Nitrogen-containing group-containing phosphine phenol nickel catalyst as well as preparation method and application thereof

By introducing nitrogen-containing groups into nickel catalysts and increasing the steric hindrance, the problem of insufficient catalytic activity and heat resistance stability of nickel catalysts in polar solvents is solved, and a polyolefin material with high molecular weight and high thermal stability is achieved Production.

CN119060090APending Publication Date: 2024-12-03UNIV OF SCI & TECH OF CHINA
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310631828.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-31
Publication Date
2024-12-03

AI Technical Summary

Technical Problem

The catalytic activity of existing nickel catalysts in polar solvents is limited, and it is difficult to balance the catalytic activity and heat resistance of the catalyst, resulting in insufficient molecular weight and thermal stability of the polyolefin material.

Method used

A phosphine phenol nickel catalyst containing nitrogen-containing groups was designed. By introducing phosphine phenol groups and nitrogen-containing groups, the steric hindrance of the catalyst is increased, the polymerization performance of the transition metal salt catalyst is optimized, and the elimination of β-H is inhibited. to improve the molecular weight and thermal stability of the polyolefin material.

Benefits of technology

The thermal stability of the catalyst and the molecular weight of the polyolefin material are significantly improved, and the balance between high catalytic activity and high thermal stability is achieved, which promotes the development of polyolefin materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004258619230000021
    Figure BDA0004258619230000021
  • Figure BDA0004258619230000022
    Figure BDA0004258619230000022
  • Figure BDA0004258619230000023
    Figure BDA0004258619230000023
Patent Text Reader

Abstract

The invention provides a phosphine-phenol compound containing a nitrogen-containing group, a phosphine-phenol nickel catalyst containing the nitrogen-containing group, and a preparation method and application of the phosphine-phenol compound and the phosphine-phenol nickel catalyst. The catalyst provided by the invention is a catalyst with a structure as shown in a formula (II), a phosphorus-containing ligand and a nitrogen-containing group are connected to obtain a phosphine-phenol compound containing the nitrogen-containing group, and the phosphine-phenol compound is coordinated with nickel salt to obtain the novel phosphine-phenol nickel catalyst containing the nitrogen-containing group. The prepared catalyst has good catalytic activity and thermal stability when applied to olefin polymerization reaction, and is suitable for a polymerization reaction system with polar monomers.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure belongs to the field of catalyst technology, and in particular relates to a phosphine phenol nickel catalyst containing a nitrogen-containing group and a preparation method and application thereof. Background Art

[0002] Polyolefin materials are a type of polymer material with the largest output and widest application. Among them, with the development of petrochemical industry, the production of polyethylene materials has developed rapidly, and its output can reach 1 / 4 of the total plastic output. Therefore, the research on polyolefin materials has far-reaching significance for optimizing industrial performance and developing the application of polymer materials.

[0003] The development of new catalysts is crucial for the development of high-performance polyolefin materials. In recent years, late transition metal catalysts such as nickel and palladium have been widely developed and used in academia to study the copolymerization of olefins and polar monomers due to their low hydrophilicity and high tolerance to polar groups. Among them, nickel catalysts are considered to have greater economic and environmental advantages and industrialization potential. Therefore, a series of nickel catalysts with different ligand structures continue to emerge, and representative nickel catalysts such as α-diimine nickel catalysts, α-iminoketone nickel catalysts and salicylaldehyde imine nickel catalysts have been widely studied.

[0004] In the related art, the catalytic activity of nickel-based catalysts for catalyzing polyolefins in polar solvents is limited, and it is difficult to balance the catalytic activity and thermal stability of the catalyst. Therefore, developing a catalyst with a new structure for olefin homopolymerization and copolymerization with polar monomers to ensure high thermal stability, high catalytic activity and olefin molecular weight is one of the keys to promote the development of polyolefins. Summary of the invention

[0005] In view of this, in order to solve at least one of the technical problems described above and in other aspects of the related art, the present disclosure proposes a phosphine phenol nickel catalyst containing a nitrogen-containing group and its preparation method and application, and designs and synthesizes a new structural catalyst with aromatic hydrocarbons as the main body, introducing phosphine phenol groups and nitrogen-containing groups, and improving the catalyst stability and polyolefin catalytic activity and molecular weight by increasing steric hindrance.

[0006] In one aspect of the present disclosure, a phosphinophenol compound containing a nitrogen-containing group is provided, and its structure is shown in formula (I),

[0007]

[0008] Among them, R 1 ~R 3 is independently selected from hydrogen, halogen, hydroxyl, substituted or unsubstituted C1-C20 alkyl, R 1 ~R 3 Any two adjacent ones of can form a loop with each other;

[0009] R 4 and R 5 is independently selected from one of hydrogen, C1-C20 alkyl, C6-C20 aryl, or R 4 and R 5 They are cyclically connected to form one of an oxygen-containing heterocycle, a nitrogen-containing heterocycle, and a sulfur-containing heterocycle;

[0010] R 6 Independently selected from substituted or unsubstituted C1-C20 alkyl, C5-C20 cycloalkyl, C6-C20 aryl;

[0011] When the above substituted or unsubstituted group has a substituent, the substituent is selected from one of phenyl and halogen.

[0012] According to the embodiment of the present disclosure, R 1 ~R 3 are respectively selected from hydrogen; preferably, R 4 , R 5 are selected from methyl, or R 4 , R 5 Form a morpholinyl group or a carbazole group; preferably, R 6 Selected from phenyl.

[0013] According to the embodiment of the present disclosure, its structural formula is shown in any one of the following formulas (I-1) to (I-3):

[0014]

[0015] In another aspect of the present disclosure, a phosphine phenol nickel catalyst containing a nitrogen-containing group is provided, and its structure is shown in formula (II),

[0016]

[0017] Among them, R 1 ~R 3 is independently selected from hydrogen, halogen, hydroxyl, substituted or unsubstituted C1-C20 alkyl, R 1 ~R 3 Any two adjacent ones of can form a loop with each other;

[0018] R 4 and R 5 is independently selected from one of hydrogen, C1-C20 alkyl, C6-C20 aryl, or R 4 and R 5 They are cyclically connected to form one of an oxygen-containing heterocycle, a nitrogen-containing heterocycle, and a sulfur-containing heterocycle;

[0019] R 6Independently selected from substituted or unsubstituted C1-C20 alkyl, C5-C20 cycloalkyl, C6-C20 aryl;

[0020] R 7 and R 8 is independently selected from one of hydrogen, halogen, C1-C20 alkyl, C6-C20 aryl, and pyridyl;

[0021] When the above substituted or unsubstituted group has a substituent, the substituent is selected from benzene and halogen.

