Overcurrent protection element
By using fluorine-containing copolymers and carbon black materials in overcurrent protection elements, adjusting the resistance start-up temperature, the problem of insufficient resistance stability and high-temperature operation in the prior art is solved, and high-efficiency current protection in automotive environments is achieved .
Patent Information
- Application Number
- CN202310654722.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2023-06-05
- Publication Date
- 2024-11-22
AI Technical Summary
The existing overcurrent protection elements have poor resistance stability in the low-temperature zone and the operating temperature is not sufficient to meet the high-temperature overheating protection needs of the automotive market.
Use fluorine-containing copolymer as polymer substrate, combined with carbon black conductive filler, adjust the resistance start-up temperature to between 200℃ and 210℃, ensuring that the low-resistance state is maintained in the low-temperature zone and the current is quickly cut off at high temperatures. .
The resistance stability and high-temperature operation of overcurrent protection elements in the low-temperature zone are improved, and the high-temperature protection needs of the automotive market are met, and the problems of premature current cutoff and solder softening are avoided.
Smart Images

Figure CN119008149A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an overcurrent protection element, and more particularly to an overcurrent protection element with good resistance thermal stability and high operating temperature. Background Art
[0002] The resistance of existing conductive composite materials with positive temperature coefficient (PTC) characteristics is very sensitive to changes in specific temperature. They can be used as materials for current sensing elements and are currently widely used in overcurrent protection elements or circuit elements. Specifically, the resistance of PTC conductive composite materials can be maintained at an extremely low value at normal temperature, allowing the circuit or battery to operate normally. However, when the circuit or battery has an overcurrent (over-current) or overtemperature (over-temperature) phenomenon, its resistance value will instantly increase to a high resistance state (at least 10 4 Ω or more), which is called a trip, and the overcurrent is cut off to protect the battery or circuit components.
[0003] As for the most basic structure of the overcurrent protection element, it is composed of a PTC material layer and metal electrodes attached to both sides thereof. The PTC material layer will at least include a substrate and a conductive filler. The substrate is composed of a polymer, and the conductive filler is dispersed in the polymer as a conductive channel. Traditionally, in response to the high temperature overheating protection requirements of electronic devices, polymers often use polyvinylidene fluoride (PVDF) with a high melting point (compared to the commonly used polyethylene) as its main component. In order to improve the voltage resistance characteristics, the conductive filler is composed of carbon black instead of a combination of carbon black and metal materials. Based on the combination of polyvinylidene fluoride and pure carbon black, a high voltage overcurrent protection element for high temperature overheating protection can be made. However, there are at least two problems with this type of overcurrent protection element: first, the resistance stability of the overcurrent protection element is poor in the low temperature section before triggering; second, the high temperature operability of polyvinylidene fluoride cannot meet the application requirements of the automotive market for high temperature overheating protection. As for the first point, in the low temperature section of about 40°C to 130°C before being triggered, the resistance value of the overcurrent protection element has a significant increase, which makes the electronic device susceptible to temperature during normal operation and reduces the amount of current flowing through. As for the second point, the operating temperature of polyvinylidene fluoride is around 160°C, which is too low for the automotive market. The operating temperature can also be called the resistance starting temperature, which refers to the temperature point corresponding to when the resistance value begins to rise sharply. It should be understood that the normal operating temperature of several electronic components included in the automotive electronic module can reach about 150°C to 160°C. If the operating temperature of the overcurrent protection element is lower than or around 160°C, it means that the current of the overcurrent protection element will be gradually or completely cut off before the temperature rises to this temperature, causing the automotive electronic components that were originally able to operate normally to stop operating. In addition, with the development trend of the automotive market, the normal operating temperature of automotive electronic components may be further increased in the future (i.e., exceeding 160°C), so the operating temperature of the overcurrent protection element must be much higher than 160°C.
[0004] From the above, it can be seen that the existing overcurrent protection devices still have considerable room for improvement in terms of resistance stability and high temperature operation performance. Summary of the invention
[0005] The present invention provides an overcurrent protection element that is resistant to high voltage and has a high operating temperature, which is particularly suitable as a protection element for automotive components. The overcurrent protection element has a thermistor layer that exhibits a positive temperature coefficient characteristic, and the thermistor layer has a high molecular polymer substrate and a conductive filler composed of carbon black. It should be particularly noted that the high molecular polymer substrate of the present invention is mainly composed of a fluorine-containing copolymer. The fluorine-containing copolymer can improve the defects of the aforementioned conductive filler regarding resistance stability, so that the overcurrent protection element maintains a stable low-resistance state in the low temperature section (40°C to 130°C) before being triggered. Secondly, under the appropriate proportion of the deployment, the fluorine-containing copolymer can adjust the resistance tripping temperature of the overcurrent protection element to between 200°C and 210°C. After this adjustment, the overcurrent protection element can meet the needs of the automotive market for high-temperature overheating protection.
