 180° C. to obtain composite body 5;
[0072] (7) The temperature of the roller press was set to 80° C. and the pressure was set to 0.3 MPa. The composite 5 prepared in step (6) was passed through the roller press and then thoroughly dried at 150° C. to obtain a water electrolysis bipolar membrane with water flowing in the middle.
[0073] Example 3
[0074] (1) Weigh 100 g of perfluorosulfonic acid resin and dissolve it in 900 g of ethanol to form a 10% perfluorosulfonic acid resin solution;
[0075] (2) The proton exchange membrane with a single-sided protective membrane is installed on a coating device, and the 10% perfluorosulfonic acid resin solution prepared in step (1) is sprayed on the side without the protective membrane using the spraying parameters of 200 mm / s and 3 mL / min to form a composite body, wherein the perfluorosulfonic acid resin loading is 3 mg / cm 2 ;
[0076] (3) Laying a metal titanium plate with a pore size of 0.2 mm, a flow channel depth of 1 mm, and a flow channel width of 1 mm on the surface of the composite body 1 prepared in step (2) to form a composite body 2;
[0077] (4) weighing 150 g of functionalized polybenzimidazole and dissolving it in 850 g of dimethyl sulfoxide to form a 15% anion exchange resin solution;
[0078] (5) coating the anion exchange membrane resin solution prepared in step (4) on the surface of composite body 2 in step (3) using coating parameters 1 of a coating wet thickness of 130 μm and a coating speed of 0.4 m / min, and drying at 90° C. to obtain composite body 3;
[0079] (6) Laying a porous polytetrafluoroethylene non-woven fabric on the surface of the composite body 3 obtained in step (5) to obtain a composite body 4; continuing to use coating parameters 2 of a coating wet thickness of 280 μm and a coating speed of 0.6 m / min to coat the anion exchange resin solution prepared in step (4) on the surface of the porous polytetrafluoroethylene non-woven fabric, and drying at 160° C. to obtain a composite body 5;
[0080] (7) The temperature of the roller press was set to 70° C. and the pressure was set to 0.2 MPa. The composite 5 prepared in step (6) was passed through the roller press and then thoroughly dried at 140° C. to obtain a water electrolysis bipolar membrane with water flowing in the middle.
[0081] Comparative Example 1 (no spraying of perfluorosulfonic acid resin)
[0082] (1) Installing a proton exchange membrane with a single-sided protective membrane on a coating device;
[0083] (2) laying a metal titanium plate with a double-sided mastoid structure having a pore size of 0.3 mm, a mastoid diameter of 0.8 mm, and a depth of 3 mm on the surface of the proton exchange membrane in step (1) to form a second composite;
[0084] (3) weighing 100 g of functionalized poly(arylpiperidine) resin and dissolving it in 900 g of N,N-dimethylacetamide to form a 10% anion exchange resin solution;
[0085] (4) coating the anion exchange membrane resin solution prepared in step (3) on the surface of composite body 2 in step (2) using coating parameters 1 with a coating wet thickness of 100 μm and a coating speed of 0.2 m / min, and drying at 80° C. to obtain composite body 3;
[0086] (5) Laying a porous polyolefin nonwoven fabric on the surface of the composite body 3 obtained in step (4) to obtain a composite body 4; continuing to use coating parameters 2 of a coating wet thickness of 220 μm and a coating speed of 0.4 m / min to coat the anion exchange resin solution prepared in step (3) on the surface of the porous polyolefin nonwoven fabric, and drying at 140° C. to obtain a composite body 5;
[0087] (6) The temperature of the roller press was set to 60° C. and the pressure was set to 0.1 MPa. The composite 5 prepared in step (5) was passed through the roller press and then thoroughly dried at 130° C. to obtain a water electrolysis bipolar membrane with water flowing in the middle.
