Preparation method of quasi-two-dimensional perovskite nanocrystalline film and red-light perovskite light-emitting diode
Preparation of quasi-two-dimensional perovskite nanocrystal films by one-step spin-coating film method solves the problems of complex preparation technology of existing red perovskite LEDs and low luminous brightness, realizing the preparation of high-efficiency red light perovskite light emitting diodes, improving the The current injection and external quantum efficiency of the device are obtained.
Patent Information
- Application Number
- CN202310633507.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-30
- Publication Date
- 2024-12-03
AI Technical Summary
The existing thermal solvent preparation process of red perovskite LEDs is complex and has low luminous brightness, which limits the development of red perovskite LEDs in display applications.
The quasi-two-dimensional perovskite nanocrystalline film was prepared by one-step spin-coated film method. By adding organic amine salts and zwitterionic internal salts to the perovskite precursor solution, a layered quasi-two-dimensional perovskite structure was formed to inhibit grains. Grow and agglomerate to improve film quality.
The preparation of a quasi-two-dimensional perovskite nanocrystal film with low defects and smooth surface is achieved, and the efficiency and external quantum efficiency of red light perovskite light emitting diodes are improved.
Smart Images

Figure CN119061459A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of perovskite light emitting diodes, and in particular to a quasi-two-dimensional perovskite nanocrystalline film, a method for preparing the quasi-two-dimensional perovskite nanocrystalline film, and a red light perovskite light emitting diode prepared by using the quasi-two-dimensional perovskite nanocrystalline film. Background Art
[0002] Metal halide perovskite materials have excellent semiconductor properties and outstanding optoelectronic properties, and have great application potential in the field of display and lighting. At present, the main material of perovskite LEDs that meet the needs of red display (620nm~650nm) is composed of perovskite quantum dots. However, its thermal solvent preparation process is complicated and the luminous brightness is low, which restricts the development of red perovskite LEDs in display applications. Therefore, it is urgent to simplify the preparation process of red perovskite light-emitting layers and improve the efficiency of red perovskite light-emitting devices. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a quasi-two-dimensional perovskite nanocrystalline film, a method for preparing the film, and a high-efficiency red light perovskite light-emitting diode in view of the deficiencies in the prior art.
[0004] The technical solution of the present invention is as follows:
[0005] A method for preparing a quasi-two-dimensional perovskite nanocrystalline film, the method is to add an organic amine salt and a zwitterionic inner salt to a perovskite precursor solution, and prepare the film by a one-step spin coating method; wherein the perovskite precursor solution is mixed with an organic amine salt, AX, BX2 and a zwitterionic inner salt in a molar ratio of 0.01-10:0.1-10:0.1-10:0.01-10, A is a cationic group, B is a metal cation, and X is a halogen anion. Preferably, the molar ratio of organic ammonium salt:AX:BX2:zwitterionic inner salt is 0.01-1:0.1-10:0.1-10:0.01-1.
[0006] The perovskite precursor solution is mixed under stirring at room temperature for 3-5 hours.
[0007] The above cationic group is Rb + , Cs + 、MA + and FA + Any one or more of the following;
[0008] The above metal cation is Pb 2+ , Sn 2+ , Cu 2+ Any one or more of the following;
[0009] The above halogen anion is I - Br - , Cl - Any one or more of .
[0010] The general formula of the quasi-two-dimensional perovskite structure is A'2A n-1 B n X 3n+1 (n=1-7), a quasi-two-dimensional multi-quantum well structure, wherein A' is a large-sized organic cation group, such as a guanidine cation (GA + ), phenylethylamine cation (PEA + ), phenylbutanamine cation (PBA + ) etc.; A is a cationic group, and the cationic group is Rb + , Cs + 、MA + and FA + Any one or more of; wherein B is a metal cation, including Pb 2+ , Sn 2+ , Cu + , Cu 2+ , Mn 2+ ,Eu 2+ , Ni 2+ ,Co 2+ Any one or more of; wherein X is a halogen anion, including I - Br - , Cl - and F - Any one or more of .
