Preparation method of aerogel composite polyamide fiber and fabric

By preparing aerogel composite polyamide fibers in textiles, the combination of polydopamine and silica aerogels is used to solve the problem of insufficient warming performance of textiles in cold environments, and efficient heat retention and fiber uniformity are achieved. Significantly improves the warmth performance of the fabric.

CN118996659AInactive Publication Date: 2024-11-22ZHEJIANG JUPITER EXPERIMENTAL TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411480061.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-23
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult for existing textiles to effectively maintain body temperature in cold environments, resulting in heat loss and affecting the immune and circulation systems. The existing warm-keeping technology has problems such as poor integration and limited thermal resistance improvement.

Method used

By reacting polyamide slices with aqueous dopamine hydrochloride solution to form polydopamine composite polyamide slices, and forming silica aerogel on its surface, the aerogel composite polyamide fiber is prepared by melt spinning to achieve the aerogel and fiber Evenly distributed and well-connected.

Benefits of technology

The prepared aerogel composite polyamide fiber fabric showed significant improvement in warming performance, significantly improved thermal resistance, excellent warming performance, and good fiber uniformity and spinning properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of textile products, and relates to a preparation method of aerogel composite polyamide fibers and a fabric. The preparation method comprises the following steps: adding polyamide slices into a dopamine hydrochloride aqueous solution, then adding ethanol and ammonia water to react, centrifuging and washing to obtain polydopamine composite polyamide slices; mixing the silicon dioxide precursor, water and a solvent, then adding an acid solution to adjust the pH value, and stirring for reaction to obtain silicon dioxide sol; then adding a polydopamine composite polyamide slice, continuously stirring, taking out the polydopamine composite polyamide slice, standing, and then drying to obtain an aerogel-polydopamine-polyamide slice; the aerogel-polydopamine-polyamide slices are subjected to melt spinning and winding, and the aerogel composite polyamide fiber is obtained. The fabric prepared from the aerogel composite polyamide fiber disclosed by the invention has excellent thermal insulation performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of textile products and relates to a preparation method of aerogel composite polyamide fiber and a fabric material. Background Art

[0002] Textile fibers can be divided into two categories according to their sources and manufacturing methods: natural fibers and chemical fibers. Natural fibers mainly include fibers from plants such as cotton and hemp, as well as wool and silk from animals. Chemical fibers are produced on the basis of modern industrial development. They are fibers made by chemically processing natural or synthetic polymer compounds, and are further divided into regenerated fibers and synthetic fibers. Regenerated fibers refer to those fibers that are converted into spinnable forms by chemical means, such as rayon; while synthetic fibers originated from the invention of polyamide fibers and have become one of the most common types of fibers on the market, such as polyester fibers and nylon. With the advancement of science and technology and the development of society, people's demand for textiles is no longer limited to basic clothing needs, but they hope that textiles have more functionality, such as heat preservation, breathability, and antibacterial. Especially in cold conditions, how to effectively maintain body temperature has become an important topic. In a severe cold environment, the human body is prone to rapid heat loss, resulting in a drop in body temperature, which in turn causes freezing, frostbite and other problems. In severe cases, it will affect the normal functioning of the immune system and circulatory system, and even threaten life safety. Therefore, it is particularly important to develop textiles with good warmth retention and heat storage functions.

[0003] The thermal insulation performance of textiles is affected by many factors, including the type of fiber, the structure of the fabric, the thickness and tightness of the product, and the production process. In order to improve the thermal insulation performance of textiles, three main methods are currently adopted: (1) Surface finishing method, which includes direct finishing method of phase change materials and thermal storage microcapsule finishing method. The direct finishing method of phase change materials is a finishing method in which textiles are impregnated with finishing liquid made of phase change materials, crosslinking agents and catalysts; the thermal storage microcapsule finishing method is a finishing method in which microcapsules made of natural or synthetic polymers are used to wrap the phase change material in liquid in microspheres, and then the finishing liquid is made to impregnate, coat or spray the textiles. The microcapsules containing phase change materials absorb and release heat accordingly with the changes in the external environment temperature, and a thermal insulation textile can be obtained. (2) Hollow fiber filling method, this method fills the phase change material into the fiber, and uses the internal space of the fiber to store and release heat, so as to achieve the effect of temperature regulation and heat preservation. (3) Direct spinning method: This method mixes phase change materials or microcapsules containing phase change materials into the spinning solution to directly spin fibers with temperature regulating and heat preservation functions.

