Preparation method and evaluation method of ultrathin asphalt mixture overlay composite test piece

Through the preparation and evaluation method of ultra-thin asphalt mixture cover composite specimens, considering the actual thickness and service status, the problem of inaccurate performance evaluation of ultra-thin asphalt mixture in the existing technology is solved, and more accurate performance reflection and evaluate.

CN119000265AActive Publication Date: 2024-11-22JIANGSU SOBUTE NEW MATERIALS CO LTD +1
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202310567685.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-19
Publication Date
2024-11-22
Estimated Expiration
2043-05-19

AI Technical Summary

Technical Problem

The existing evaluation methods of ultra-thin asphalt mixtures cannot truly reflect their performance during actual service. They are affected by factors such as disease type and aging of the lower bearing material, and the thickness and size differences lead to inconsistent performance.

Method used

The preparation method of ultra-thin asphalt mixture cover composite specimens is adopted, and molded composite specimens are prepared through mold design, aging treatment and disease pretreatment. Considering the actual thickness and service conditions, high temperature stability, water-resistance and slip resistance are carried out. , evaluation of interlayer bonding properties and fatigue life.

Benefits of technology

It more accurately reflects the performance of ultra-thin asphalt mixture under actual engineering and service conditions, provides a more realistic performance evaluation result, and overcomes the performance differences caused by thickness and size differences in existing methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004237246830000031
    Figure BDA0004237246830000031
  • Figure BDA0004237246830000041
    Figure BDA0004237246830000041
  • Figure BDA0004237246830000071
    Figure BDA0004237246830000071
Patent Text Reader

Abstract

The invention discloses a preparation method of an ultrathin asphalt mixture overlay composite test piece, which comprises the following steps: determining the thickness of an upper surface layer and the thickness of a lower surface layer of a test piece mold according to the design thickness of an ultrathin overlay and the actual thickness and gradation of the upper surface layer of an original pavement structure; determining the plane size of the test piece mold according to each evaluation index of the ultrathin overlay asphalt mixture; determining the aging time of the asphalt mixture of the lower surface layer according to the service time of the upper surface layer, and performing aging treatment; according to the thickness of the lower surface layer and the plane size of a test piece mold, preparing the lower surface layer of the molded composite test piece from the aged asphalt mixture; carrying out disease pretreatment on the formed lower surface layer according to the disease type of the upper surface layer, and uniformly coating the surface of the lower surface layer with an interlayer bonding material; and according to the determined thickness of the upper surface layer and the plane size of the test piece mold, paving an ultra-thin asphalt mixture overlay on the lower surface layer coated with the interlayer binding material to prepare the upper surface layer of the molded composite test piece so as to obtain the test composite test piece.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of asphalt pavement, and in particular relates to a method for preparing an ultra-thin asphalt mixture overlay composite specimen and an evaluation method thereof. Background Art

[0002] Ultra-thin overlay technology is a technology for paving ultra-thin asphalt mixtures with a thickness of 10mm to 25mm, which is only 1 / 3 to 1 / 2 of the traditional 4cm asphalt concrete wear layer. Ultra-thin overlay is mainly used as a functional wear layer on the road surface, with the advantages of noise reduction, restoration of surface texture, improvement of surface aesthetics, fast construction, and low resource consumption. Ultra-thin overlay is mainly used for preventive and daily maintenance of asphalt pavements, repairing mild rutting, cracks, granulation, insufficient anti-skid and other diseases of asphalt pavements, and can also be used to change white cement pavements to black.