[0011] The zwitterionic inner salt is an organic molecule composed of anions, cations and organic groups connecting zwitterionic inner salts. The anions of the zwitterionic inner salts may include but are not limited to carboxylate (-COO - ), sulfonate (-SO3 -) , trifluoroborate (-BF3 - ) and other organic acid radical ions; the cations of the zwitterionic inner salt may include but are not limited to primary amine salts (-NH3 + ), secondary amine salt (-RNH2 + ), tertiary amine salt (-R2NH + ), quaternary ammonium salt (-R3N + ) and other organic cations; the organic group connecting the zwitterion may include an aliphatic functional group and an aromatic functional group, and the aliphatic functional group includes a straight chain group, an alicyclic hydrocarbon group (-C n H 2n-1 ); straight chain groups include alkyl (-C n H 2n+1 ), alkenyl (-C n H2n-1 ), alkynyl (-C n H 2n-2 ); the aromatic functional group includes a benzene ring, a naphthalene ring, an anthracene ring, an imidazole ring, a benzimidazole ring, a pyridine ring, a quinoline ring, an indole ring and other condensed rings, a five-membered heterocycle, and a six-membered heterocycle. Preferably, the zwitterionic inner salt is one or more of sulfobetaine 8, sulfobetaine 10, methacryloylethyl sulfobetaine or (pyrrolidinium-1-ylmethyl) trifluoroborate inner salt.
[0012] In the above organic amine salts, the cations thereof include but are not limited to guanidine (-CN3H5 + ), amine group (-CN2H4 + ) and hydrazine (-N2H4 + ) and other organic cations, as well as primary amine salts (-NH3 + ), secondary amine salt (-RNH2 + ), tertiary amine salt (-R2NH + ), quaternary ammonium salt (-R3N + ) and other organic cations, and their anions include I - Br - , Cl - 、F - Preferably, the organic amine salt is one or more of GAI, PEAI, PBAI or PMAI.
[0013] The above-mentioned zwitterionic inner salt needs to be completely dissolved in the precursor solution, and the molecular structure has a large steric hindrance, which can promote the dissolution of the raw materials AX and BX2.
[0014] The precursor solution component is preferably a mixture of PEAI, GAI, CsI, PbI2, PbBr2 and sulfobetaine-8 (SB3-8). The molar ratio of the mixture of PEAI, GAI, CsI, PbI2, PbBr2 and sulfobetaine-8 (SB3-8) is preferably 0.2-0.4:0.2-0.4:1-1.15:0.25-0.4:0.6-0.75:0.1.
[0015] The one-step spin coating method uses a rotation speed of 3000-5000 rpm and a spin coating time of 30-60 seconds. The obtained perovskite film is annealed on a heating plate at 80-110° C. for 6-15 minutes and then cooled to room temperature.
[0016] Preferably, the one-step spin coating method uses a rotation speed of 3000-4000 rpm and a spin coating time of 60 s. The obtained perovskite film is annealed on a heating plate at 90-100° C. for 10 min and then cooled to room temperature.
[0017] The perovskite film is distributed on any one of glass, flexible substrates and metal sheets.
[0018] The quasi-two-dimensional perovskite nanocrystal film is prepared using the above method.
[0019] The structure of a light-emitting diode comprises, from bottom to top, a substrate layer, a hole transport-electron blocking layer, a perovskite light-emitting layer, an electron transport-hole blocking layer, an electrode modification layer and an electrode, wherein the perovskite layer is a quasi-two-dimensional perovskite nanocrystalline film prepared by the above method.