[0004] Aerogel has high porosity and large specific surface area, low density, and is filled with air as a dispersion medium, so its thermal conductivity is low. Introducing aerogel materials into fiber materials can improve the thermal insulation and heat storage performance of fibers, bringing new performance and application directions to fiber materials. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides a method for preparing an aerogel composite polyamide fiber and a fabric. The prepared fabric has excellent thermal insulation performance.

[0006] One object of the present invention is achieved by the following technical solutions: A method for preparing an aerogel composite polyamide fiber comprises the following steps: (1) adding a polyamide slice into a dopamine hydrochloride aqueous solution, then adding ethanol and ammonia water to react, centrifuging, and washing the precipitate to obtain a polydopamine composite polyamide slice; (2) Mixing a silica precursor, water, and a solvent, then adding an acid solution to adjust the pH to 2.5 to 4, stirring the reaction for 1 to 10 hours, and obtaining a silica sol; then adding a polydopamine composite polyamide slice, continuing to stir for 10 to 60 minutes, taking out the polydopamine composite polyamide slice, standing at 30 to 65°C for 1 to 24 hours, and then drying to obtain an aerogel-polydopamine-polyamide slice; (3) The aerogel-polydopamine-polyamide slices are subjected to melt spinning and winding processes to obtain aerogel composite polyamide fibers.

[0007] The polyamide slices are in the form of columnar particles with a length of about 2 to 5 mm and a diameter of about 2 to 4 mm; they include one or more of polyamide 6 slices, polyamide 66 slices, polyamide 610 slices, polyamide 11 slices, polyamide 12 slices, and the like.

[0008] Preferably, the concentration of the dopamine hydrochloride aqueous solution is 0.01 to 20 g / mL, and more preferably 0.1 to 10 g / mL. Preferably, the concentration of the ammonia water is 20 to 30% (w / w).

[0009] Preferably, the mass ratio of the polyamide slice to dopamine hydrochloride is 1:0.01 to 1. Preferably, the volume ratio of the dopamine hydrochloride aqueous solution, ethanol, and ammonia water is 10 to 100:5 to 50:1.

[0010] Preferably, the reaction temperature of step (1) is 10-40° C., and the reaction time is 0.5-5 hours.

[0011] Preferably, in step (2), the silicon dioxide precursor is one or more of tetraethyl orthosilicate (TEOS), butyl orthosilicate (TBOS), methyl orthosilicate (TMOS), methyltriethoxysilane (MTES), diethoxydimethylsilane (DEDMS), methyltrimethoxysilane (MTMS), polysiloxane (PEDS), the solvent is one or more of ethanol, methanol, acetone, isopropanol, and the acid solution is one or more of hydrochloric acid, nitric acid, acetic acid, sulfuric acid, citric acid, etc.

[0012] Preferably, the volume ratio of the silica precursor, the solvent and water is 1:(1-5):(0.3-1).

[0013] Preferably, the ratio of the mass of the polydopamine-composite polyamide slice to the volume of the silica sol is 1 g: 1-100 ml.

[0014] Preferably, the drying in step (2) includes freeze drying or normal pressure drying.

[0015] In step (2) of the present invention, the polydopamine composite polyamide slice is immersed in a silica sol, and the silica sol is uniformly formed on the surface of the polydopamine composite polyamide slice. The sol is then allowed to stand to transform into a gel, and then an aerogel is formed by drying, thereby obtaining a silica aerogel on the surface of the polydopamine composite polyamide slice.