[0022] According to the embodiment of the present disclosure, R 1 ~R 3 are respectively selected from hydrogen; preferably, R 4 , R 5 are selected from methyl, or R 4 , R 5 Form a morpholinyl group or a carbazole group; preferably, R 6 is selected from phenyl; preferably, R 7 , R 8 are respectively selected from pyridyl or methyl.

[0023] According to the embodiment of the present disclosure, its structural formula is shown in any one of the following formulas (II-1) to (II-3):

[0024]

[0025] In another aspect of the present disclosure, a method for preparing the above-mentioned phosphine phenol nickel catalyst containing a nitrogen-containing group is provided, comprising:

[0026] In an atmosphere of nitrogen or argon, reacting a compound of formula (A), butyl lithium and a compound of formula (B) to obtain a phosphine phenol compound containing a nitrogen-containing group as shown in formula (I);

[0027]

[0028] A solution of a phosphinophenol compound containing a nitrogen-containing group is added dropwise to a nickel salt solution, and after reacting at room temperature for 1 to 12 hours, a phosphinophenol nickel catalyst containing a nitrogen-containing group as shown in formula (II) is obtained, wherein the molar ratio of the phosphinophenol compound containing a nitrogen-containing group to the nickel salt is 1:1.5 to 1:5.

[0029] According to an embodiment of the present disclosure, reacting a compound of formula (A) with butyl lithium and a compound of formula (B) comprises:

[0030] The compound of formula (A) undergoes a substitution reaction with dihydropyran to obtain a compound of formula (A');

[0031] After reacting a compound of formula (A') with butyl lithium, a compound of formula (B) is added to the obtained reaction solution to obtain a phosphine phenol compound containing a nitrogen-containing group protected by dihydropyran as shown in formula (C);

[0032] Removing the dihydropyran protecting group of the compound shown in formula (C) to obtain a phosphine phenol compound containing a nitrogen-containing group as shown in formula (I),

[0033]

[0034] In another aspect of the present disclosure, a method for preparing polyethylene using the above-mentioned nickel phosphine phenolate catalyst containing nitrogen-containing groups is provided, comprising: injecting a liquid nickel phosphine phenolate catalyst containing nitrogen-containing groups into ethylene in a protective gas atmosphere, reacting for 0.1 to 20 hours under the conditions of 30 to 150° C. and 8 to 30 MPa to obtain polyethylene;

[0035] Preferably, injecting a phosphine phenol nickel catalyst liquid containing a nitrogen-containing group into ethylene comprises: mixing and dissolving the phosphine phenol nickel catalyst containing a nitrogen-containing group and a metal Lewis acid in a molar ratio of 1:0.5 to 1:5 to obtain a catalyst mixed liquid, and injecting the catalyst mixed liquid into ethylene, wherein the metal Lewis acid comprises one of zinc acetate, N,N,N',N'-tetramethylethylenediamine zinc acetate, and nickel acetate.

[0036] In another aspect of the present disclosure, a method for preparing polyethylene modified with a polar monomer using the above-mentioned nickel phosphine phenolate catalyst containing a nitrogen-containing group is provided, comprising: in a protective gas atmosphere, ethylene, a polar monomer and the nickel phosphine phenolate catalyst containing a nitrogen-containing group are mixed and dissolved, and reacted at 30 to 150° C. and 8 to 30 MPa for 0.1 to 20 hours to obtain polyethylene modified with a polar monomer;

[0037] Wherein, the polar monomer includes at least one of methyl acrylate, tert-butyl acrylate, methyl 10-undecenoate and 10-undecenol;

[0038] The molar ratio of the polar monomer to the phosphine phenol nickel catalyst containing a nitrogen-containing group ranges from 1:100 to 1:5000. According to the embodiment of the present disclosure, the phosphorus-containing ligand and the nitrogen-containing group are connected to obtain a phosphine phenol compound containing a nitrogen-containing group, and after coordination with a nickel salt, a new type of phosphine phenol nickel catalyst containing a nitrogen-containing group is obtained. The introduction of the nitrogen-containing group increases the steric hindrance of the catalyst, optimizes the polymerization performance of the transition metal salt catalyst, and effectively inhibits the elimination of β-H to produce a high molecular weight polyolefin material. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 is the hydrogen nuclear magnetic resonance spectrum of the compound prepared in Example 1 of the present disclosure;

[0040] Figure 2 is the nuclear magnetic resonance phosphorus spectrum of the compound prepared in Example 1 of the present disclosure;

[0041] Figure 3 is the carbon nuclear magnetic resonance spectrum of the compound prepared in Example 1 of the present disclosure;

[0042] Figure 4 is an electrospray ionization mass spectrum (ESI-MS) of the compound prepared in Example 1 of the present disclosure;

[0043] Figure 5 is the hydrogen nuclear magnetic resonance spectrum of the compound prepared in Example 2 of the present disclosure;

[0044] Figure 6 is the nuclear magnetic resonance phosphorus spectrum of the compound prepared in Example 2 of the present disclosure;

[0045] Figure 7 is the carbon nuclear magnetic resonance spectrum of the compound prepared in Example 2 of the present disclosure;

[0046] Figure 8 is an electrospray ionization mass spectrum (ESI-MS) of the compound prepared in Example 2 of the present disclosure;

[0047] Fig. 9 is the hydrogen nuclear magnetic resonance spectrum of the compound prepared in Example 3 of the present disclosure;

[0048] Fig.10 is the nuclear magnetic resonance phosphorus spectrum of the compound prepared in Example 3 of the present disclosure;

[0049] Fig.11 is the carbon nuclear magnetic resonance spectrum of the compound prepared in Example 3 of the present disclosure;

[0050] Fig.12 is an electrospray ionization mass spectrum (ESI-MS) of the compound prepared in Example 3 of the present disclosure;

[0051] Fig.13 is the hydrogen nuclear magnetic resonance spectrum of the catalyst prepared in Example 4 of the present disclosure;