[0020] Compared with the prior art, the present invention has the following beneficial effects: the organic amine salt in the present invention participates in the crystallization of perovskite to form a layered quasi-two-dimensional perovskite, the anions in the zwitterionic inner salt have electrostatic interactions with the A-position cations and the organic amine salt in the precursor component, thereby inhibiting the growth of perovskite grains, and at the same time, the outer aromatic ring or fatty chain group has a large steric hindrance, thereby inhibiting the agglomeration between the grains; ultimately, a low-defect, smooth-surfaced quasi-two-dimensional perovskite nanocrystalline film is formed, the device current injection is improved, efficient red light emission of the device is achieved, and the external quantum efficiency of the red perovskite light-emitting diode (PeLED) is improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a schematic structural diagram of a perovskite light-emitting device according to Example 1 of the present invention;
[0022] Figure 2 This is a SEM image of the perovskite film morphology of Example 1 of the present invention;
[0023] Figure 3 This is the ultraviolet-visible light absorption spectrum of the perovskite film of Example 1 of the present invention;
[0024] Figure 4 This is a graph of external quantum efficiency-current density of the device of Example 1 of the present invention;
[0025] Figure 5 is a voltage-current density-brightness curve diagram of the device of Example 1 of the present invention;
[0026] Figure 6 This is an electroluminescence spectrum diagram of the device of Example 1 of the present invention;
[0027] Figure 7 The electroluminescence spectra of the device of Example 1 of the present invention at different voltages;
[0028] Figure 8 is an external quantum efficiency-current density curve diagram of the device of Example 2 of the present invention;
[0029] Fig. 9 The electroluminescence spectra of the device of Example 2 of the present invention at different voltages;
[0030] Fig.10 This is a graph of external quantum efficiency-current density of the device of Example 3 of the present invention;
[0031] Fig.11 The electroluminescence spectra of the device of Example 3 of the present invention at different voltages;
[0032] Fig.12 is an external quantum efficiency-current density curve diagram of the device of Example 4 of the present invention;
[0033] Fig.13 The electroluminescence spectra of the device of Example 4 of the present invention at different voltages;
[0034] Fig.14 This is a graph of external quantum efficiency-current density of the device of Example 5 of the present invention;
[0035] Fig.15 The electroluminescence spectra of the device of Example 5 of the present invention at different voltages;
[0036] Fig.16 is an external quantum efficiency-current density curve diagram of the device of Example 6 of the present invention;
[0037] Fig.17 The electroluminescence spectra of the device of Example 6 of the present invention at different voltages;
[0038] Fig.18 This is a graph of external quantum efficiency-current density of the device of Comparative Example 1 of the present invention;
[0039] Fig.19 This is a graph of external quantum efficiency-current density of the device of Comparative Example 2 of the present invention; DETAILED DESCRIPTION
[0040] The present invention is described in detail below in conjunction with specific embodiments.
[0041] The following example solutions were prepared using the following method:
[0042] The perovskite ABX3 precursor solution is prepared by mixing AX, BX2, organic amine salt and zwitterionic inner salt in a certain proportion in a solvent to form different concentrations. + , Cs + 、MA + and FA + Any one of the multiple types), B is the fourth main group metal (Pb 2+ , Sn 2+ ) or transition metal ions (Cu 2+ , Ni 2+ ,Co 2+ , Fe 2+, Mn 2+ ,Eu 2+ ), X is a halogen element (Cl, Br, I, F). The ratio of organic ammonium salt: AX: BX2: zwitterion inner salt is 0.05-100: 1-10: 1-10: 0.05-100, and the solvent refers to any one or more of dimethyl sulfoxide (DMSO), N,N-dimethylformamide (DMF), and γ-butyrolactone. The concentration refers to the percentage of solute (perovskite ABX3, organic amine salt and zwitterion inner salt) in the total mass of solute and solvent, which is 0.1% to 99.9%.