[0016] Preferably, in step (3), the spinning temperature is 220-300° C., and the spinning speed is 800-4500 m / min.

[0017] The second object of the present invention is achieved by the following technical solutions: An aerogel composite polyamide fiber is prepared by the above preparation method.

[0018] The third object of the present invention is achieved by the following technical solutions: A fabric material is woven from the aerogel composite polyamide fiber.

[0019] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a special method for preparing aerogel composite polyamide fiber, firstly, dopamine hydrochloride is polymerized under alkaline conditions to form polydopamine, and polydopamine composite polyamide slices are obtained; then, silica aerogel is formed on the surface of the polydopamine composite polyamide slices, and fibers are obtained by melt spinning. Through this preparation method, the silica aerogel is evenly distributed in the polyamide slices and has good bonding with the polyamide slices, and uniform aerogel composite polyamide fibers can be prepared. The fabric woven with the aerogel composite polyamide fiber has excellent thermal insulation performance. DETAILED DESCRIPTION

[0020] The technical scheme of the present invention is further described below by specific embodiments. It should be understood that the specific embodiments described herein are only used to help understand the present invention and are not intended to be used for specific limitations of the present invention. Unless otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.

[0021] In the following examples and comparative examples, the size of the polyamide 66 slice is: a length of about 2-5 mm, a diameter of about 2-4 mm, and a room temperature of about 30°C.

[0022] Example 1 The aerogel composite polyamide fiber of this embodiment is prepared by the following method: (1) A dopamine hydrochloride aqueous solution with a concentration of 0.05 g / mL was prepared, 100 g of polyamide 66 slices were added to 400 ml of the dopamine hydrochloride aqueous solution, and then 100 ml of ethanol and 10 ml of 28% (w / w) ammonia water were added, and the mixture was reacted at room temperature for 3 h under stirring at 400 rpm, and centrifuged. The precipitate was washed with water and ethanol respectively, and then dried to obtain polydopamine composite polyamide slices; (2) 50 ml of tetraethyl orthosilicate, 25 ml of water and 150 ml of ethanol were mixed, and then 0.1 mol / L hydrochloric acid solution was added to adjust the pH to 3.5, and stirred at 400 rpm for 6 h at room temperature to obtain a silica sol; 100 g of the polydopamine composite polyamide slice prepared in step (1) was added to the silica sol, and stirred at 400 rpm for 30 min. The polydopamine composite polyamide slice was taken out, and allowed to stand at 60° C. for 20 h, and then freeze-dried to obtain an aerogel-polydopamine-polyamide slice; (3) The aerogel-polydopamine-polyamide slices were put into a melt spinning machine, passed through a spinning box at 260°C, ejected from a spinneret, cooled, and wound to obtain aerogel composite polyamide 6 fibers at a spinning speed of 1400 m / min.

[0023] Example 2 The aerogel composite polyamide fiber of this embodiment is prepared by the following method: (1) A dopamine hydrochloride aqueous solution with a concentration of 0.02 g / mL was prepared, 100 g of polyamide 66 slices were added to 500 ml of the dopamine hydrochloride aqueous solution, and then 100 ml of ethanol and 12 ml of 25% (w / w) ammonia water were added, and the mixture was reacted at room temperature for 2 h under stirring at 500 rpm, and then centrifuged. The precipitate was washed with water and ethanol respectively, and then dried to obtain polydopamine composite polyamide slices; (2) 60 ml of methyltrimethoxysilane, 30 ml of water and 160 ml of isopropanol were mixed, and then 0.1 mol / L hydrochloric acid solution was added to adjust the pH to 3, and stirred at 500 rpm for 5 h at room temperature to obtain a silica sol; 100 g of the polydopamine composite polyamide slice prepared in step (1) was added to the silica sol, and stirred at 500 rpm for 15 min. The polydopamine composite polyamide slice was taken out, and allowed to stand at 55° C. for 24 h, and then dried at normal pressure to obtain an aerogel-polydopamine-polyamide slice; (3) The aerogel-polydopamine-polyamide slices were put into a melt spinning machine, passed through a spinning box at 255°C, ejected from a spinneret, cooled, and wound to obtain aerogel composite polyamide 6 fibers at a spinning speed of 1200 m / min.