[0003] When evaluating the performance of ultra-thin overlays indoors, the high temperature stability, water seepage resistance and structural depth of ultra-thin overlays are usually evaluated by forming a 50mm thick single-layer rutting plate, the low temperature stability of ultra-thin overlays is evaluated by forming a 50mm thick single-layer rutting plate and cutting it into small beams, and the interlayer pull-out strength of ultra-thin overlays is evaluated by forming a 50mm+50mm composite specimen. It can be seen that the existing evaluation method of ultra-thin overlay asphalt mixtures still uses the evaluation method of thick layer asphalt mixtures, but the existing evaluation method has the following problems:

[0004] (1) The cooling rate of the 25 mm thick ultra-thin overlay is twice that of the 40 mm thick asphalt mixture. Under the same mixing temperature and compaction work, the rolling states of the thin layer and the thick layer are different, resulting in performance differences;

[0005] (2) The performance of the mixture indoors and on site is affected by the size of the specimen, and the same material may exhibit different performance at different sizes.

[0006] In addition, when ultra-thin overlay is used as a maintenance method for asphalt pavement, its actual service performance is affected by the disease type and service time of the underlying asphalt mixture, and factors such as cracking and aging of the underlying material need to be considered. Therefore, affected by these factors, the existing evaluation method for ultra-thin overlay mixture cannot truly reflect the performance of ultra-thin overlay in actual service. Summary of the invention

[0007] The purpose of the present invention is to overcome the deficiencies in the prior art and to provide a method for preparing an ultra-thin asphalt mixture overlay composite specimen and an evaluation method thereof.

[0008] To achieve the above object, the present invention is implemented by adopting the following technical solutions:

[0009] In a first aspect, the present invention provides a method for preparing an ultra-thin asphalt mixture overlay composite specimen, comprising the following steps:

[0010] According to the designed thickness of the ultra-thin overlay, the actual thickness and gradation of the upper layer of the original pavement structure, the thickness of the upper layer and the thickness of the lower layer of the test piece mold are determined;

[0011] Determine the plane size of the specimen mold according to various evaluation indicators of the ultra-thin overlay asphalt mixture;

[0012] The aging time of the asphalt mixture of the lower layer of the composite specimen is determined according to the service time of the upper layer of the original pavement structure and an aging treatment is performed;

[0013] According to the thickness of the lower layer and the plane size of the specimen mold, the lower layer of the molded composite specimen is prepared using the aged asphalt mixture;

[0014] According to the type of upper layer disease of the original pavement structure, the formed lower layer is pretreated for disease, and after the pretreatment, the surface of the lower layer is evenly coated with interlayer bonding material;

[0015] According to the determined upper layer thickness and specimen mold plane size, an ultra-thin asphalt mixture overlay is laid on the lower layer of the coating interlayer bonding material to prepare the upper layer of the molded composite specimen, thereby obtaining a composite specimen for experimental testing.

[0016] Furthermore, the evaluation indexes include high temperature stability, water seepage resistance, skid resistance, interlayer adhesion, low temperature stability and fatigue life.

[0017] Furthermore, when the evaluation index is high temperature stability, interlayer bonding performance, low temperature stability, water seepage resistance, and skid resistance, the plane size of the test piece mold is 300 mm × 300 mm;

[0018] When the evaluation index is fatigue life, the plane size of the specimen mold is 400 mm×300 mm.

[0019] Furthermore, the thickness of the upper layer is 10 mm to 25 mm, and the thickness of the lower layer is 30 mm to 80 mm.

[0020] Furthermore, the bottom layer asphalt mixture is heated and aged in an oven at 85°C;

[0021] When the original pavement structure has been in service for no more than 3 years, the aging time shall not exceed 2 days;

[0022] When the upper layer of the original pavement structure has been in service for more than 3 years and less than 5 years, the aging time is more than 2 days and less than 4 days;

[0023] When the upper layer of the original pavement structure has been in service for more than 5 years, the aging time exceeds 4 days.

[0024] Further, the disease pretreatment includes:

[0025] The rutting damage of the original pavement structure is realized by rutting test loading, and the depth of rutting damage does not exceed 15mm;

[0026] The crack damage of the original pavement structure is solved by cutting, the crack depth does not exceed 80% of the thickness of the underlying layer, and the crack width does not exceed 10mm.