[0052] Fig.14 is the nuclear magnetic resonance phosphorus spectrum of the catalyst prepared in Example 4 of the present disclosure;

[0053] Fig.15 is the carbon nuclear magnetic resonance spectrum of the catalyst prepared in Example 4 of the present disclosure;

[0054] Fig.16 is the hydrogen nuclear magnetic resonance spectrum of the catalyst prepared in Example 5 of the present disclosure;

[0055] Fig.17is the nuclear magnetic resonance phosphorus spectrum of the catalyst prepared in Example 5 of the present disclosure;

[0056] Fig.18 is the carbon nuclear magnetic resonance spectrum of the catalyst prepared in Example 5 of the present disclosure;

[0057] Fig.19 is the hydrogen nuclear magnetic resonance spectrum of the catalyst prepared in Example 6 of the present disclosure;

[0058] Fig. 20 is the nuclear magnetic resonance phosphorus spectrum of the catalyst prepared in Example 6 of the present disclosure;

[0059] Fig.21 It is the carbon nuclear magnetic resonance spectrum of the catalyst prepared in Example 6 of the present disclosure. DETAILED DESCRIPTION

[0060] In order to make the objectives, technical solutions and advantages of the present disclosure more clearly understood, the present disclosure is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings.

[0061] The endpoints and any values ​​of the ranges disclosed in this disclosure are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, and these numerical ranges should be regarded as specifically disclosed in this disclosure.

[0062] The terms used herein are only for describing specific embodiments and are not intended to limit the present disclosure. The terms "comprise", "include", etc. used herein indicate the existence of the features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.

[0063] All terms (including technical and scientific terms) used herein have the meanings commonly understood by those skilled in the art, unless otherwise defined. It should be noted that the terms used herein should be interpreted as having a meaning consistent with the context of this specification, and should not be interpreted in an idealized or overly rigid manner.

[0064] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the present disclosure shall have the usual meanings understood by persons with ordinary skills in the field to which the present disclosure belongs. If the full text involves descriptions such as "first", "second", etc., the descriptions such as "first", "second", etc. are only used to distinguish similar objects, and cannot be understood as indicating or implying their relative importance, order of precedence, or implicitly indicating the number of technical features indicated. It should be understood that the data described by "first", "second", etc. can be interchangeable under appropriate circumstances.

[0065] The "metal saltization" strategy of introducing a metal source into the catalyst can improve the thermal stability and polymerization performance of the catalyst by appropriately increasing the steric hindrance of the metal salt catalyst molecule. Nickel phosphine phenolate catalyst is a type of late transition metal catalyst, which has good prospects in catalyzing olefin polymerization and synthesizing high molecular weight functionalized polyolefins with high polar monomer doping at low polar monomer concentrations. At the same time, nitrogen-containing groups can be mixed with other reagents to form a regulatory strategy to adjust the thermal stability, catalytic activity and molecular weight of the catalyst.

[0066] In one aspect of the present disclosure, a phosphinophenol compound containing a nitrogen-containing group is provided, and its structure is shown in formula (I),

[0067]

[0068] Among them, R 1 ~R 3 is independently selected from hydrogen, halogen, hydroxyl, substituted or unsubstituted C1-C20 alkyl, R 1 ~R 3 Any two adjacent ones of can form a loop with each other;

[0069] R 4 and R 5 is independently selected from one of hydrogen, C1-C20 alkyl, C6-C20 aryl, or R 4 and R 5 They are cyclically connected to form one of an oxygen-containing heterocycle, a nitrogen-containing heterocycle, and a sulfur-containing heterocycle;

[0070] R 6 Independently selected from substituted or unsubstituted C1-C20 alkyl, C5-C20 cycloalkyl, C6-C20 aryl;

[0071] When the above-mentioned substituted or unsubstituted group has a substituent, the substituent is selected from one of phenyl and halogen. According to the embodiment of the present disclosure, the phosphorus-containing ligand and the nitrogen-containing group are connected to obtain a phosphophenol compound containing a nitrogen-containing group, and after coordination with a nickel salt, a new type of phosphophenol nickel catalyst containing a nitrogen-containing group is obtained. The introduction of the nitrogen-containing group increases the steric hindrance of the catalyst, optimizes the polymerization performance of the transition metal salt catalyst, and effectively inhibits the elimination of β-H to produce a high molecular weight polyolefin material.

[0072] According to the embodiment of the present disclosure, R 1 ~R 3 are respectively selected from hydrogen; preferably, R 4 , R 5 are selected from methyl, or R 4 , R 5Form a morpholinyl group or a carbazole group; preferably, R 6 Selected from phenyl.

[0073] According to the embodiment of the present disclosure, its structural formula is shown in any one of the following formulas (I-1) to (I-3):

[0074]

[0075] In the embodiments of the present disclosure, phosphinophenol compounds containing nitrogen-containing groups with structural formulae (I-1) to (I-3) were synthesized and their structures were verified by nuclear magnetic resonance detection and mass spectrometry.

[0076] In another aspect of the present disclosure, a phosphine phenol nickel catalyst containing a nitrogen-containing group is provided, and its structure is shown in formula (II),

[0077]

[0078] Among them, R 1 ~R 3 is independently selected from hydrogen, halogen, hydroxyl, substituted or unsubstituted C1-C20 alkyl, R 1 ~R 3 Any two adjacent ones of can form a loop with each other;

[0079] R 4 and R 5 is independently selected from one of hydrogen, C1-C20 alkyl, C6-C20 aryl, or R 4 and R 5 They are cyclically connected to form one of an oxygen-containing heterocycle, a nitrogen-containing heterocycle, and a sulfur-containing heterocycle;

[0080] R 6 Independently selected from substituted or unsubstituted C1-C20 alkyl, C5-C20 cycloalkyl, C6-C20 aryl;

[0081] R 7 and R 8 is independently selected from one of hydrogen, halogen, C1-C20 alkyl, C6-C20 aryl, and pyridyl;

[0082] When the above substituted or unsubstituted group has a substituent, the substituent is selected from benzene and halogen.