[0024] Example 3 The aerogel composite polyamide fiber of this embodiment is prepared by the following method: (1) A dopamine hydrochloride aqueous solution with a concentration of 0.1 g / mL was prepared, 100 g of polyamide 66 slices were added to 300 ml of the dopamine hydrochloride aqueous solution, and then 60 ml of ethanol and 8 ml of 25% (w / w) ammonia water were added, and the mixture was reacted at room temperature for 4 h under stirring at 600 rpm, and centrifuged. The precipitate was washed with water and ethanol respectively, and then dried to obtain polydopamine composite polyamide slices; (2) 70 ml of tetraethyl orthosilicate, 30 ml of water and 200 ml of ethanol were mixed, and then 0.1 mol / L hydrochloric acid solution was added to adjust the pH to 4.0, and stirred at 600 rpm for 10 h at room temperature to obtain a silica sol; 100 g of the polydopamine composite polyamide slice prepared in step (1) was added to the silica sol, and stirred at 500 rpm for 30 min. The polydopamine composite polyamide slice was taken out, and allowed to stand at 65° C. for 20 h, and then freeze-dried to obtain an aerogel-polydopamine-polyamide slice; (3) The aerogel-polydopamine-polyamide slices were put into a melt spinning machine, passed through a spinning box at 265°C, ejected from a spinneret, cooled, and wound to obtain aerogel composite polyamide 6 fibers at a spinning speed of 1600 m / min.

[0025] Comparative Example 1 In comparative example 1, polyamide 66 chips are directly put into a melt spinning machine, passed through a spinning box at 265° C., ejected through a spinneret, cooled, and wound to obtain polyamide 6 fibers, with a spinning speed of 1600 m / min.

[0026] Comparative Example 2 The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 does not contain composite polydopamine, and the specific preparation method is as follows: (1) 50 ml of tetraethyl orthosilicate, 25 ml of water and 150 ml of ethanol were mixed, and then 0.1 mol / L hydrochloric acid solution was added to adjust the pH to 3.5, and stirred at 400 rpm for 6 h at room temperature to obtain silica sol; 100 g of polyamide 6 slices were added to the silica sol, and stirred at 400 rpm for 30 min. The polyamide 6 slices were taken out, and allowed to stand at 60°C for 20 h, and then freeze-dried to obtain aerogel-polyamide slices; (2) The aerogel-polyamide slices were put into a melt spinning machine, passed through a spinning box at 260°C, ejected from a spinneret, cooled, and wound to obtain aerogel composite polyamide 6 fibers at a spinning speed of 1400 m / min.

[0027] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that no aerogel is formed in Comparative Example 3. The specific preparation method is as follows: (1) A dopamine hydrochloride aqueous solution with a concentration of 0.05 g / mL was prepared, 100 g of polyamide 66 slices were added to 400 ml of the dopamine hydrochloride aqueous solution, and then 100 ml of ethanol and 10 ml of 28% (w / w) ammonia water were added, and the mixture was reacted at room temperature for 3 h under stirring at 400 rpm, and centrifuged. The precipitate was washed with water and ethanol respectively, and then dried to obtain polydopamine composite polyamide slices; (2) The polydopamine composite polyamide chips were put into a melt spinning machine, passed through a spinning box at 260° C., ejected from a spinneret, cooled, and wound to obtain polydopamine composite polyamide 6 fibers at a spinning speed of 1400 m / min.

[0028] Comparative Example 4 The aerogel of Comparative Example 4 was physically mixed with the polydopamine composite polyamide slices: The mass of the aerogel-polydopamine-polyamide slice obtained by freeze-drying in step (2) of Example 1 was weighed to be 105 g, and it was found that the mass of the aerogel formed on the surface was approximately 5 g.