[0006] According to one embodiment of the present invention, an overcurrent protection element comprises an electrode layer and a thermistor layer. The electrode layer has an upper metal layer and a lower metal layer. The thermistor layer contacts the upper metal layer and the lower metal layer and is stacked therebetween. The thermistor layer has a positive temperature coefficient characteristic and comprises a polymer matrix and a conductive filler. The polymer matrix comprises a fluorine-containing copolymer. The fluorine-containing copolymer is a copolymer of a fluorine-free olefin monomer and a fluorine-containing olefin monomer and has a melting point between 215°C and 240°C. The conductive filler is composed of carbon black and is dispersed in the polymer matrix to form a conductive path of the thermistor layer. Furthermore, the overcurrent protection element has a resistance jump rate between 1.2 and 1.3 between 40°C and 130°C.
[0007] According to some embodiments, the resistance value of the over-current protection element at 130° C. is 0.02Ω to 0.03Ω.
[0008] According to some embodiments, the overcurrent protection element has a resistor trip temperature between 200°C and 210°C.
[0009] According to some embodiments, the overcurrent protection element has a peak resistance greater than 4×10 4 Ω.
[0010] According to some embodiments, based on 100% of the volume of the thermistor layer, the volume percentage of the fluorine-containing copolymer is 48% to 60%.
[0011] According to some embodiments, the fluorine-containing copolymer is an ethylene-tetrafluoroethylene copolymer.
[0012] According to some embodiments, based on 100% of the volume of the thermistor layer, the volume percentage of the conductive filler is 27% to 34%.
[0013] According to some embodiments, the polymer matrix further comprises a nucleating agent. The nucleating agent is selected from the group consisting of polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, perfluorocarbon oxide-modified tetrafluoroethylene, difluoroethylene-tetrafluoroethylene polymer, tetrafluoroethylene-perfluorodioxole copolymer, difluoroethylene-hexafluoropropylene copolymer, difluoroethylene-hexafluoropropylene-tetrafluoroethylene terpolymer, and mixtures or copolymers of any combination thereof. Based on the volume of the thermistor layer being 100%, the volume percentage of the nucleating agent is 4% to 6%.
[0014] According to some embodiments, the polymer matrix does not include poly(chlorotrifluorotetrafluoroethylene).
[0015] According to some embodiments, the melting point of the fluorine-containing copolymer is lower than the melting point of the nucleating agent, and the melting point of the fluorine-containing copolymer differs from the melting point of the nucleating agent by 110° C. to 140° C.
[0016] According to some embodiments, the thickness of the thermistor layer is 0.12 mm to 0.15 mm.
[0017] According to some embodiments, the nucleating agent is polytetrafluoroethylene.
[0018] According to some embodiments, the overcurrent protection element has a first trigger current thermal drop ratio of 65% to 79%. The first trigger current thermal drop ratio is defined as the trigger current required by the overcurrent protection element in an environment of 85°C divided by the trigger current required by the overcurrent protection element in an environment of 25°C, and converted into a percentage.
[0019] According to some embodiments, the overcurrent protection element has a second trigger current thermal drop ratio of 53% to 60%. The second trigger current thermal drop ratio is defined as the trigger current required by the overcurrent protection element in an environment of 125°C divided by the trigger current required by the overcurrent protection element in an environment of 25°C, and converted into a percentage.
[0020] According to some embodiments, the overcurrent protection element has a third trigger current thermal drop ratio of 69% to 82%. The third trigger current thermal drop ratio is defined as the trigger current required by the overcurrent protection element at 125°C divided by the trigger current required by the overcurrent protection element at 85°C, converted into a percentage.
[0021] According to some embodiments, the thermistor layer further includes a flame retardant. The flame retardant is selected from the group consisting of zinc oxide, antimony oxide, aluminum oxide, silicon oxide, calcium carbonate, magnesium sulfate or barium sulfate, magnesium hydroxide, aluminum hydroxide, calcium hydroxide and barium hydroxide. The volume percentage of the flame retardant is 9% to 13% based on the volume of the thermistor layer as 100%.
[0022] According to some embodiments, the flame retardant is magnesium hydroxide.
[0023] According to some embodiments, the overcurrent protection element has a withstand voltage value of 24V and can pass a cycle life test set at the withstand voltage value without burning out. The cycle life test is performed at a power of 24V / 40A for 500 cycles.
[0024] According to some embodiments, the power handling capacity per unit area of the overcurrent protection element at 25° C. is 1.9 W / mm 2 Up to 2.7W / mm 2 .
[0025] According to some embodiments, the power handling capacity per unit area of the overcurrent protection element at 125° C. is 1 W / mm 2 Up to 1.5W / mm 2 . BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 A cross-sectional view showing an overcurrent protection element according to an embodiment of the present invention;
[0027] Figure 2 show Figure 1 a top view of an overcurrent protection element; and
[0028] Figure 3 , Figure 4 and Figure 5 Displays the resistance value-temperature curve of the overcurrent protection element.