[0088] Comparative Example 2 (Metal Thin Material without Flow Channel and Mastoid Structure)
[0089] (1) Weigh 100 g of perfluorosulfonic acid resin and dissolve it in 1900 g of isopropanol to form a 5% perfluorosulfonic acid resin solution;
[0090] (2) The proton exchange membrane with a single-sided protective membrane is mounted on a coating device, and the 5% perfluorosulfonic acid resin solution prepared in step (1) is sprayed on the surface of the side without the protective membrane using spraying parameters of 100 mm / s and 5 mL / min to form a composite body, wherein the loading amount of the perfluorosulfonic acid resin is 1 mg / cm 2 ;
[0091] (3) laying a metal titanium plate with a pore size of 0.3 mm on the surface of the composite body 1 prepared in step (2) to form a composite body 2;
[0092] (4) weighing 100 g of functionalized poly(arylpiperidine) resin and dissolving it in 900 g of N,N-dimethylacetamide to form a 10% anion exchange resin solution;
[0093] (5) coating the anion exchange membrane resin solution prepared in step (4) on the surface of composite body 2 in step (3) using coating parameters 1 with a coating wet thickness of 100 μm and a coating speed of 0.2 m / min, and drying at 80° C. to obtain composite body 3;
[0094] (6) Laying the porous polyolefin nonwoven fabric on the surface of the composite body 3 obtained in step (5) to obtain composite body 4; continuing to use coating parameter 2 of coating wet thickness of 220 μm and coating speed of 0.4 m / min to coat the anion exchange resin solution prepared in step (4) on the surface of the porous polyolefin nonwoven fabric, and drying at 140° C. to obtain composite body 5;
[0095] (7) The temperature of the roller press was set to 60° C. and the pressure was set to 0.1 MPa. The composite 5 prepared in step (6) was passed through the roller press and then thoroughly dried at 130° C. to obtain a water electrolysis bipolar membrane with water flowing in the middle.
[0096] Comparative Example 3 (without roller pressing)
[0097] (1) Weigh 100 g of perfluorosulfonic acid resin and dissolve it in 1900 g of isopropanol to form a 5% perfluorosulfonic acid resin solution;
[0098] (2) The proton exchange membrane with a single-sided protective membrane is mounted on a coating device, and the 5% perfluorosulfonic acid resin solution prepared in step (1) is sprayed on the surface of the side without the protective membrane using spraying parameters of 100 mm / s and 5 mL / min to form a composite body, wherein the loading amount of the perfluorosulfonic acid resin is 1 mg / cm 2 ;
[0099] (3) Laying a metal titanium plate with a double-sided mastoid structure having a pore size of 0.3 mm, a mastoid diameter of 0.8 mm, and a depth of 3 mm on the surface of the composite body 1 prepared in step (2) to form a composite body 2;
[0100] (4) weighing 100 g of functionalized poly(arylpiperidine) resin and dissolving it in 900 g of N,N-dimethylacetamide to form a 10% anion exchange resin solution;
[0101] (5) coating the anion exchange membrane resin solution prepared in step (4) on the surface of composite body 2 in step (3) using coating parameters 1 with a coating wet thickness of 100 μm and a coating speed of 0.2 m / min, and drying at 80° C. to obtain composite body 3;
[0102] (6) Laying a porous polyolefin nonwoven fabric on the surface of the composite body 3 obtained in step (5) to obtain a composite body 4; continuing to use coating parameter 2 of a coating wet thickness of 220 μm and a coating speed of 0.4 m / min to coat the anion exchange resin solution prepared in step (4) on the surface of the porous polyolefin nonwoven fabric, and drying at 140° C. to obtain a water electrolysis bipolar membrane with water flowing in the middle.
[0103] The membrane electrode prepared by the present invention is cut into a sheet of 10*10 cm in size, the proton exchange membrane side is the cathode, and 0.4 mg Pt / cm 2 The precious metal of the anion exchange membrane is the anode, and 1.0 mg Ir / cm 2 The precious metals were assembled into membrane electrodes for testing under the following test conditions: water temperature 60°C, flow rate 300mL / min.
[0104] Table 1 Membrane electrode electrolysis current density table
[0105]
[0106] It can be seen from Table 1 that in the process of water electrolysis, at the same current density, the lower the electrolysis voltage, the better the performance. Among them, Example 1 has the best performance because the bipolar composite membrane prepared is thin and the ion transmission resistance is small; the bipolar composite membrane prepared in Example 2 has the largest thickness, so the performance is relatively poor; Example 3 is in the middle. In the comparative examples, in Example 1, since perfluorosulfonic acid resin is not sprayed on the surface of the proton exchange membrane, the contact of the metal sheet is poor and the impedance is large, so the performance is poor; in Example 2, no metal sheet is added, resulting in obstruction of water transmission, so the performance is the worst; in Example 3, there is no roller pressing process, and the contact resistance is also large, and the electrolysis performance is low.