[0027] Furthermore, the interlayer bonding material type is one of emulsified asphalt, solvent-based asphalt, and epoxy material.

[0028] In a second aspect, the present invention provides a method for evaluating the performance of an ultra-thin asphalt mixture overlay composite specimen, comprising the following steps:

[0029] Prepare an ultra-thin asphalt mixture overlay composite specimen according to the preparation method described in the first aspect;

[0030] The composite specimens were processed according to various evaluation indicators:

[0031] When evaluating the high temperature stability, water seepage resistance, and skid resistance of composite specimens, there is no need to treat the composite specimens;

[0032] When evaluating the low temperature stability and fatigue life of composite specimens, the composite specimens need to be cut to obtain small beam composite specimens:

[0033] Among them, when evaluating the low-temperature stability, the length, height and width of the beam composite specimen were 250 mm, 35 mm and 30 mm, respectively, and the thickness of the upper layer of the beam composite specimen remained unchanged;

[0034] When evaluating fatigue life, the length, height, and width of the beam composite specimen were 380 mm, 50 mm, and 63 mm, respectively, and the thickness of the upper layer of the beam composite specimen remained unchanged;

[0035] When evaluating the interlayer bonding performance of the composite specimen, the composite specimen needs to be cored, where the core diameter is 50 mm and the core depth is at least 10 mm to 20 mm beyond the upper layer of the composite specimen;

[0036] The treated composite specimens were subjected to performance evaluation tests according to various evaluation indicators.

[0037] Furthermore, when evaluating the low-temperature stability of the composite specimen, a -10°C low-temperature bending test was performed to obtain a force-displacement curve. The fracture energy of the composite specimen was calculated through the force-displacement curve to evaluate the low-temperature stability of the composite specimen. The calculation formula of the fracture energy is as follows:

[0038]

[0039] Where x represents displacement, and the upper limit of displacement x is the displacement corresponding to the second peak value, F(x) represents load, and A represents fracture area.

[0040] For the three-point beam test of asphalt mixture, the specification requires the use of low-temperature bending strain as the evaluation index, and the fracture energy is calculated by integrating the force-displacement curve to obtain the area including the coordinate axis. Fracture energy is used here instead of low-temperature bending strain because two peaks will appear in the three-point beam specimen of the double-layer composite specimen. The calculation of the low-temperature bending strain index in the existing specification is only applicable to the first peak, so this index is not suitable for evaluating composite specimens, while fracture energy can cover the entire process of the two peaks, so the fracture energy index evaluation is more accurate and reliable.

[0041] Further, when evaluating the interlayer bonding performance, the composite specimen is subjected to a pull-out strength test, which includes the following steps in order:

[0042] 1) Place the composite specimen in a 25℃ environmental chamber for more than 4 hours;

[0043] 2) Use two-component epoxy AB glue to bond and fix the pulling head to the core sample on the surface of the composite specimen;

[0044] 3) Place the composite specimen in a 25°C environment box and cure for more than 30 minutes;

[0045] 4) Take out the composite specimen, place the chuck on the pulling head and fix it, and test it with an automatic pulling machine with a test loading rate of 0.2 MPa / s.

[0046] Compared with the prior art, the present invention has the following beneficial effects:

[0047] The method for preparing ultra-thin asphalt mixture overlay composite specimens and the method for evaluating their performance provided by the present invention introduce factors such as the actual thickness of the ultra-thin overlay and the thickness of the underlying supporting layer of the road structure in service, the type of disease, the degree of aging, etc., and evaluate the high-temperature stability, low-temperature stability, skid resistance, water permeability resistance, interlayer bonding performance and fatigue life of the ultra-thin overlay by molding composite specimens. The proposed preparation and evaluation methods are closer to the actual molding process and service conditions of the project, and can better reflect the actual performance of the ultra-thin overlay. DETAILED DESCRIPTION

[0048] The present invention is further described below. The following examples are only used to more clearly illustrate the technical solution of the present invention, and are not intended to limit the protection scope of the present invention.