[0083] According to the embodiment of the present disclosure, a phosphorus-containing ligand and a nitrogen-containing group are connected to obtain a phosphophenol compound containing a nitrogen-containing group, and after coordination with a nickel salt, a new type of phosphophenol nickel catalyst containing a nitrogen-containing group is obtained. The introduction of the nitrogen-containing group increases the steric hindrance of the catalyst, optimizes the polymerization performance of the transition metal salt catalyst, and effectively inhibits the elimination of β-H to produce a high molecular weight polyolefin material.

[0084] According to the embodiment of the present disclosure, R 1 ~R 3 are respectively selected from hydrogen; preferably, R 4 , R 5 are selected from methyl, or R 4 , R 5 Form a morpholinyl group or a carbazole group; preferably, R 6 Selected from phenyl; preferably, R7 and R8 are selected from pyridyl or methyl.

[0085] According to the embodiment of the present disclosure, its structural formula is shown in any one of the following formulas (II-1) to (II-3):

[0086]

[0087] In the embodiments of the present disclosure, phosphine phenol nickel catalysts containing nitrogen-containing groups with structural formulas such as formula (II-1) to (II-3) were synthesized and their structures were verified by nuclear magnetic resonance detection and mass spectrometry.

[0088] In another aspect of the present disclosure, a method for preparing the above catalyst is proposed, comprising:

[0089] In an atmosphere of nitrogen or argon, reacting a compound of formula (A), butyl lithium and a compound of formula (B) to obtain a phosphine phenol compound containing a nitrogen-containing group as shown in formula (I);

[0090]

[0091] A solution of a phosphinophenol compound containing a nitrogen-containing group is added dropwise to a nickel salt solution, and after reacting at room temperature for 1 to 12 hours, a phosphinophenol nickel catalyst containing a nitrogen-containing group as shown in formula (II) is obtained, wherein the molar ratio of the phosphinophenol compound containing a nitrogen-containing group to the nickel salt is 1:1.5 to 1:5.

[0092] According to an embodiment of the present disclosure, reacting a compound of formula (A) with butyl lithium and a compound of formula (B) comprises:

[0093] The compound of formula (A) undergoes a substitution reaction with dihydropyran to obtain a compound of formula (A');

[0094] After reacting a compound of formula (A') with butyl lithium, a compound of formula (B) is added to the obtained reaction solution to obtain a phosphine phenol compound containing a nitrogen-containing group protected by dihydropyran as shown in formula (C);

[0095] Removing the dihydropyran protecting group of the compound shown in formula (C) to obtain a phosphine phenol compound containing a nitrogen-containing group as shown in formula (I),

[0096]

[0097] In another aspect of the present disclosure, a method for preparing polyethylene using the above-mentioned phosphine phenol nickel catalyst containing nitrogen-containing groups is provided, comprising: injecting the above-mentioned phosphine phenol nickel catalyst liquid containing nitrogen-containing groups into ethylene in a protective gas atmosphere, and reacting for 0.1 to 20 hours under the conditions of 30 to 150° C. and 8 to 30 MPa to obtain polyethylene;

[0098] Preferably, injecting a phosphine phenol nickel catalyst liquid containing a nitrogen-containing group into ethylene comprises: mixing and dissolving the phosphine phenol nickel catalyst containing a nitrogen-containing group and a metal Lewis acid in a molar ratio of 1:0.5 to 1:5 to obtain a catalyst mixed liquid, and injecting the catalyst mixed liquid into ethylene, wherein the metal Lewis acid comprises one of zinc acetate, N,N,N',N'-tetramethylethylenediamine zinc acetate, and nickel acetate.

[0099] According to the embodiments of the present disclosure, Lewis acid can form coordination with nitrogen atoms in the phosphine phenol nickel catalyst containing nitrogen groups to increase steric hindrance, thereby significantly improving the structural rigidity, thermal stability and molecular weight of the polyolefin material of the phosphine phenol nickel catalyst containing nitrogen groups.

[0100] In another aspect of the present disclosure, a method for preparing polyethylene modified with a polar monomer using the above-mentioned phosphine phenol nickel catalyst containing a nitrogen-containing group is provided, comprising: in a protective gas atmosphere, ethylene, a polar monomer and the above-mentioned phosphine phenol nickel catalyst containing a nitrogen-containing group are mixed and dissolved, and reacted at 30 to 150° C. and 8 to 30 MPa for 0.1 to 20 hours to obtain polyethylene modified with a polar monomer;

[0101] Wherein, the polar monomer includes at least one of methyl acrylate, tert-butyl acrylate, methyl 10-undecenoate and 10-undecenol;

[0102] The molar ratio of the polar monomer to the phosphine phenol nickel catalyst containing a nitrogen-containing group ranges from 1:100 to 1:5000.

[0103] It should be noted that the described embodiments are only part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the embodiments of the present disclosure, other embodiments obtained by ordinary technicians in the field without creative work are all within the scope of protection of the present disclosure.

[0104] The following examples illustrate the specific content of the present disclosure, and the data provided include the synthesis of ligands, the synthesis of metal compounds, and the ethylene polymerization or copolymerization method, wherein the synthesis of the complex and the polymerization process are carried out under anhydrous and oxygen-free conditions, all sensitive substances are stored in a glove box, all solvents are strictly dried and dehydrated, and ethylene gas is purified by a dehydration and deoxygenation column. Unless otherwise specified, all compounds are commercially purchased and used in the present disclosure.

[0105] The nuclear magnetic resonance detection was performed by a Bruker 400 MHz nuclear magnetic resonance instrument, the molecular weight and molecular weight distribution were determined by high temperature gel permeation chromatography (GPC), and the mass spectrum was determined by a Thermo LTQ Orbitrap XL.

[0106] Example 1: Synthesis of Compound I-1

[0107] 50mmol of tert-butylphenol was reacted with 55mmol of dihydropyran, PTSA catalyst and an appropriate amount of dichloromethane solution at room temperature for 12h under stirring to obtain a product with a tetrahydropyran protective group. It was dissolved in 200mL of tetrahydrofuran, placed at 0°C, and 55mmol of n-BuLi was added dropwise. After reacting for 2h, 50mmol of a compound of formula (B-1) was added, and the temperature was slowly raised to room temperature, and the reaction was continued for 12h. Water was added to quench, and the organic phase was extracted with ether. The obtained organic phase was concentrated to 100mL and deoxygenated by freezing cycle. 10mL of concentrated hydrochloric acid was added under a nitrogen atmosphere, and the reaction was continued for 2h. NaHCO 3 The aqueous solution was neutralized, quenched with water, and the organic phase was extracted with ether and anhydrous MgSO 4 After drying, filtration and concentration, flash column chromatography was performed to obtain a white solid compound of formula (I-1).