[0043] Example 1
[0044] Preparation of red LED with 649nm emission band: The perovskite CsPb(IBr)3 precursor solution is made of PEAI, GAI, CsI, PbI2, PbBr2 and sulfobetaine-8 (SB3-8) in a molar ratio of 0.2:0.2:1.0:0.4:0.6:0.1 dissolved in solvent N,N dimethylformamide (DMF), stirred at room temperature for 4h, and a clear and transparent colorless perovskite precursor solution is obtained. The entire device structure is described as: glass substrate / ITO / PEDOT:PASS / PTAA / CsPb(IBr)3 / TPBi / LiF / Al.
[0045] The device preparation method is as follows:
[0046] The structure of perovskite light-emitting devices is as follows Figure 1 As shown, it includes a cathode layer, a transparent conductive substrate layer, and a hole transport-electron blocking layer, a perovskite light-emitting layer, an electron transport-hole blocking layer, an electrode modification layer and an electrode are sequentially arranged on the substrate layer.
[0047] ① The substrate is indium tin oxide (ITO) conductive glass, the square resistance of the ITO film is 15Ω, and the film thickness is 20-200nm. The transparent conductive substrate ITO glass is ultrasonically cleaned twice using isopropyl alcohol, acetone and ethanol solutions respectively. After drying the ITO glass, the ITO is transferred to an oxygen plasma surface cleaning machine and cleaned with oxygen plasma.
[0048] ② Preparation of hole transport-electron blocking layer. The purchased PEDOT:PSS (Al4083) solution was filtered with a water-soluble filter head, and then coated on the treated ITO conductive glass by spin coating. After annealing at 150°C for 15 minutes, a dense PEDOT:PSS film was formed. The substrate was transferred to a nitrogen-filled glove box, and the purchased poly [bis (4-phenyl) (2,4,6-trimethylphenyl) amine] (PTAA) was dissolved in chlorobenzene and covered on the PEDOT:PPS film by spin coating. After annealing at 100°C for 10 minutes, a dense PTAA film was obtained.
[0049] ③ Preparation of perovskite light-emitting layer: In a nitrogen glove box, the perovskite precursor solution was taken and a one-step spin coating method was used. The rotation speed was 3000 rpm and the spin coating time was 60 s. The obtained perovskite film was annealed at 90 ° C on a heating plate for 10 min and cooled to room temperature.
[0050] ④ Preparation of electron transport-hole blocking layer: The prepared perovskite film was transferred to a vacuum evaporation chamber for preparation of electron transport layer TPBi, with an air pressure of 6×10 -7 Torr, the evaporation rate is controlled at 0.05-0.1 nm / s, the thickness is 30-50 nm, and the evaporation rate and thickness are monitored by a film thickness meter.
[0051] ⑤ Preparation of electrode modification layer and electrode: In the vacuum evaporation chamber, continue to prepare the electrode modification layer (LiF) and electrode (Al). When evaporating the electrode modification layer, the evaporation rate is controlled below 0.01nm / s, the thickness is 1.0nm, and the evaporation rate of the electrode is maintained at 0.1nm / s, and the thickness is 100nm.
[0052] PeLED devices were prepared respectively, and the device performance was tested in a glove box.
[0053] Test the device's current-voltage-radiation intensity and other characteristics, and also test the device's luminescence spectrum parameters.
[0054] Figure 2 This is the morphology of the perovskite film. Under the synergistic effect of organic ammonium salts (PEAI, GAI) and zwitterionic inner salts (SB3-8), perovskite forms high-quality layered quasi-two-dimensional perovskite nanocrystals. Figure 3 This is the UV-visible absorption spectrum of the perovskite film. It can be seen that the organic ammonium salts (PEAI, GAI) can self-assemble to form layered perovskites with n=2. Figure 4 This is a curve diagram showing the relationship between the external quantum efficiency (EQE) and current density of the perovskite device. The EQE of the device can reach 17.88%. Figure 5 This is the voltage-current-brightness relationship curve of the perovskite device. Figure 6 This is the electroluminescence spectrum of the perovskite film. It can be seen that the luminescence peak is at 649nm. Figure 7 The electroluminescence spectra of perovskite films under different voltages show that the spectrum of perovskite LEDs working at 3 to 5 V is stable.