[0049] Example 1

[0050] The designed thickness of the ultra-thin overlay is 2 cm, and the gradation type is dense skeleton embedded high-toughness asphalt mixture HTUC-10; the actual thickness of the upper layer of the original pavement structure is 5 cm, and the gradation type is suspended dense asphalt concrete AC-13; therefore, the thickness of the upper layer and the lower layer of the specimen mold are determined to be 2 cm and 5 cm respectively.

[0051] In this embodiment, the high temperature stability of the asphalt mixture, that is, the dynamic stability index of the asphalt mixture, is evaluated, so the plane size of the test piece mold is determined to be 300 mm×300 mm.

[0052] The service life of the upper layer of the original pavement structure is 1 year and no more than 3 years. Therefore, the lower layer asphalt mixture of the ultra-thin asphalt mixture overlay composite specimen is treated by heating aging in an oven at 85°C for 16 hours.

[0053] The lower layer of the molded composite specimen was prepared using aged asphalt mixture, with a lower layer thickness of 5 cm and a specimen mold plane size of 300 mm × 300 mm.

[0054] The upper layer of the original pavement structure has no rutting and cracking defects, so there is no need to pre-treat the defects of the formed lower layer. The interlayer bonding material is directly and evenly coated on the surface of the lower layer. The interlayer bonding material is non-stick emulsified asphalt.

[0055] An ultra-thin asphalt mixture overlay is laid on the lower layer of the specimen coated with the interlayer bonding material to prepare the upper layer of the molded composite specimen, thereby obtaining a composite specimen for experimental testing.

[0056] According to the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (T0719-2011), a rutting test was carried out on the composite specimen to obtain the rutting depth and dynamic stability of the composite specimen.

[0057] In order to illustrate the advancement and creativity of the method for preparing ultra-thin asphalt mixture overlay composite specimens and the evaluation method thereof proposed in the present invention, in addition to the experimental results of the composite specimens, this embodiment also compares the rutting test results of 5 cm suspended dense asphalt concrete AC13, 5 cm dense skeleton embedded high-toughness asphalt mixture HTUC-10, and 5 cm suspended dense asphalt concrete AC13 + 5 cm dense skeleton embedded high-toughness asphalt mixture HTUC-10, as shown in Table 1.

[0058] Table 1 Comparative evaluation of high temperature anti-rutting performance of different specimen combinations

[0059]

[0060]

[0061] The results show that by forming a composite specimen combination that takes into account the actual thickness and service condition, and conducting rutting tests, the results can better reflect the actual performance level of the pavement structure with an additional overlay layer thickness than single-layer specimens and the commonly used 5cm+5cm composite specimens.

[0062] Example 2

[0063] The design thickness of the ultra-thin overlay is 1.5 cm, and the gradation type is a dense skeleton embedded high-toughness asphalt mixture HTUC-5; the actual thickness of the upper layer of the original pavement structure is 5 cm, and the gradation type is a skeleton dense asphalt mixture SMA-13; therefore, the thickness of the upper layer and the lower layer of the specimen mold are determined to be 1.5 cm and 5 cm respectively.

[0064] In this embodiment, the fatigue life of the asphalt mixture, that is, the 15°C four-point bending fatigue life index of the asphalt mixture is evaluated, so the plane size of the test piece mold is determined to be 400mm×300mm.

[0065] The service life of the upper layer of the original pavement structure is 4 years, so the lower layer asphalt mixture of the ultra-thin asphalt mixture overlay composite specimen is treated by heating aging in an oven at 85°C for 96 hours.

[0066] The lower layer of the molded composite specimen was prepared using aged asphalt mixture, with a lower layer thickness of 5 cm and a specimen mold plane size of 400 mm × 300 mm.