[0029] 50 ml of tetraethyl orthosilicate, 25 ml of water and 150 ml of ethanol were mixed, and then 0.1 mol / L hydrochloric acid solution was added to adjust the pH to 3.5. The mixture was stirred at 400 rpm for 6.5 h at room temperature to obtain a silica sol, which was allowed to stand at 60°C for 20 h and then freeze-dried to obtain a silica aerogel. The silica aerogel was crushed, 5 g of the mixture was mixed with 100 g of polydopamine composite polyamide slices for melt extrusion, and the melt was passed through a spinning box at 260°C and then ejected through a spinneret, cooled and wound to obtain aerogel-polydopamine composite polyamide 6 fiber at a spinning speed of 1400 m / min.

[0030] Comparative Example 5 The aerogel of Comparative Example 5 was physically mixed with the polydopamine composite polyamide slice: 50 ml of tetraethyl orthosilicate, 25 ml of water and 150 ml of ethanol were mixed, and then 0.1 mol / L hydrochloric acid solution was added to adjust the pH to 3.5. The mixture was stirred at 400 rpm for 6.5 h at room temperature to obtain a silica sol, which was allowed to stand at 60°C for 20 h and then freeze-dried to obtain a silica aerogel. The silica aerogel was crushed, 10 g of the aerogel was mixed with 100 g of polydopamine composite polyamide slices for melt extrusion, and the melt was passed through a spinning box at 260°C and then ejected through a spinneret, cooled and wound to obtain aerogel-polydopamine composite polyamide 6 fiber at a spinning speed of 1400 m / min.

[0031] The fibers prepared in Examples 1-3 and Comparative Examples 1-5 were plain woven into fabrics, with a warp density of 368 strands / 10 cm and a weft density of 250 strands / 10 cm. The thermal insulation performance of the fabrics was tested in a thermal resistance tester according to GB / T 11048-2008 "Determination of thermal resistance and moisture resistance of textiles under steady-state conditions for physiological comfort", as shown in Table 1: Table 1 Thermal resistance values ​​of fabrics prepared in Examples and Comparative Examples Example 1 Example 2 Example 3 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 Comparative Example 5 <![CDATA[Thermal resistance / (m 2 ·K·W -1 )]]> 0.296 0.311 0.317 0.103 0.223 0.112 0.214 0.282 It can be seen from Table 1 that the thermal insulation performance of the fabric prepared from the aerogel composite polyamide fiber of the embodiment is significantly improved, and the thermal resistance value is nearly 3 times that of the fabric prepared from the polyamide 6 fiber of Example 1, and the thermal insulation performance is excellent.

[0032] In Comparative Example 2, no polydopamine was compounded, and aerogel was formed alone on the surface of the polyamide slice. The bonding between the aerogel and the polyamide slice was poor, which affected the uniformity of the fiber and had limited improvement in the thermal insulation performance. In Comparative Example 3, no aerogel was added, and the thermal resistance value of the fabric prepared solely from polydopamine composite polyamide fiber was not much different from that of Comparative Example 1.

[0033] In Comparative Example 4, the aerogel and the polydopamine composite polyamide slices were physically mixed, and the thermal insulation performance of the fabric was not as good as that of Example 1. In Comparative Example 5, the weight of the aerogel was increased to 10 g, and the thermal resistance of the fabric was improved, but it was still lower than that of Example 1. This may be because a large amount of aerogel could not be evenly distributed in the polyamide, resulting in a limited increase in the thermal resistance of the fabric; and in Comparative Example 5, due to the addition of a large amount of aerogel, the fibers were uneven, resulting in easy breakage of the fibers, and the spinnability was poor.

[0034] The various aspects, embodiments, and features of the present invention should be considered to be illustrative in all aspects and not limiting of the present invention, the scope of which is defined solely by the claims. Other embodiments, modifications, and uses will be apparent to those skilled in the art without departing from the spirit and scope of the claimed invention.