[0108]

[0109] Compound I-1 was subjected to nuclear magnetic resonance detection to verify its specific structure, and electrospray ionization mass spectrometry was used to detect its structural multiply charged molecular ions to identify small molecule materials.

[0110] Figure 1 It is the hydrogen nuclear magnetic resonance spectrum of the compound prepared in Example 1 of the present disclosure.

[0111] like Figure 1 As shown, its hydrogen spectrum data is: 1 H NMR (400 MHz, CDCl 3)δ7.68(s,1H),7.43–7.28(m,6H),7.23–7.15(m,1H),7.11(s,2H),6.91(s,1H),6.76(t,J=7.5Hz,1H),2.54(s,6H),1.42(s,9H).

[0112] Figure 2 It is the nuclear magnetic resonance phosphorus spectrum of the compound prepared in Example 1 of the present disclosure.

[0113] like Figure 2 As shown, its phosphorus spectrum data is: 31 PNMR (162MHz,CDCl3)δ-41.48.

[0114] Figure 3 It is the carbon nuclear magnetic resonance spectrum of the compound prepared in Example 1 of the present disclosure.

[0115] like Figure 3 As shown, its carbon spectrum data is: 13 C NMR (101 MHz, CDCl 3 )δ157.61,157.40,132.15,131.98,128.97,127.29,127.22,127.18,127.04, 121.19,120.40,120.37,118.90,118.89,76.30,75.98,75.67,44.34,44.31.

[0116] Figure 4 is an electrospray ionization mass spectrum (ESI-MS) of the compound prepared in Example 1 of the present disclosure;

[0117] like Figure 4 As shown, its electrospray mass spectrometry data is: ESI-MS (m / z): 378.19809 [M+H] + .

[0118] Example 2: Synthesis of Compound I-2

[0119] 50mmol of tert-butylphenol was reacted with 55mmol of dihydropyran, PTSA catalyst and an appropriate amount of dichloromethane solution at room temperature for 12h under stirring to obtain a product with a tetrahydropyran protective group. It was dissolved in 200mL of tetrahydrofuran, placed at 0°C, and 55mmol of n-BuLi was added dropwise. After reacting for 2h, 50mmol of a compound of formula (B-2) was added, and the temperature was slowly raised to room temperature, and the reaction was continued for 12h. Water was added to quench, and the organic phase was extracted with ether. The obtained organic phase was concentrated to 100mL and deoxygenated by freezing cycle. 10mL of concentrated hydrochloric acid was added under a nitrogen atmosphere, and the reaction was continued for 2h. NaHCO 3The aqueous solution was neutralized, quenched with water, and the organic phase was extracted with ether and anhydrous MgSO 4 After drying, filtration and concentration, flash column chromatography was performed to obtain a white solid compound of formula (I-2).

[0120]

[0121] Figure 5 It is the hydrogen nuclear magnetic resonance spectrum of the compound prepared in Example 2 of the present disclosure.

[0122] like Figure 5 As shown, its hydrogen spectrum data is: 1 H NMR (400MHz, CDCl3) δ7.47–7.34(m,7H),7.31(dd,J=7.5,1.8Hz,1H),7.22(m,J=7.8,4.7,0.9Hz,1H),7.12(t,J=7.5Hz,1H),6. 94(m,J=7.6,4.7,1.5Hz,1H),6.87–6.75(m,2H),3.59(t,J=4.4Hz,4H),2.97–2.84(m,2H),2.63(d,J=10.5Hz,2H),1.46(s,9H).

[0123] Figure 6 It is the nuclear magnetic resonance phosphorus spectrum of the compound prepared in Example 2 of the present disclosure.

[0124] like Figure 6 As shown, its phosphorus spectrum data is: 31 PNMR (162MHz,CDCl3)δ-41.83.

[0125] Figure 7 It is the carbon nuclear magnetic resonance spectrum of the compound prepared in Example 2 of the present disclosure.

[0126] like Figure 7 As shown, its carbon spectrum data is: 13 C NMR (101 MHz, CDCl 3 )δ158.27,158.06,155.19,155.03,135.95,133.85,133.66,133.06,132.46,130.18,128.77,128.60,128.5 3,125.98,125.96,122.43,122.41,120.14,120.11,77.40,77.08,76.76,67.19,52.82,34.98,34.96,29.62.

[0127] Figure 8is an electrospray ionization mass spectrum (ESI-MS) of the compound prepared in Example 2 of the present disclosure.

[0128] like Figure 8 As shown, its electrospray mass spectrometry data is: ESI-MS (m / z): 420.20844 [M+H] + .

[0129] Example 3: Synthesis of Compound I-3

[0130] 50mmol of tert-butylphenol was reacted with 55mmol of dihydropyran, PTSA catalyst and an appropriate amount of dichloromethane solution at room temperature for 12h under stirring to obtain a product with a tetrahydropyran protective group. It was dissolved in 200mL of tetrahydrofuran, placed at 0°C, and 55mmol of n-BuLi was added dropwise. After reacting for 2h, 50mmol of a compound of formula (B-3) was added, and the temperature was slowly raised to room temperature, and the reaction was continued for 12h. Water was added to quench, and the organic phase was extracted with ether. The obtained organic phase was concentrated to 100mL and deoxygenated by freezing cycle. 10mL of concentrated hydrochloric acid was added under a nitrogen atmosphere, and the reaction was continued for 2h. NaHCO 3 The aqueous solution was neutralized, quenched with water, and the organic phase was extracted with ether and anhydrous MgSO 4 After drying, filtration and concentration, flash column chromatography was performed to obtain a white solid compound of formula (I-3).

[0131]

[0132] Fig. 9 It is the hydrogen nuclear magnetic resonance spectrum of the compound prepared in Example 3 of the present disclosure.