[0067] The upper layer of the original pavement structure has rutting and cracking defects, so the formed lower layer needs to be pretreated. The rutting depth is 13mm, the crack depth is 3.5cm, and the width is 9mm. After the pretreatment, the surface of the lower layer is evenly coated with interlayer bonding material, and the material type is high-viscosity and high-elastic emulsified asphalt;

[0068] On the lower layer of the specimen coated with the interlayer bonding material, a 1.5 cm ultra-thin asphalt mixture overlay was laid to prepare the upper layer of the molded composite specimen, thereby obtaining a composite specimen for experimental testing.

[0069] By cutting the composite specimens and keeping the thickness of the upper layer of the composite specimens unchanged, composite beams with a length, height and width of 380 mm, 50 mm and 63 mm respectively were obtained.

[0070] According to the "Test Procedures for Asphalt and Asphalt Mixtures in Highway Engineering" (T0739-2011), a four-point bending fatigue life test of asphalt mixture was carried out on the composite specimens to obtain the fatigue life times of the composite specimens.

[0071] In addition to the experimental results of the composite specimens, this embodiment also compares the four-point bending fatigue life test results of single-layer dense skeleton asphalt concrete SMA13 and single-layer dense skeleton embedded high-toughness asphalt mixture HTUC-5. The test conditions are 15°C and 400με. The results are shown in Table 2.

[0072] Table 2 Comparative evaluation of four-point bending fatigue life of different specimen combinations

[0073] Specimen combination type Fatigue life / times SMA-13+HTUC-5 421981 SMA-13 95814 HTUC-5 1000000

[0074] The results show that the four-point bending fatigue life test is carried out by forming a composite specimen combination that takes into account the actual thickness and service condition. The results are better than those of single-layer specimens to reflect the actual performance level of the pavement structure with the added overlay layer.

[0075] Example 3

[0076] The design thickness of the ultra-thin overlay is 1 cm, and the gradation type is a dense skeleton embedded high-toughness asphalt mixture HTUC-5; the actual thickness of the upper layer of the original pavement structure is 4 cm, and the gradation type is a skeleton dense asphalt mixture SMA-13; therefore, the thickness of the upper layer and the lower layer of the specimen mold are determined to be 1 cm and 4 cm respectively.

[0077] In this embodiment, the interlayer bonding performance of the asphalt mixture, that is, the interlayer tensile strength index of the asphalt mixture is evaluated, so the plane size of the test piece mold is determined to be 300mm×300mm.

[0078] The service life of the upper layer of the original pavement structure is 2 years, so the lower layer asphalt mixture of the ultra-thin asphalt mixture overlay composite specimen is treated by heating aging in an oven at 85°C for 16 hours.

[0079] The lower layer of the molded composite specimen was prepared using aged asphalt mixture with a lower layer thickness of 4 cm and a specimen mold plane size of 300 mm × 300 mm.

[0080] The upper layer of the original pavement structure has no obvious rutting and cracking diseases, so there is no need to pre-treat the formed lower layer. The interlayer bonding material is evenly coated on the surface of the lower layer. The material type is water-based epoxy emulsified asphalt;

[0081] On the lower layer of the specimen coated with the interlayer bonding material, a 1 cm ultra-thin asphalt mixture overlay was laid to prepare the upper layer of the molded composite specimen, thereby obtaining a composite specimen for experimental testing.

[0082] The composite specimen is subjected to core drilling, wherein the core drilling diameter is 50 mm and the core drilling depth exceeds the upper layer of the composite specimen by at least 10 mm to 20 mm.

[0083] The pull-out strength test of the composite specimen includes the following steps in order:

[0084] 1) Place the composite specimen in a 25℃ environmental chamber for more than 4 hours;

[0085] 2) Use two-component epoxy AB glue to bond and fix the pulling head to the core sample on the surface of the composite specimen;

[0086] 3) Place the composite specimen in a 25°C environment box and cure for more than 30 minutes;

[0087] 4) Take out the composite specimen, place the chuck on the pulling head and fix it, and test it with an automatic pulling machine with a test loading rate of 0.2 MPa / s.