[0107] The preferred specific embodiments of the present invention are described in detail above. It should be understood that ordinary technicians in the field can make many modifications and changes based on the concept of the present invention without creative work. Therefore, all technical solutions that can be obtained by technicians in the technical field based on the concept of the present invention through logical analysis, reasoning or limited experiments on the basis of the prior art should be within the scope of protection determined by the claims.
Claims
1. A method for preparing a bipolar membrane for hydrogen production by water electrolysis, characterized in that: The method comprises the following steps: S10, installing a proton exchange membrane with a single-sided protective membrane on a coating device, and spraying a perfluorosulfonic acid resin solution on a surface of the proton exchange membrane without the protective membrane to form a composite body 1; S20, laminating a metal thin material on the surface of the first composite body to form a second composite body; S30, coating the anion exchange resin solution on the surface of the second composite, and drying to obtain the third composite; S40, laying a reinforced porous fiber membrane on the surface of the composite body 3 to form a composite body 4; S50, coating the anion exchange resin solution on the surface of the composite body 4, and obtaining the composite body 5 after drying; S60, rolling the composite five and then drying it to obtain a bipolar membrane.
2. The method for preparing a bipolar membrane for hydrogen production by water electrolysis according to claim 1, characterized in that: The concentration of the perfluorosulfonic acid resin solution is 5-25%, and the solvent of the perfluorosulfonic acid resin solution is one or more of isopropanol, ethanol, n-propanol, and methanol; the spraying parameters of the perfluorosulfonic acid resin solution are a spraying speed of 100-400 mm / s and a spraying flow rate of 5-10 mL / min; The loading of the perfluorosulfonic acid resin is 1-4 mg / cm 2 .
3. The method for preparing a bipolar membrane for hydrogen production by water electrolysis according to claim 1, characterized in that: The metal thin material has a microscopic porous cavity structure.
4. The method for preparing a bipolar membrane for producing hydrogen by electrolysis of water according to claim 3, characterized in that: The metal thin material is any one of a metal titanium plate with a porous double-sided papillary structure, a metal titanium woven mesh with a porous structure, and a metal thin plate with a porous double-sided flow channel structure.
5. The method for preparing a bipolar membrane for producing hydrogen by electrolysis of water according to claim 4, characterized in that: The metal titanium plate with a porous double-sided mastoid structure has a hemispherical structure with a pore size of 0.3mm, a mastoid diameter of 0.8mm, and a depth of 3mm; the metal titanium woven mesh with a porous structure has a pore size of 0.5mm, and a woven mesh wire diameter of 0.8mm; the metal titanium plate with a porous double-sided flow channel structure has a flow channel on the first side and a spine on the second side, with a pore size of 0.2mm, a flow channel depth of 1mm, and a flow channel width of 1mm.
6. The method for preparing a bipolar membrane for producing hydrogen by electrolysis of water according to claim 1, characterized in that: The anion exchange resin in the anion exchange resin solution is any one of functionalized polyresin, functionalized polystyrene, and functionalized polybenzimidazole; the concentration of the anion exchange resin solution is 10-25%; and the solvent in the anion exchange resin solution is one or more of N,N-dimethylformamide, N,N-dimethylacetamide, dimethyl sulfoxide, and N-methylpyrrolidone.
7. The method for preparing a bipolar membrane for producing hydrogen by electrolysis of water according to claim 1, characterized in that: The coating parameters when the anion exchange resin solution is coated on the two surfaces of the composite are as follows: a coating wet thickness of 100-160 μm, a coating speed of 0.2-0.6 m / min, and a drying temperature of 80-100° C.
8. The method for preparing a bipolar membrane for producing hydrogen by electrolysis of water according to claim 1, characterized in that: The reinforced porous fiber membrane is any one of polyolefin non-woven fabric, polyurethane fiber membrane, polyketone membrane and polytetrafluoroethylene non-woven fabric.
9. The method for preparing a bipolar membrane for producing hydrogen by electrolysis of water according to claim 1, characterized in that: The coating parameters when the anion exchange resin solution is coated on the four surfaces of the composite are as follows: a coating wet thickness of 220-380 μm, a coating speed of 0.4-0.9 m / min, and a drying temperature of 140-180°C.
10. The method for preparing a bipolar membrane for hydrogen production by electrolysis of water according to any one of claims 1 to 9, characterized in that: The temperature of the roller pressing treatment is 60-80°C, the pressure is 0.1-0.3MPa; the drying temperature is 130-150°C.