Photoresist stripping liquid with high recovery rate

By using tetranuclear alkaline ionic liquid additives in the photoresist stripping solution, the problem of damage to the molybdenum layer and copper layer of the photoresist stripping solution is solved, and the recovery rate of polar organic solvents is improved, achieving more efficient photoresist removal and environmental protection.

CN119002199APending Publication Date: 2024-11-22HEFEI SINOPISE MATERIALS CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411386432.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-30
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing photoresist stripping liquid is prone to damage the molybdenum layer and copper substrate when removing the photoresist, and the polar organic solvent recovery rate is low, resulting in environmental pollution.

Method used

A photoresist stripping liquid with high recovery rate is used, which contains 94-97% polar organic solvent, 2-5% organic alkali, 0.01-0.2% corrosion inhibitor and 0.1-1% auxiliary agent, among which The additive consists of bromine alkyl, sodium hydroxide, piperazine and potassium hydroxide, etc., and is prepared through specific reaction steps to form a tetranuclear alkaline ionic liquid, increasing the alkaline position distribution and steric hindrance, and reducing the molybdenum layer and Damage to the copper layer.

Benefits of technology

It improves the peeling effect of photoresist, reduces damage to the molybdenum layer and copper layer, improves the recovery rate of polar organic solvents, reduces the incineration and disposal rate of organic waste, and has a good environmental protection effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119002199A_ABST
    Figure CN119002199A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of photoresist, and particularly discloses a high-recovery-rate photoresist stripping liquid which comprises the following components in percentage by mass: 94-97% of a polar organic solvent, 2-5% of organic alkali, 0.01-0.2% of a corrosion inhibitor and 0.1-1% of an auxiliary agent. The photoresist stripping liquid provided by the invention can enhance the stripping effect of the photoresist and reduce the damage to a molybdenum layer and a substrate copper layer, the recovery rate of the polar organic solvent is improved, and the incineration disposal rate of organic wastes is reduced, so that the photoresist stripping liquid plays a positive role in environmental protection.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photoresists, and in particular relates to a photoresist stripping solution with a high recovery rate. Background Art

[0002] In the process of manufacturing semiconductor materials, a photoresist mask is formed on the surface of some material substrates, and the pattern is transferred after exposure. After obtaining the required pattern, the residual photoresist needs to be stripped off before the next process. The main function of the photoresist stripping solution is to dissolve and remove the photoresist through chemical reactions. In this process, it is required to completely remove the unnecessary photoresist, and in order to reduce the wiring line width in high-generation panels to save space, copper wiring with better resistivity is selected to replace aluminum wiring. However, the adhesion of copper wiring to the glass substrate is poor, and the copper lower layer needs to be supplemented by one of molybdenum, molybdenum alloy, titanium, and titanium alloy. Among them, titanium and titanium alloy are expensive, and molybdenum and molybdenum alloys have a higher cost performance. Because the commercially available photoresist stripping solution corrodes the molybdenum layer, forming an undercut; at the same time, due to the nature of copper itself, it is easy to be oxidized to form an oxidized state, resulting in a change in resistance. Therefore, the photoresist stripping solution is required to micro-corrode the copper metal film layer while not corroding the molybdenum and copper substrate.

[0003] In addition, since the photoresist stripping solution contains a variety of complex organic solvents and additives, these components will undergo complex chemical reactions during use, resulting in more complex and variable components in the waste liquid. The complex components not only increase the difficulty of recycling, but may also cause secondary pollution during the recycling process, reducing the recovery rate. At present, the recycling of organic stripping liquid waste is usually carried out by recycling the organic solvents therein and incinerating the non-recyclable parts; however, the existing organic stripping liquid generally uses a large amount of amine additives, which cannot be recycled, and the recovery rate of polar organic solvents in the stripping liquid is low, resulting in a large amount of organic matter being incinerated and discharged, which in turn causes serious environmental pollution. Summary of the invention

[0004] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a photoresist stripping solution with a high recovery rate, which can enhance the stripping effect of the photoresist, reduce the damage to the molybdenum layer and the copper layer of the substrate, and improve the recovery rate of the polar organic solvent, thereby reducing the incineration disposal rate of organic waste, thereby playing a positive role in environmental protection.