[0088] In addition to the experimental results of the composite specimens, this embodiment also compares the interlayer tensile strength of the double-layer composite specimens of 5cm dense skeleton asphalt concrete SMA13 + 5cm dense skeleton embedded high-toughness asphalt mixture HTUC-5, as well as the adhesion tensile strength between the interlayer bonding material and the dense skeleton asphalt concrete SMA13. The results are shown in Table 3.

[0089] Table 3 Comparative evaluation of pull-out strength of different specimen combinations

[0090] Specimen combination type Pull-out strength / Mpa 5cm SMA-13+5cm HTUC-5 0.94 5cm SMA-13+2cm HTUC-5 0.61 SMA13+Epoxy Emulsified Asphalt 2.08

[0091] The results show that the interlayer bond strength test is carried out by forming a combination of composite specimens that take into account the actual thickness and service condition. The results are better able to reflect the actual performance level of the pavement structure when the overlay layer is added, compared with the material adhesion strength test and the commonly used 5cm+5cm composite specimens.

[0092] It should be noted that in the above-mentioned embodiments of the present invention, according to the Highway Asphalt Pavement Design Specifications (JTGD50-2017), the gradings with different nominal maximum particle sizes have different recommended thicknesses. Taking into account factors such as compaction and paving, the thickness is generally 2 to 3 times the nominal maximum particle size. For example, the grading type is SMA-10, the nominal maximum particle size is 13.2 mm, and the recommended design thickness is 2 cm to 3 cm. The grading type is SMA13, the nominal maximum particle size is 16 mm, and the recommended design thickness is 3 to 5 cm.

[0093] Table 4 Thickness of asphalt mixture layer with different particle sizes

[0094]

[0095] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing an ultra-thin asphalt mixture overlay composite specimen, characterized in that: The steps include: According to the designed thickness of the ultra-thin overlay, the actual thickness and gradation of the upper layer of the original pavement structure, the thickness of the upper layer and the thickness of the lower layer of the test piece mold are determined; Determine the plane size of the specimen mold according to various evaluation indicators of the ultra-thin overlay asphalt mixture; The aging time of the asphalt mixture of the lower layer of the composite specimen is determined according to the service time of the upper layer of the original pavement structure and an aging treatment is performed; According to the thickness of the lower layer and the plane size of the specimen mold, the lower layer of the molded composite specimen is prepared using the aged asphalt mixture; According to the type of upper layer disease of the original pavement structure, the formed lower layer is pretreated for disease, and after the pretreatment, the surface of the lower layer is evenly coated with interlayer bonding material; According to the determined upper layer thickness and specimen mold plane size, an ultra-thin asphalt mixture overlay is laid on the lower layer of the coating interlayer bonding material to prepare the upper layer of the molded composite specimen, thereby obtaining a composite specimen for experimental testing.

2. The method for preparing an ultra-thin asphalt mixture overlay composite specimen according to claim 1, characterized in that: The evaluation indexes include high temperature stability, water seepage resistance, skid resistance, interlayer bonding performance, low temperature stability and fatigue life.

3. The method for preparing an ultra-thin asphalt mixture overlay composite specimen according to claim 2, characterized in that: When the evaluation index is high temperature stability, interlayer bonding performance, low temperature stability, water seepage resistance, and skid resistance, the plane size of the test piece mold is 300mm×300mm; When the evaluation index is fatigue life, the plane size of the specimen mold is 400 mm×300 mm.

4. The method for preparing an ultra-thin asphalt mixture overlay composite specimen according to claim 3, characterized in that: The thickness of the upper layer is 10 mm to 25 mm, and the thickness of the lower layer is 30 mm to 80 mm.