[0055] Example 2
[0056] Preparation of red light LED in the 655nm emission band: The difference between this embodiment and Example 1 is that the precursor solution components PEAI, GAI, CsI, PbI2, PbBr2 and sulfobetaine-8 (SB3-8) are in a molar ratio of 0.2:0.2:1.15:0.4:0.6:0.1, and the device preparation method refers to Example 1.
[0057] like Figure 8 As shown, the EQE of the 655nm CsPb(IBr)3 light-emitting device reaches 20.29%, and its electroluminescence peak position remains basically unchanged under different voltages (see Fig. 9 ).
[0058] Example 3
[0059] A red light LED with a 645nm emission band. The difference between this embodiment and Example 1 is that the precursor solution components PEAI, GAI, CsI, PbI2, PbBr2 and sulfobetaine-8 (SB3-8) are in a molar ratio of 0.2:0.2:1.10:0.3:0.7:0.1, and the device preparation method refers to Example 1.
[0060] like Fig.10 As shown, the EQE of the 645nm CsPb(IBr)3 light-emitting device reaches 18.71%, and its electroluminescence peak position remains basically unchanged under different voltages (see Fig.11 ).
[0061] Example 4
[0062] A red light LED with a 641nm emission band. The difference between this embodiment and Example 1 is that the precursor solution components PEAI, GAI, CsI, PbI2, PbBr2 and sulfobetaine-8 (SB3-8) are in a molar ratio of 0.2:0.2:1.05:0.3:0.7:0.1, and the device preparation method refers to Example 1.
[0063] like Fig.12 As shown, the EQE of the 641nm CsPb(IBr)3 light-emitting device reaches 17.53%, and its electroluminescence peak position remains basically unchanged under different voltages (see Fig.13 ).
[0064] Example 5
[0065] A red light LED with a 637nm emission band. The difference between this embodiment and Example 1 is that the precursor solution components PEAI, GAI, CsI, PbI2, PbBr2 and sulfobetaine-8 (SB3-8) are in a molar ratio of 0.2:0.2:1.0:0.3:0.7:0.1, and the device preparation method refers to Example 1.
[0066] like Fig.14 As shown, the EQE of the 637nm CsPb(IBr)3 light-emitting device reaches 15.60%, and its electroluminescence peak position remains basically unchanged under different voltages (see Fig.15 ).
[0067] Example 6
[0068] The present embodiment is different from the embodiment 1 in that the precursor solution components PEAI, GAI, CsI, PbI2, PbBr2 and sulfobetaine-8 (SB3-8) are in a molar ratio of 0.2:0.2:1.05:0.25:0.75:0.1, and the device preparation method is similar to the embodiment 1. Fig.16 As shown, the EQE of the 633nm CsPb(IBr)3 light-emitting device reaches 14.11%, and its electroluminescence peak position remains basically unchanged under different voltages (see Fig.17 ).
[0069] Comparative Example 1
[0070] The difference between this comparative example and Example 1 is that the precursor solution components PEAI, CsI, PbI2, PbBr2 and sulfobetaine-8 (SB3-8) are in a molar ratio of 5.0:1.15:0.4:0.6:0.1, and the device preparation method refers to Example 1.
[0071] like Fig.18 As shown, when the molar ratio of the organic amine salt PEAI exceeds the preferred range, the EQE of the device is only 1.82%, which is much lower than the high-efficiency device in Example 1.
[0072] Comparative Example 2
[0073] The difference between this comparative example and Example 1 is that the precursor solution components CsI, PbI2, PbBr2 and sulfobetaine-8 (SB3-8) are in a molar ratio of 1.15:0.4:0.6:0.1, and the device preparation method refers to Example 1.
[0074] like Fig.19 As shown, in the absence of organic amine salt, the EQE of the device is only 0.56%, which is much lower than the high-efficiency device in Example 1.