[0133] like Fig. 9 As shown, its hydrogen spectrum data is: 1 H NMR (400 MHz, CDCl 3 )δ8.03(dd,J=17.7,7.5Hz,2H),7.57(d,J=7.5Hz,1H),7.50(s,1H),7.38(d,J=16.1Hz,2H),7.31(s,1H),7.26–7.20(m,4H),7. 20–7.10(m,5H),7.04(d,J=8.1Hz,1H),6.88(dd,J=6.8,5.7Hz,1H),6.73(t,J=7.6Hz,1H),6.64(d,J=8.0Hz,1H),1.19(s,9H).

[0134] Fig.10 It is the nuclear magnetic resonance phosphorus spectrum of the compound prepared in Example 3 of the present disclosure.

[0135] like Fig.10As shown, its phosphorus spectrum data is: 31 PNMR (162MHz, CDCl 3 )δ-44.19.

[0136] Fig.11 It is the carbon nuclear magnetic resonance spectrum of the compound prepared in Example 3 of the present disclosure.

[0137] like Fig.11 As shown, its carbon spectrum data is: 13 C NMR (101 MHz, CDCl 3 )δ158.54,158.32,133.63,133.44,128.50,128.43,125.46,120.17,11 9.95,119.67,119.64,77.35,77.24,77.04,76.72,34.68,34.66,29.35.

[0138] Fig.12 is an electrospray ionization mass spectrum (ESI-MS) of the compound prepared in Example 3 of the present disclosure;

[0139] like Fig.12 As shown, its electrospray mass spectrometry data is: ESI-MS (m / z): 500.21375 [M+H] +

[0140] Example 4: Synthesis of Catalyst II-1

[0141] In a nitrogen atmosphere, 1.0 mmol of compound (I-1) and 1.1 mmol of Py 2 NiMe 2 Dissolve them in toluene respectively, and drop the compound (I-1) solution into Py 2 NiMe 2 The solution was stirred and reacted at room temperature for 1 hour, and a brown-yellow solution was obtained by filtering. The solvent was removed in vacuo to obtain a catalyst having the structure of formula (II-1).

[0142]

[0143] Fig.13 It is the hydrogen nuclear magnetic resonance spectrum of the catalyst prepared in Example 4 of the present disclosure.

[0144] like Fig.13 As shown, its hydrogen spectrum data is: 1 H NMR (400 MHz, C 6 D 6)δ8.50(s,2H),7.58(t,J=7.7Hz,2H),7.19–7.01(m,2H),6.79(s,5H),6.54(s ,2H),6.24(d,J=5.8Hz,3H),2.44(s,6H),1.32(s,9H),-0.78(d,J=4.6Hz,3H).

[0145] Fig.14 It is the nuclear magnetic resonance phosphorus spectrum of the catalyst prepared in Example 4 of the present disclosure.

[0146] like Fig.14 As shown, its phosphorus spectrum data is: 31 PNMR (162MHz, C 6 D 6 )δ13.36.

[0147] Fig.15 It is the carbon nuclear magnetic resonance spectrum of the catalyst prepared in Example 4 of the present disclosure.

[0148] like Fig.15 As shown, its carbon spectrum data is: 13 C NMR (101 MHz, C 6 D 6 )δ173.98,173.77,157.25,157.14,137.11,137.02,132.60,131.84,131.75,130.10,129.48,126.88,126.64,126.39 ,123.62,123.54,122.11,122.05,118.69,118.17,112.08,112.01,44.72,33.87,28.30,-17.19(d,J=38.5Hz,Ni-Me).

[0149] Example 5: Synthesis of Catalyst II-2

[0150] In a nitrogen atmosphere, 1.0 mmol of compound (I-2) and 1.1 mmol of Py 2 NiMe 2 Dissolve them in toluene respectively, and drop the compound (I-2) solution into Py 2 NiMe 2 The solution was stirred and reacted at room temperature for 1 hour, and a brown-yellow solution was obtained by filtering. The solvent was removed in vacuo to obtain a catalyst having the structure of formula (II-2).

[0151]

[0152] Fig.16It is the hydrogen nuclear magnetic resonance spectrum of the catalyst prepared in Example 5 of the present disclosure.

[0153] like Fig.16 As shown, its hydrogen spectrum data is: 1 H NMR (400 MHz, C 6 D 6 )δ8.79(s,2H),7.95(s,2H),7.37–7.25(m,2H),7.16–7.06(m,5H),6.93(t,J=7.9Hz,1H),6.86–6.73(m,2H),6. 57–6.41(m,3H),4.12(dd,J=49.3,42.7Hz,4H),3.14(s,2H),2.75(s,2H),1.58(s,9H),-0.49(d,J=4.9Hz,3H).

[0154] Fig.17 It is the nuclear magnetic resonance phosphorus spectrum of the catalyst prepared in Example 5 of the present disclosure.

[0155] like Fig.17 As shown, its phosphorus spectrum data is: 31 PNMR (162MHz, C 6 D 6 )δ18.72.

[0156] Fig.18 This is the carbon nuclear magnetic resonance spectrum of the catalyst prepared in Example 5 of the present disclosure.

[0157] like Fig.18 As shown, its carbon spectrum data is: 13 C NMR (101 MHz, C 6 D 6 )δ156.64,156.55,138.26,138.17,134.64,134.61,133.26,133.17,131.60, 131.54,131.53,129.92,129.25,129.23,129.00,128.49,128.40,127.95,12 7.83,127.71,127.59,127.46,125.25,125.17,124.05,123.99,121.13,113. 15,113.08,67.34,53.97,34.89,34.87,29.44,-15.82(d,J=39.2Hz,Ni-Me).

[0158] Example 6: Synthesis of Catalyst II-3

[0159] In a nitrogen atmosphere, 1.0 mmol of compound (I-3) and 1.1 mmol of Py 2 NiMe 2 Dissolve them in toluene respectively, and drop the compound (I-3) solution into Py 2 NiMe 2 The solution was stirred and reacted at room temperature for 1 hour, and a brown-yellow solution was obtained by filtering. The solvent was removed in vacuo to obtain a catalyst having the structure of formula (II-3).

[0160]

[0161] Fig.19 It is the hydrogen nuclear magnetic resonance spectrum of the catalyst prepared in Example 6 of the present disclosure.

[0162] like Fig.19 As shown, its hydrogen spectrum data is: 1 H NMR (400 MHz, C 6 D 6 )δ8.06–7.97(m,2H),7.75(dd,J=23.7,13.9Hz,6H),7.43–7.22(m,4H),7.03(m,J=40.8,21. 5,5.6Hz,8H),6.77–6.56(m,4H),6.33(s,2H),1.30(d,J=3.4Hz,9H),-0.83(t,J=4.4Hz,3H).