5. The method for preparing an ultra-thin asphalt mixture overlay composite specimen according to any one of claims 1 to 4, characterized in that: The lower layer of asphalt mixture is heated and aged in an oven at 85°C; When the original pavement structure has been in service for no more than 3 years, the aging time shall not exceed 2 days; When the upper layer of the original pavement structure has been in service for more than 3 years and less than 5 years, the aging time is more than 2 days and less than 4 days; When the upper layer of the original pavement structure has been in service for more than 5 years, the aging time exceeds 4 days.

6. The method for preparing an ultra-thin asphalt mixture overlay composite specimen according to claim 5, characterized in that: The disease pretreatment includes: The rutting damage of the original pavement structure is realized by rutting test loading, and the depth of rutting damage does not exceed 15mm; The crack damage of the original pavement structure is solved by cutting, the crack depth does not exceed 80% of the thickness of the underlying layer, and the crack width does not exceed 10mm.

7. The method for preparing an ultra-thin asphalt mixture overlay composite specimen according to claim 6, characterized in that: The interlayer bonding material type is one of emulsified asphalt, solvent-based asphalt, and epoxy-based material.

8. A method for evaluating the performance of ultra-thin asphalt mixture overlay composite specimens, characterized in that: The steps include: Prepare an ultra-thin asphalt mixture overlay composite specimen according to the preparation method described in claims 1 to 7; The composite specimens were processed according to various evaluation indicators: When evaluating the high temperature stability, water seepage resistance, and skid resistance of composite specimens, there is no need to treat the composite specimens; When evaluating the low temperature stability and fatigue life of composite specimens, the composite specimens need to be cut to obtain small beam composite specimens: Among them, when evaluating the low-temperature stability, the length, height and width of the beam composite specimen were 250 mm, 35 mm and 30 mm, respectively, and the thickness of the upper layer of the beam composite specimen remained unchanged; When evaluating fatigue life, the length, height, and width of the beam composite specimen were 380 mm, 50 mm, and 63 mm, respectively, and the thickness of the upper layer of the beam composite specimen remained unchanged; When evaluating the interlayer bonding performance of the composite specimen, the composite specimen needs to be cored, where the core diameter is 50 mm and the core depth is at least 10 mm to 20 mm beyond the upper layer of the composite specimen; The treated composite specimens were subjected to performance evaluation tests according to various evaluation indicators.

9. The method for evaluating the performance of ultra-thin asphalt mixture overlay composite specimens according to claim 8, characterized in that: When evaluating the low-temperature stability of the composite specimen, a -10°C low-temperature bending test is used to obtain a force-displacement curve. The fracture energy of the composite specimen is calculated through the force-displacement curve to evaluate the low-temperature stability of the composite specimen. The calculation formula of the fracture energy is as follows: Where x represents displacement, and the upper limit of displacement x is the displacement corresponding to the second peak value, F(x) represents load, and A represents fracture area.

10. The method for evaluating the performance of ultra-thin asphalt mixture overlay composite specimens according to claim 9, characterized in that: When evaluating the interlayer bonding performance, the composite specimen is subjected to a pull-out strength test, which includes the following steps in order: 1) Place the composite specimen in a 25℃ environmental chamber for more than 4 hours; 2) Use two-component epoxy AB glue to bond and fix the pulling head to the core sample on the surface of the composite specimen; 3) Place the composite specimen in a 25°C environment box and cure for more than 30 minutes; 4) Take out the composite specimen, place the chuck on the pulling head and fix it, and test it with an automatic pulling machine with a test loading rate of 0.2 MPa / s.

Citation Information

Patent Citations

  • Water-based epoxy emulsified asphalt low-temperature performance prediction method based on low-temperature evaporation method

    CN115014984A

  • Indoor aging simulation method based on aging characteristics of middle surface layer material on asphalt pavement

    CN115615909A