[0005] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:

[0006] A photoresist stripping solution with a high recovery rate, comprising, by mass percentage: 94-97% polar organic solvent, 2-5% organic base, 0.01-0.2% corrosion inhibitor, and 0.1-1% auxiliary agent;

[0007] The auxiliary agent has a structure shown in formula (I):

[0008]

[0009] Wherein, n is any integer between 8 and 12, and m is any integer between 4 and 8.

[0010] Furthermore, the preparation method of the auxiliary agent comprises the following steps:

[0011] S1. Evenly mix bromoalkane and sodium hydroxide, and heat to 40-50°C to obtain a mixed solution 1; evenly mix piperazine and water, and heat to 70-80°C to obtain a mixed solution 2; dropwise add the mixed solution 2 to the mixed solution 1, and after the addition of the mixed solution 2 is completed within 1-2 hours, heat to 120-130°C and stir to react for 6-8 hours; wait for the reaction product to cool to room temperature, stand for 2-4 hours, and take the upper layer of liquid to obtain compound A;

[0012] S2, adding compound A to dibromoalkane, stirring and reacting at 110-120° C. for 7-8 hours, and after the reaction, vacuum drying at 50-60° C. for 24 hours to obtain compound B;

[0013] S3. Add compound B and potassium hydroxide to anhydrous ethanol, stir and react at room temperature for 36-48 hours, filter, distill the filtrate under reduced pressure to remove the solvent, wash and purify with acetone, and vacuum dry at 80°C for 48 hours to obtain an auxiliary agent.

[0014] Further, in step S1, the brominated alkane is any one of brominated octane, brominated nonane, brominated decane, brominated undecane, and brominated dodecane;

[0015] In step S2, the dibromoalkane is any one of 1,4-dibromobutane, 1,5-dibromopentane, 1,6-dibromohexane, 1,7-dibromoheptane and 1,8-dibromooctane.

[0016] Further, in step S1, the molar ratio of the bromoalkane, piperazine, sodium hydroxide, and water is (2-2.5):1:(2.1-2.2):20;

[0017] In step S2, the molar ratio of compound A to dibromoalkane is 1:(1-1.3);

[0018] In step S3, the molar ratio of compound B to potassium hydroxide is 1:(4.1-4.3).

[0019] Furthermore, the reaction formula of the preparation method of the auxiliary agent is as follows:

[0020]

[0021] Furthermore, the polar organic solvent is any one of N-methylformamide, N-methylpyrrolidone, N,N-dimethylformamide, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether, or a combination of two or more thereof.

[0022] Furthermore, the organic base is any one of diglycolamine, ethylene glycolamine, diethanolamine, triethanolamine, methyldiethanolamine, and hydroxyethylethylenediamine, or a combination of two or more thereof.

[0023] Furthermore, the corrosion inhibitor is a nitrogen azole compound and / or an organic polyphenol compound.

[0024] Furthermore, the azole compound is any one of tolyltriazole, benzotriazole, and 5-aminotetrazole, or a combination of two or more thereof.

[0025] Furthermore, the organic polyphenol compound is any one of catechin, gallic acid, tannic acid, and pyrogallol, or a combination of more than one thereof.

[0026] Compared with the prior art, the present invention has the following beneficial effects:

[0027] 1. The present invention provides a photoresist stripping solution with a high recovery rate, wherein the auxiliary agent is a tetranuclear alkaline ionic liquid. The tetranuclear structure increases the distribution of alkaline sites, which helps to soften the photoresist layer, reduce its adhesion to the chip surface, and enhance the stripping effect; at the same time, a long alkyl chain is introduced so that the obtained auxiliary agent has a larger steric hindrance, thereby reducing the damage of the stripping solution to the molybdenum layer and the copper layer of the substrate.

[0028] 2. Compared with the organic stripping solution in the prior art, the photoresist stripping solution provided by the present invention has lower use cost while maintaining the same stripping effect. At the same time, since it contains a higher component of polar organic solvents, the recovery rate of polar organic solvents is improved, which reduces the pressure on environmental protection equipment to dispose of organic waste, and has a positive impact on environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:

[0030] Figure 1 It is the OM image and cross-sectional SEM image of the substrate sample provided by the present invention; Figure 1 In the figure, (A) is the planar OM image of the substrate sample; (B) is the cross-sectional SEM image of the substrate sample.