[0035] In the preparation method of the present invention, the order of each step is not limited to the order listed. For those skilled in the art, without creative work, the order of each step is also within the protection scope of the present invention. In addition, two or more steps or actions can be performed simultaneously.

[0036] Finally, it should be noted that the specific embodiments described herein are merely examples of the present invention, and are not intended to limit the implementation methods of the present invention. A person skilled in the art of the present invention may make various modifications or supplements to the specific embodiments described, or replace them in a similar manner. It is not necessary and impossible to provide all examples of all implementation methods here. However, these obvious changes or modifications derived from the essential spirit of the present invention still fall within the scope of protection of the present invention, and interpreting them as any additional limitation is contrary to the spirit of the present invention.

Claims

1. A method for preparing an aerogel composite polyamide fiber, characterized in that: The preparation method comprises the following steps: (1) adding a polyamide slice into a dopamine hydrochloride aqueous solution, then adding ethanol and ammonia water to react, centrifuging, and washing the precipitate to obtain a polydopamine composite polyamide slice; (2) Mixing a silica precursor, water, and a solvent, then adding an acid solution to adjust the pH to 2.5 to 4, stirring the reaction for 1 to 10 hours, and obtaining a silica sol; then adding a polydopamine composite polyamide slice, continuing to stir for 10 to 60 minutes, taking out the polydopamine composite polyamide slice, standing at 30 to 65°C for 1 to 24 hours, and then drying to obtain an aerogel-polydopamine-polyamide slice; (3) The aerogel-polydopamine-polyamide slices are subjected to melt spinning and winding processes to obtain aerogel composite polyamide fibers.

2. The method for preparing an aerogel composite polyamide fiber according to claim 1, characterized in that: The mass ratio of polyamide slices to dopamine hydrochloride is 1:0.01~1.

3. The method for preparing an aerogel composite polyamide fiber according to claim 1, characterized in that: The concentration of dopamine hydrochloride aqueous solution is 0.01 to 20 g / mL; Ammonia concentration is 20~30% (w / w); The volume ratio of dopamine hydrochloride aqueous solution, ethanol and ammonia water is 10~100:5~50:

1.

4. The method for preparing an aerogel composite polyamide fiber according to claim 1, characterized in that: The reaction temperature of step (1) is 10-40° C., and the reaction time is 0.5-5 hours.

5. The method for preparing an aerogel composite polyamide fiber according to claim 1, characterized in that: The silicon dioxide precursor is one or more of tetraethyl orthosilicate, butyl orthosilicate, methyl orthosilicate, methyltriethoxysilane, diethoxydimethylsilane, methyltrimethoxysilane, and polysiloxane; The solvent is one or more of ethanol, methanol, acetone, and isopropanol; The acid solution is one or more of hydrochloric acid, nitric acid, acetic acid, sulfuric acid, and citric acid.

6. The method for preparing an aerogel composite polyamide fiber according to claim 1, characterized in that: The volume ratio of silica precursor, solvent and water is 1:(1~5):(0.3~1).

7. The method for preparing an aerogel composite polyamide fiber according to claim 1, characterized in that: The ratio of the mass of the polydopamine composite polyamide slice to the volume of the silica sol is 1 g: 1-100 ml.

8. The method for preparing an aerogel composite polyamide fiber according to claim 1, characterized in that: In step (3), the spinning temperature is 220-300° C., and the spinning speed is 800-4500 m / min.

9. An aerogel composite polyamide fiber, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 8.

10. A fabric, characterized in that: It is woven from the aerogel composite polyamide fiber described in claim 9.

Citation Information

Patent Citations

  • Preparation method of aerogel modified synthetic fiber and synthetic fiber prepared by same

    CN103388193A

  • Thin warm type aerogel textile fiber fabric and preparation method thereof

    CN111850729A

  • Polydopamine nanosphere / boron nitride quantum dot / graphene solid lubricant, and preparation method, application and composite material thereof

    CN113861679A

  • Graphene-containing conductive antibacterial nylon composite fiber as well as preparation method and application thereof

    CN114381821A