[0075] It is stated again that for technicians in the relevant professions of the present invention, the same effect as the present invention can be achieved through obvious and simple component adjustments and molecular changes, which is also within the protection scope of the present invention.
Claims
1. A method for preparing a quasi-two-dimensional perovskite nanocrystalline film, characterized in that The method is prepared by adding organic amine salt and zwitterionic inner salt to a perovskite precursor solution and adopting a one-step spin coating thin film method; wherein the precursor solution is mixed with organic amine salt, AX, BX2 and zwitterionic inner salt in a molar ratio of 0.01-10:0.1-10:0.1-10:0.01-10, A is a cationic group, B is a metal cation, and X is a halogen anion.
2. The method for preparing a quasi-two-dimensional perovskite nanocrystalline film according to claim 1, characterized in that The molar ratio of the organic amine salt, AX, BX2 and zwitterionic inner salt is 0.01-1:0.1-10:0.1-10:0.01-1.
3. The method for preparing a quasi-two-dimensional perovskite nanocrystalline film according to claim 1, characterized in that The cationic group is Rb + , Cs + 、MA + and FA + Any one or more of; the metal cation is Pb 2+ , Sn 2+ , Cu 2+ Any one or more of; the halogen anion is I - Br - , Cl - Any one or more of .
4. The method for preparing a quasi-two-dimensional perovskite nanocrystalline film according to claim 1, characterized in that The quasi-two-dimensional perovskite structure has the general formula A'2A n-1 B n X 3n+1 , n=1-7; wherein A' is a large-sized organic cationic group, and the large-sized organic cationic group is a guanidine cation, a phenethylamine cation or a phenbutylamine cation.
5. The preparation method according to claim 1, characterized in that: The organic amine salts include, but are not limited to, guanidine, diamine and hydrazine, primary amine salts, secondary amine salts, tertiary amine salts and quaternary ammonium salts; and anions include I - Br - , Cl - 、F - .
6. The method for preparing a quasi-two-dimensional perovskite nanocrystalline film according to claim 1, characterized in that The zwitterionic inner salt is an organic molecule composed of anions, cations and organic groups connecting zwitterions. The anions include but are not limited to organic acid ions, the cations include but are not limited to organic cations, and the organic groups connecting zwitterions include aliphatic functional groups and aromatic functional groups.
7. The method for preparing a quasi-two-dimensional perovskite nanocrystalline film according to claim 6, characterized in that: The organic acid radical ions are carboxylates, sulfonates, and trifluoroborate; the organic cations are primary amine salts, secondary amine salts, tertiary amine salts, and quaternary ammonium salts; the organic groups connecting zwitterions include aliphatic functional groups and aromatic functional groups. The aliphatic functional groups include alicyclic hydrocarbon groups, alkyl groups, alkenyl groups, and alkynyl groups; the aromatic functional groups include benzene rings, naphthalene rings, anthracene rings, imidazole rings, benzimidazole rings, pyridine rings, quinoline rings, indole rings, and other condensed rings, five-membered heterocycles, and six-membered heterocycles.
8. The method for preparing a quasi-two-dimensional perovskite nanocrystalline film according to claim 1, characterized in that The one-step spin coating method adopts a rotation speed of 3000-6000 rpm and a spin coating time of 30-60 seconds. The obtained perovskite film is annealed on a heating plate at 80-110° C. for 6-15 minutes and then cooled to room temperature.
9. A quasi-two-dimensional perovskite nanocrystalline film, characterized in that The method is prepared by the method described in any one of claims 1 to 8.
10. A red perovskite light emitting diode, characterized in that The structure of the light-emitting diode is, from bottom to top, a substrate layer, a hole transport-electron blocking layer, a perovskite light-emitting layer, an electron transport-hole blocking layer, an electrode modification layer and an electrode; wherein the perovskite layer is a quasi-two-dimensional perovskite nanocrystalline film as described in claim 9; and the substrate layer is glass, a flexible substrate or a metal sheet.