[0031] Figure 2OM image and cross-sectional SEM image of the sample after stripping using the photoresist stripping solution of Example 1 of the present invention; Figure 2 In the figure, (A) is a planar OM image of the sample after being stripped using the photoresist stripping solution of Example 1; (B) is a cross-sectional SEM image of the sample after being stripped using the photoresist stripping solution of Example 1.

[0032] Figure 3 OM image and cross-sectional SEM image of the sample after stripping using the photoresist stripping solution of Comparative Example 1 of the present invention; Figure 2 In the figure, (A) is a planar OM image of the sample after stripping using the photoresist stripping solution of Comparative Example 1; (B) is a cross-sectional SEM image of the sample after stripping using the photoresist stripping solution of Comparative Example 1.

[0033] Figure 4 OM image and cross-sectional SEM image of the sample after stripping using the photoresist stripping solution of Comparative Example 2 of the present invention; Figure 2 In the figure, (A) is a planar OM image of the sample after being stripped using the photoresist stripping solution of Comparative Example 2; (B) is a cross-sectional SEM image of the sample after being stripped using the photoresist stripping solution of Comparative Example 2;

[0034] Figure 5 OM image and cross-sectional SEM image of the sample after stripping using the photoresist stripping solution of Comparative Example 3 of the present invention; Figure 2 In the figure, (A) is a planar OM image of the sample after stripping using the photoresist stripping solution of Comparative Example 3; (B) is a cross-sectional SEM image of the sample after stripping using the photoresist stripping solution of Comparative Example 3;

[0035] Figure 6 OM image and cross-sectional SEM image of the sample after stripping using the photoresist stripping solution of Comparative Example 4 of the present invention; Figure 2 In the figure, (A) is a planar OM image of the sample after stripping using the photoresist stripping solution of Comparative Example 4; (B) is a cross-sectional SEM image of the sample after stripping using the photoresist stripping solution of Comparative Example 4. DETAILED DESCRIPTION

[0036] The following will be combined with the accompanying drawings to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Preparation Example 1

[0038] This preparation example provides an auxiliary agent, and the preparation method of the auxiliary agent is as follows:

[0039] S1. Mix 2 mol of octane bromide and 2.1 mol of sodium hydroxide evenly, and heat to 40°C to obtain a mixed solution 1; mix 1 mol of piperazine and 20 mol of water evenly, and heat to 70°C to obtain a mixed solution 2; add the mixed solution 2 dropwise to the mixed solution 1, and after the mixed solution 2 is added dropwise within 1 hour, heat to 120°C and stir to react for 6 hours; wait for the reaction product to cool to room temperature, stand for 2 hours, and take the upper liquid to obtain compound A;

[0040] S2, adding 1 mol of compound A to 1.3 mol of 1,6-dibromohexane, stirring and reacting at 110° C. for 8 h, and after the reaction, vacuum drying at 50° C. for 24 h to obtain compound B;

[0041] S3, adding 1 mol of compound B and 4.1 mol of potassium hydroxide to 1000 mL of anhydrous ethanol, stirring at room temperature for 36 hours, filtering, distilling the filtrate under reduced pressure to remove the solvent, washing and purifying with acetone, and vacuum drying at 80°C for 48 hours to obtain an auxiliary agent;

[0042] The molecular structure formula of the prepared additive is:

[0043]

[0044] Preparation Example 2

[0045] This preparation example provides an auxiliary agent, and the preparation method of the auxiliary agent is as follows:

[0046] S1. Mix 2.5 mol of dodecane bromide and 2.2 mol of sodium hydroxide evenly, and heat to 50°C to obtain a mixed solution 1; mix 1 mol of piperazine and 20 mol of water evenly, and heat to 80°C to obtain a mixed solution 2; add the mixed solution 2 dropwise to the mixed solution 1, and after the mixed solution 2 is added dropwise within 2 hours, heat to 130°C and stir to react for 8 hours; wait for the reaction product to cool to room temperature, stand for 4 hours, and take the upper liquid to obtain compound A;

[0047] S2, adding 1 mol of compound A to 1.3 mol of 1,4-dibromobutane, stirring and reacting at 120°C for 7 hours, and after the reaction, vacuum drying at 60°C for 24 hours to obtain compound B;