[0163] Fig. 20 It is the nuclear magnetic resonance phosphorus spectrum of the catalyst prepared in Example 6 of the present disclosure.

[0164] like Fig. 20 As shown, its phosphorus spectrum data is: 31 PNMR (162MHz, C 6 D 6 )δ-18.94.

[0165] Fig.21 It is the carbon nuclear magnetic resonance spectrum of the catalyst prepared in Example 6 of the present disclosure.

[0166] like Fig.21 As shown, its carbon spectrum data is: 13 C NMR (101 MHz, C 6 D 6)δ149.09,143.00,142.61,137.59,134.83,134.10,133.08,131.79,13 1.70,130.80,128.95,128.26,127.56,127.46,127.09,126.85,126.61, 125.13,124.24,123.84,122.95,121.55,119.02,118.79,118.43,116. 82, 112.59, 111.71, 110.76, 33.77, 28.43, -14.59 (d, J=36.3Hz, Ni-Me).

[0167] Application Example 1

[0168] The catalysts prepared in Examples 4 to 6 were used to carry out ethylene polymerization, and the specific polymerization method was as follows:

[0169] In a glove box with a nitrogen atmosphere, 18 mL of toluene was added into a 350 mL autoclave equipped with a magnetic stirring device, an oil bath heating device and a thermometer. The container was connected to a high-pressure pipeline and the pipeline was evacuated. The container was heated to 80°C with an oil bath and kept warm for 10 minutes.

[0170] 2 mL of a toluene solution containing 1 μmol of the catalyst prepared in Examples 4 to 6 was injected into the container using a syringe, the valve was closed, and the ethylene pressure was adjusted to 8 atmospheres, and the reaction was carried out for 15 minutes.

[0171] The reaction was stopped, the reactor was opened, ethanol was added thereto to precipitate solids, and the solids were filtered and dried under reduced pressure to obtain white polyethylene solids.

[0172] In this application example, under the same conditions, the catalyst prepared in the example was not added, and 1 equivalent of the above Lewis acid was added as a control group, and it was found that no polyethylene was produced. That is, when Lewis acid exists alone, it has no catalytic activity.

[0173] The results of ethylene polymerization catalyzed by the catalysts prepared in Examples 4-6 are shown in Table 1:

[0174] Table 1

[0175] Project a catalyst Polyethylene / g Active b Melting point c / ℃ Number average molecular weight <![CDATA[Molecular weight distribution d > 1 Example 4 (II-1) 0.8 3.2 118.0 4.8 2.6 2 Example 5 (II-2) 1.2 4.8 127.4 14.6 2.7 3 Example 6 (II-3) 2.9 11.6 130.9 42.6 3.8 <![CDATA[4 e ]]> Example 4 (II-1) 1.0 4.0 122.0 15.6 2.6 <![CDATA[5 f ]]> Example 4 (II-1) 0.9 3.6 123.3 19.6 2.5 <![CDATA[6 g ]]> Example 4 (II-1) 0.8 3.2 119.4 10.7 2.7 <![CDATA[7 e ]]> Example 5 (II-2) 1.2 4.8 133.1 144.8 2.5 <![CDATA[8 f ]]> Example 5 (II-2) 1.0 4..0 133.9 192.7 2.3 <![CDATA[9 g ]]> Example 5 (II-2) 0.9 3.6 132.8 156.5 2.4 <![CDATA[10 e ]]> Example 6 (II-3) 2.1 8.4 135.1 415.9 2.5 <![CDATA[11 f ]]> Example 6 (II-3) 1.9 7.6 135.4 472.0 2.3 <![CDATA[12 g ]]> Example 6 (II-3) 1.8 7.2 135.3 429.8 2.3

[0176] in, a Polymerization conditions: The amount of the phosphine phenol nickel catalyst containing a nitrogen group: 1 μmol, ethylene polymerization conditions: 0.8 MPa, 80°C, with 20 mL of toluene as solvent for 15 minutes;

[0177] b Activity Unit: 10 6g / (mol cat.×h);

[0178] c Melting point of polyethylene;

[0179] d Number average molecular weight unit: kg / mol;

[0180] e Metal Lewis acid addition amount: 1.0equivNi(OAc) 2 ;

[0181] f Metal Lewis acid addition amount: 1.0equiv Zn(OAc) 2 ;

[0182] g Metal Lewis acid addition amount: 1.0equiv(TMEDA)Zn(OAc) 2 .

[0183] No metal Lewis acid was added in the experiments No. 1 to 3 in Table 1; Lewis acids of different metals were added in the experiments No. 4 to 12. It can be seen from the data in Table 1 that under the regulation of the metal Lewis acid, the metal Lewis acid and the N atom in the phosphine phenol nickel catalyst containing a nitrogen-containing group are coordinated to form a steric hindrance, which improves the thermal stability of the phosphine phenol nickel catalyst containing a nitrogen-containing group and significantly improves the molecular weight of the polyethylene product.

[0184] Application Example 2

[0185] The phosphine phenol nickel catalyst containing nitrogen-containing groups prepared in Example 6 is used to carry out copolymerization of ethylene and polar monomers, providing a method for preparing polar functional group-modified polyethylene using the phosphine phenol nickel catalyst containing nitrogen-containing groups as shown in the above formula (II-3). The specific experimental steps and results are shown in Table 2:

[0186] Table 2

[0187]

[0188] in: a Polymerization conditions: the amount of the phosphine phenol nickel catalyst containing a nitrogen group: 5 μmol, ethylene polymerization conditions: 0.8 MPa, tert-butyl acrylate 0.2 mol / L, methyl acrylate 0.1 mol / L, 10-undecenoic acid ester 1.0 mol / L, 10-undecenoic acid alcohol 1.0 mol / L, 80°C, toluene 20 mL, 30 minutes;

[0189] b Activity Unit: 10 5 g / (mol cat.×h);

[0190] c Melting point of copolymer;

[0191] d The mole fraction of polar monomer units in the copolymer;

[0192] e Number average molecular weight unit: kg / mol.