[0048] S3, add 1 mol of compound B and 4.3 mol of potassium hydroxide to 1000 mL of anhydrous ethanol, stir and react at room temperature for 48 hours, filter, distill the filtrate under reduced pressure to remove the solvent, wash and purify with acetone, and vacuum dry at 80°C for 48 hours to obtain an auxiliary agent;

[0049] The molecular structure formula of the prepared additive is:

[0050]

[0051] Comparative Preparation Example 1

[0052] This comparative preparation example provides an auxiliary agent, and the preparation method of the auxiliary agent is as follows:

[0053] S1. Mix 2 mol of octane bromide and 2.1 mol of sodium hydroxide evenly, and heat to 40°C to obtain a mixed solution 1; mix 1 mol of piperazine and 20 mol of water evenly, and heat to 70°C to obtain a mixed solution 2; add the mixed solution 2 dropwise to the mixed solution 1, and after the mixed solution 2 is added dropwise within 1 hour, heat to 120°C and stir to react for 6 hours; wait for the reaction product to cool to room temperature, stand for 2 hours, and take the upper liquid to obtain compound A;

[0054] S2, adding 1 mol of compound A to 0.7 mol of bromohexane, stirring and reacting at 110° C. for 8 h, and after the reaction, vacuum drying at 50° C. for 24 h to obtain compound B;

[0055] S3, adding 1 mol of compound B and 2.1 mol of potassium hydroxide to 1000 mL of anhydrous ethanol, stirring at room temperature for 36 hours, filtering, distilling the filtrate under reduced pressure to remove the solvent, washing and purifying with acetone, and vacuum drying at 80°C for 48 hours to obtain an auxiliary agent;

[0056] The molecular structure formula of the prepared additive is:

[0057]

[0058] Example 1

[0059] The present embodiment provides a photoresist stripping solution with a high recovery rate, which comprises the following components by mass percentage: 72.4% of diethylene glycol monomethyl ether, 24% of N-methylformamide, 1.5% of methyldiethanolamine, 1.0% of hydroxyethylethylenediamine, 0.1% of toluenetriazole, and 1% of an auxiliary agent;

[0060] The auxiliary agent is the auxiliary agent prepared in Preparation Example 1.

[0061] Example 2

[0062] This embodiment provides a photoresist stripping solution with a high recovery rate, which includes the following components by mass percentage: 76.4% of diethylene glycol monomethyl ether, 20% of N-methylformamide, 1.5% of methyldiethanolamine, 1.0% of diglycolamine, 0.1% of 5-aminotetrazole, and 1% of an auxiliary agent;

[0063] The auxiliary agent is the auxiliary agent prepared in Preparation Example 1.

[0064] Example 3

[0065] The present embodiment provides a photoresist stripping solution with a high recovery rate, which comprises the following components by mass percentage: 61.4% of diethylene glycol monomethyl ether, 34.0% of N-methylpyrrolidone, 2.5% of diethanolamine, 1.5% of methyldiethanolamine, 0.08% of methylbenzotriazole, 0.02% of gallic acid, and 0.5% of an auxiliary agent;

[0066] The auxiliary agent is the auxiliary agent prepared in Preparation Example 1.

[0067] Example 4

[0068] The present embodiment provides a photoresist stripping solution with a high recovery rate, which comprises the following components by mass percentage: 50.4% of diethylene glycol monobutyl ether, 46.5% of N-methylpyrrolidone, 1.0% of diethanolamine, 1.0% of diglycolamine, 0.08% of benzotriazole, 0.02% of gallic acid, and 1% of an auxiliary agent;

[0069] Among them, the auxiliary agent adopts the auxiliary agent prepared in Preparation Example 2.

[0070] Example 5

[0071] The present embodiment provides a photoresist stripping solution with a high recovery rate, which comprises the following components by mass percentage: 67.2% of diethylene glycol monomethyl ether, 27.5% of N-methylformamide, 2.0% of methyldiethanolamine, 3.0% of ethylene glycolamine, 0.15% of methylbenzotriazole, 0.05% of catechin, and 0.1% of an auxiliary agent;

[0072] The auxiliary agent is the auxiliary agent prepared in Preparation Example 2.

[0073] Example 6

[0074] This embodiment provides a photoresist stripping solution with a high recovery rate, which includes the following components by mass percentage: 73% of diethylene glycol monomethyl ether, 24% of N-methylformamide, 1.5% of methyldiethanolamine, 1.0% of hydroxyethylethylenediamine, 0.01% of tannic acid, and 0.49% of an additive;

[0075] The auxiliary agent is the auxiliary agent prepared in Preparation Example 1.

[0076] Example 7

[0077] The present embodiment provides a photoresist stripping solution with a high recovery rate, which comprises the following components by mass percentage: 70% of diethylene glycol monomethyl ether, 24% of N-methylformamide, 3.0% of methyldiethanolamine, 2.0% of hydroxyethylethylenediamine, 0.1% of toluenetriazole, and 0.9% of an auxiliary agent;

[0078] The auxiliary agent is the auxiliary agent prepared in Preparation Example 1.

[0079] Comparative Example 1

[0080] This comparative example provides a photoresist stripping solution, which is different from Example 1 only in that an equal mass of piperazine is used to replace the auxiliary agent, as follows:

[0081] The photoresist stripping solution comprises the following components in percentage by mass: 72.4% of diethylene glycol monomethyl ether, 24% of N-methylformamide, 1.5% of methyldiethanolamine, 1.0% of hydroxyethylethylenediamine, 0.1% of toluenetriazole and 1% of piperazine.

[0082] Comparative Example 2

[0083] This comparative example provides a photoresist stripping solution, which is different from Example 1 only in that an auxiliary agent (the auxiliary agent prepared in Comparative Preparation Example 1) of equal mass is used to replace the auxiliary agent (the auxiliary agent prepared in Preparation Example 1), as follows:

[0084] The photoresist stripping solution comprises the following components by weight percentage: 72.4% of diethylene glycol monomethyl ether, 24% of N-methylformamide, 1.5% of methyldiethanolamine, 1.0% of hydroxyethylethylenediamine, 0.1% of toluenetriazole, and 1% of an auxiliary agent;

[0085] The auxiliary agent is the auxiliary agent prepared in Comparative Preparation Example 1.

[0086] Comparative Example 3

[0087] This comparative example provides a photoresist stripping solution, which comprises the following components in percentage by mass: 35.5% of diethylene glycol monobutyl ether, 34% of N-methylformamide, 17% of diisopropylamine, 13% of ethylenediamine, and 0.5% of tolutriazole.

[0088] Comparative Example 4

[0089] This comparative example provides a photoresist stripping solution, which comprises the following components in percentage by mass: 34.5% of diethylene glycol monomethyl ether, 30% of N-methylpyrrolidone, 15% of diethanolamine, 20% of n-butylamine, and 0.5% of benzotriazole.

[0090] Performance Testing

[0091] The photoresist stripping solution prepared in the embodiment and the comparative example was used to treat the substrate containing the photoresist, and the stripping effect of the stripped substrate was evaluated. The relevant experimental process and evaluation parameters are as follows:

[0092] Stripping method: At 60° C., a substrate sample containing photoresist is immersed in the photoresist stripping solution prepared in the embodiments of the present invention and the comparative example for stripping for 120 seconds, then rinsed with ultrapure water for 1 minute, and finally dried with high-purity nitrogen to prepare a sample after stripping with the photoresist stripping solution.

[0093] Stripping effect: After the photoresist stripping liquid is stripped, the sample is cleaned, and after cleaning, the plane is observed using OM and the cross-section is observed using SEM. OM is used to check whether there is any photoresist residue, and SEM is used to check the corrosion of the metal material. Stripping evaluation: ○: good stripping property, Δ: relatively good stripping property, ×: average stripping property; Corrosion evaluation: A: the metal layer is not corroded, B: the metal layer is slightly corroded, C: the metal layer is corroded; the specific results are shown in Table 1.

[0094] Recovery effect: The used photoresist stripping solution was subjected to rotary evaporation, and the ratio of the rotary evaporation mass to the initial solvent mass was the solvent recovery rate; recovery effect evaluation: X: recovery rate ≥ 90%, Y: 70% ≤ recovery rate < 90%, Z: recovery rate < 70%; the specific results are shown in Table 2.