[0193] As shown in Table 2, the phosphine phenol nickel catalyst containing nitrogen-containing groups as shown in formula (II-3) can catalyze the copolymerization of ethylene and polar monomers under certain conditions to obtain polyethylene materials modified with polar functional groups. Among them, the activity of the phosphine phenol nickel catalyst containing nitrogen-containing groups as shown in formula (II-3) is as high as 14.4×10 5 g mol -1 h -1 The melting point of ethylene copolymer is 117.5~122.3℃, and the maximum number average molecular weight is 42.0×10 3 g / mol.

[0194] The specific embodiments described above further illustrate the purpose, technical solutions and beneficial effects of the present disclosure. It should be understood that the above description is only a specific embodiment of the present disclosure and is not intended to limit the present disclosure. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present disclosure should be included in the protection scope of the present disclosure.

Claims

1. A phosphinophenol compound containing a nitrogen-containing group, the structure of which is shown in formula (I), in, R 1 ~R 3 is independently selected from hydrogen, halogen, hydroxyl, substituted or unsubstituted C1-C20 alkyl, R 1 ~R 3 Any two adjacent ones of can form a loop with each other; R 4 and R 5 is independently selected from one of hydrogen, C1-C20 alkyl, C6-C20 aryl, or R 4 and R 5 They are cyclically connected to form one of an oxygen-containing heterocycle, a nitrogen-containing heterocycle, and a sulfur-containing heterocycle; R 6 Independently selected from substituted or unsubstituted C1-C20 alkyl, C5-C20 cycloalkyl, C6-C20 aryl; When the above substituted or unsubstituted group has a substituent, the substituent is selected from one of phenyl and halogen.

2. The compound according to claim 1, in, R 1 ~R 3 are respectively selected from hydrogen; Preferably, R 4 , R 5 are selected from methyl, or R 4 , R 5 Forming a morpholine group or a carbazole group; Preferably, R 6 Selected from phenyl.

3. The compound according to claim 1, in, Its structural formula is shown in any one of the following formulas (I-1) to (I-3):

4. A nickel phosphine phenolate catalyst containing a nitrogen-containing group, the structure of which is shown in formula (II), in, R 1 ~R 3 is independently selected from hydrogen, halogen, hydroxyl, substituted or unsubstituted C1-C20 alkyl, R 1 ~R 3 Any two adjacent ones of can form a loop with each other; R 4 and R 5 is independently selected from one of hydrogen, C1-C20 alkyl, C6-C20 aryl, or R 4 and R 5 They are cyclically connected to form one of an oxygen-containing heterocycle, a nitrogen-containing heterocycle, and a sulfur-containing heterocycle; R 6 Independently selected from substituted or unsubstituted C1-C20 alkyl, C5-C20 cycloalkyl, C6-C20 aryl; R 7 and R 8 is independently selected from one of hydrogen, halogen, C1-C20 alkyl, C6-C20 aryl, and pyridyl; When the above substituted or unsubstituted group has a substituent, the substituent is selected from benzene and halogen.

5. The catalyst according to claim 4, in, R 1 ~R 3 are respectively selected from hydrogen; Preferably, R 4 , R 5 are selected from methyl, or R 4 , R 5 Forming a morpholine group or a carbazole group; Preferably, R 6 Selected from phenyl; Preferably, R 7 , R 8 are respectively selected from pyridyl or methyl.

6. The catalyst according to claim 4, in, Its structural formula is shown in any one of the following formulas (II-1) to (II-3):

7. A method for preparing the catalyst according to any one of claims 4 to 6, include: In an atmosphere of nitrogen or argon, reacting a compound of formula (A), butyl lithium and a compound of formula (B) to obtain a phosphine phenol compound containing a nitrogen-containing group as shown in formula (I); The phosphine phenol compound solution containing a nitrogen-containing group is added dropwise to a nickel salt solution, and after reacting at room temperature for 1 to 12 hours, a nitrogen-containing phosphine phenol nickel catalyst as shown in formula (II) is obtained, wherein the molar ratio of the phosphine phenol compound containing a nitrogen-containing group to the nickel salt is 1:1.5 to 1:

5.

8. The method according to claim 7, in, The step of reacting the compound of formula (A) with butyl lithium and the compound of formula (B) comprises: The compound of formula (A) undergoes a substitution reaction with dihydropyran to obtain a compound of formula (A'); After reacting a compound of formula (A') with butyl lithium, a compound of formula (B) is added to the obtained reaction solution to obtain a phosphine phenol compound containing a nitrogen-containing group protected by dihydropyran as shown in formula (C); Removing the dihydropyran protecting group of the compound shown in formula (C) to obtain a phosphine phenol compound containing a nitrogen-containing group as shown in formula (I), 9. A method for preparing polyethylene using the nickel phosphine phenolate catalyst containing nitrogen-containing groups as claimed in any one of claims 4 to 6, include: In a protective gas atmosphere, injecting the phosphine phenol nickel catalyst liquid containing nitrogen groups into ethylene, reacting at 30-150° C. and 8-30 MPa for 0.1-20 hours to obtain polyethylene; Preferably, injecting the phosphine phenol nickel catalyst liquid containing nitrogen-containing groups into ethylene comprises: mixing and dissolving the phosphine phenol nickel catalyst containing nitrogen-containing groups and a metal Lewis acid in a molar ratio of 1:0.5 to 1:5 to obtain a catalyst mixed liquid, and injecting the catalyst mixed liquid into ethylene, wherein the metal Lewis acid comprises one of zinc acetate, N,N,N',N'-tetramethylethylenediamine zinc acetate, and nickel acetate.

10. A method for preparing polyethylene modified with a polar monomer using the nickel phosphine phenolate catalyst containing a nitrogen-containing group as claimed in any one of claims 4 to 6, include: In a protective gas atmosphere, ethylene, a polar monomer and the phosphine phenol nickel catalyst containing a nitrogen-containing group are mixed and dissolved, and reacted at 30 to 150° C. and 8 to 30 MPa for 0.1 to 20 hours to obtain polyethylene modified with a polar monomer; Wherein, the polar monomer includes at least one of methyl acrylate, tert-butyl acrylate, methyl 10-undecenoate and 10-undecenol; The molar ratio of the polar monomer to the phosphine phenol nickel catalyst containing a nitrogen-containing group is in the range of 1:100 to 1:5000.