[0095] The OM and SEM images of the sample were collected during the photoresist stripping process. The results are as follows: Figure 1-6 As shown, Figure 1 OM image and cross-sectional SEM image of the original substrate sample (A is the planar OM image of the original substrate sample; B is the cross-sectional SEM image of the original substrate sample); Figure 2 The OM image and cross-sectional SEM image of the sample after stripping using the photoresist stripping solution of Example 1 (A is the planar OM image of the sample after stripping in Example 1; B is the cross-sectional SEM image of the sample after stripping in Example 1); Figure 3 The OM image and cross-sectional SEM image of the sample after stripping using the photoresist stripping solution of Comparative Example 1 (A is the planar OM image of the sample after stripping in Comparative Example 1; B is the cross-sectional SEM image of the sample after stripping in Comparative Example 1); Figure 4 The OM image and cross-sectional SEM image of the sample after stripping using the photoresist stripping solution of Comparative Example 2 (A is the planar OM image of the sample after stripping in Comparative Example 2; B is the cross-sectional SEM image of the sample after stripping in Comparative Example 2); Figure 5 The OM image and cross-sectional SEM image of the sample after stripping using the photoresist stripping solution of Comparative Example 3 (A is the planar OM image of the sample after stripping of Comparative Example 3; B is the cross-sectional SEM image of the sample after stripping of Comparative Example 3); Figure 6 These are the OM images and cross-sectional SEM images of the sample after stripping using the photoresist stripping solution of Comparative Example 4 (A is the planar OM image of the sample after stripping using Comparative Example 4; B is the cross-sectional SEM image of the sample after stripping using Comparative Example 4).

[0096] Table 1 Evaluation of the stripping effect of the photoresist stripping solution prepared in the examples and comparative examples

[0097]

[0098] Table 2 Recovery rate and recovery effect evaluation of the photoresist stripping solution prepared in the examples and comparative examples

[0099] Initial mass / g Solvent mass / g Rotation mass / g Recovery rate / % Evaluation of recycling effect Example 1 100 96.4 91.5 94.9 X Example 2 100 96.4 93.6 97.1 X Example 3 100 95.4 93.8 98.3 X Example 4 100 96.5 92.5 95.9 X Example 5 100 94.7 91.1 96.2 X Example 6 100 97.0 93.7 96.6 X Example 7 100 94.0 91.9 97.8 X Comparative Example 1 100 96.4 76.3 79.1 Y Comparative Example 2 100 96.4 82.4 85.5 Y Comparative Example 3 100 69.5 45.8 65.9 Z Comparative Example 4 100 64.5 41.7 64.7 Z

[0100] From Table 1, Table 2 and Figure 1-6 It can be seen that the stripping performance of the photoresist stripping solution of Examples 1-7 is significantly better than that of Comparative Examples 1-4, and the recovery rate of the stripping solution is higher.

[0101] According to the relevant data of Example 1 and Comparative Example 1 in Table 1 and Table 2, and combined with Figure 1-3 It can be seen that Example 1 adopts the auxiliary agent prepared in Preparation Example 1 of the present invention. Compared with the piperazine used in Comparative Example 1, the stripping solution prepared in Example 1 can not only obtain a good stripping effect, but also has less corrosiveness to the metal film layer, which fully demonstrates that the bipiperazine ring is better than the monopiperazine ring in dissolving the photoresist. While stripping the photoresist, the bipiperazine ring can be quickly adsorbed on the surface of the substrate to prevent the substrate from being corroded.

[0102] According to the relevant data of Example 1 and Comparative Example 2 in Table 1 and Table 2, and combined with Figure 1 , 2 4 It can be seen that the stripping effect and anti-corrosion effect of the stripping solution prepared in Example 1 using the auxiliary agent prepared in Preparation Example 1 of the present invention are better than those in Comparative Example 2 using the auxiliary agent prepared in Comparative Preparation Example 1 of the present invention; it fully demonstrates that the tetra-nuclear alkaline ionic liquid is better than the binuclear alkaline ionic liquid. The tetra-nuclear alkaline ionic liquid greatly improves the interaction between the stripping solution and the photoresist, helps to remove the photoresist, reduces the damage to the substrate, and protects the copper-molybdenum layer to a certain extent.

[0103] According to the relevant data of Example 1 and Comparative Examples 3 and 4 in Table 1 and Table 2, and combined with Figure 1 , 2 , 5, and 6 show that Example 1 uses the auxiliary agent prepared in Preparation Example 1 of the present invention. Compared with Comparative Examples 3 and 4 in which no auxiliary agent is added, which is the formula of the existing photoresist stripping solution, the formula of Example 1 is significantly better than the existing formula. Not only is the stripping effect significant, but the recovery rate of the polar organic solvent is high, which fully demonstrates that the auxiliary agent of the present invention can reduce the amount of organic base used and reduce the occurrence of complex chemical reactions, but will not affect the stripping effect of the stripping solution. At the same time, it can increase the amount of polar organic solvent used and improve the recovery rate of the stripping solution.

[0104] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0105] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A photoresist stripping solution with high recovery rate, characterized in that: According to the mass percentage, it includes: 94-97% polar organic solvent, 2-5% organic base, 0.01-0.2% corrosion inhibitor, and 0.1-1% additive; The auxiliary agent has a structure shown in formula (I): Wherein, n is any integer between 8 and 12, and m is any integer between 4 and 8.

2. The photoresist stripping solution with high recovery rate according to claim 1, characterized in that: The preparation method of the auxiliary agent comprises the following steps: S1. Evenly mix bromoalkane and sodium hydroxide, and heat to 40-50°C to obtain a mixed solution 1; evenly mix piperazine and water, and heat to 70-80°C to obtain a mixed solution 2; dropwise add the mixed solution 2 to the mixed solution 1, and after the addition of the mixed solution 2 is completed within 1-2 hours, heat to 120-130°C and stir to react for 6-8 hours; wait for the reaction product to cool to room temperature, stand for 2-4 hours, and take the upper layer of liquid to obtain compound A; S2, adding compound A to dibromoalkane, stirring and reacting at 110-120° C. for 7-8 hours, and after the reaction, vacuum drying at 50-60° C. for 24 hours to obtain compound B; S3. Add compound B and potassium hydroxide to anhydrous ethanol, stir and react at room temperature for 36-48 hours, filter, distill the filtrate under reduced pressure to remove the solvent, wash and purify with acetone, and vacuum dry at 80°C for 48 hours to obtain an auxiliary agent.

3. The photoresist stripping solution with high recovery rate according to claim 2, characterized in that: In step S1, the brominated alkane is any one of brominated octane, brominated nonane, brominated decane, brominated undecane, and brominated dodecane; In step S2, the dibromoalkane is any one of 1,4-dibromobutane, 1,5-dibromopentane, 1,6-dibromohexane, 1,7-dibromoheptane and 1,8-dibromooctane.

4. The photoresist stripping solution with high recovery rate according to claim 2, characterized in that: In step S1, the molar ratio of the bromoalkane, piperazine, sodium hydroxide and water is (2-2.5):1:(2.1-2.2):20; In step S2, the molar ratio of compound A to dibromoalkane is 1:(1-1.3); In step S3, the molar ratio of compound B to potassium hydroxide is 1:(4.1-4.3).

5. The photoresist stripping solution with high recovery rate according to claim 2, characterized in that: The reaction formula of the preparation method of the auxiliary agent is as follows:

6. The photoresist stripping solution with high recovery rate according to claim 1, characterized in that: The polar organic solvent is any one of N-methylformamide, N-methylpyrrolidone, N,N-dimethylformamide, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, and diethylene glycol monobutyl ether, or a combination of two or more thereof.

7. The photoresist stripping solution with high recovery rate according to claim 1, characterized in that: The organic base is any one of diglycolamine, ethylene glycolamine, diethanolamine, triethanolamine, methyldiethanolamine, and hydroxyethylethylenediamine, or a combination of two or more thereof.

8. The photoresist stripping solution with high recovery rate according to claim 1, characterized in that: The corrosion inhibitor is a nitrogen azole compound and / or an organic polyphenol compound.

9. A photoresist stripping solution with high recovery rate according to claim 8, characterized in that: The azole compound is any one of tolyltriazole, benzotriazole, and 5-aminotetrazole, or a combination of two or more thereof.

10. The photoresist stripping solution with high recovery rate according to claim 8, characterized in that: The organic polyphenol compound is any one of catechin, gallic acid, tannic acid and pyrogallol or a combination of more than one thereof.

Citation Information

Cited By

  • Photoresist stripping liquid for OLED (Organic Light Emitting Diode) as well as preparation method and application of photoresist stripping liquid

    CN121500699A

  • A photoresist stripping solution for OLEDs, and a preparation method and application thereof

    CN121500699B