[0029] The reference numerals are described as follows:
[0030] 10: Overcurrent protection element
[0031] 11: Thermistor layer
[0032] 12: Upper metal layer
[0033] 13: Lower metal layer
[0034] A: Length
[0035] A0: Intersection point
[0036] A1, A2: Resistance starting point
[0037] B: Width
[0038] L1: First tangent
[0039] L2: Second tangent DETAILED DESCRIPTION
[0040] In order to make the above and other technical contents, features and advantages of the present invention more clearly understood, relevant embodiments are given below and described in detail with reference to the accompanying drawings.
[0041] Please refer to Figure 1 , showing the basic state of the overcurrent protection element of the present invention. The overcurrent protection element 10 includes a thermistor layer 11 and an electrode layer. The thermistor layer 11 has an upper surface and a lower surface, and the electrode layer has an upper metal layer 12 and a lower metal layer 13 respectively attached to the upper surface and the lower surface of the thermistor layer 11. In this way, the thermistor layer 11 is physically in direct contact with the upper metal layer 12 and the lower metal layer 13, and is stacked between the two. In one embodiment, the upper metal layer 12 and the lower metal layer 13 can be composed of nickel-plated copper foil or other conductive metals. In addition, the thermistor layer 11 includes a polymer substrate and a conductive filler. The polymer substrate is an insulator that is easily expanded by heat, and the conductive filler is a conductor, whereby the thermistor layer 11 has a positive temperature coefficient characteristic. When the overcurrent protection element 10 is not actuated, the conductive filler is evenly dispersed in the polymer matrix and connected in series to form a conductive channel; when the overcurrent protection element 10 is affected by high temperature, the polymer matrix will expand rapidly, so that the particles of the conductive filler are pulled apart from each other, resulting in the truncation of the conductive channel. In other words, the type of the polymer matrix and the ratio relative to the conductive filler roughly determine the positive temperature coefficient characteristics of the thermistor layer 11. Accordingly, the polymer matrix of the present invention includes a fluorine-containing copolymer. Through the adjustment of the appropriate ratio, the fluorine-containing copolymer can enable the overcurrent protection element 10 to maintain good resistance stability and increase its operating temperature.
[0042] According to the present invention, the fluorine-containing copolymer is copolymerized by a fluorine-free olefin monomer and a fluorine-containing olefin monomer, and has a melting point between 215°C and 240°C. For example, the fluorine-free olefin monomer may be ethylene, propylene, butene, pentene or hexene, and the fluorine-containing olefin monomer may be tetrafluoroethylene. Due to the high temperature stability of the fluorine-containing copolymer, the overcurrent protection element 10 can maintain a stable low resistance state in the low temperature section (40°C to 130°C). In detail, the overcurrent protection element 10 has a first resistance value when the ambient temperature is 40°C, and has a second resistance value when the ambient temperature is 130°C. The ratio obtained by dividing the second resistance value by the first resistance value is between 1.2 and 1.3. The aforementioned ratio is also called the resistance jump rate, which can show the degree of influence of high temperature on the resistance change. The resistance jump rate of the overcurrent protection element 10 of the present invention is between 1.2 and 1.3, which is quite close to 1, which means that the resistance value does not change much in the low temperature section (40°C to 130°C) before being triggered, and the same current flow can be maintained without affecting the normal operation of the electronic component. In one embodiment, the first resistance value and the second resistance value both fall within the range of 0.02Ω to 0.03Ω. In addition, the thermistor layer in which the conductive filler is entirely composed of carbon black has a higher voltage resistance than the thermistor layer in which the conductive filler is composed of carbon black and metal materials. If the same voltage resistance value is preset, the thermistor layer 11 of the present invention can be adjusted to be thinner. In one embodiment, the thickness of the thermistor layer 11 is 0.12mm to 0.15mm. In another embodiment, the thickness of the thermistor layer 11 can be 0.12mm, 0.13mm, 0.14mm or 0.15mm. Based on the aforementioned fluorine-containing copolymer, the present invention can significantly improve the resistance stability in the low temperature range, and enable the overcurrent protection element 10 to take advantage of the carbon black conductive filler (ie, improve the withstand voltage capability) and adjust the thickness of the thermistor layer 11 to be thinner.
[0043] In addition, the present invention selects fluorinated copolymers as the main component of the polymer matrix in consideration of the needs of the automotive market for high-temperature overheat protection. Fluorinated copolymers can control the resistance tripping temperature of the overcurrent protection element 10 within the range of 200°C to 210°C, such as 200°C, 201°C, 202°C, 203°C, 204°C, 205°C, 206°C, 207°C, 208°C, 209°C or 210°C. The resistance tripping temperature in the present invention can be adjusted to 203°C to 208°C at best. That is, as long as the formula ratio of the present invention is followed (described in detail below), the resistance tripping temperature will generally fall between 203°C and 208°C. The resistance tripping temperature refers to the starting temperature point corresponding to when the resistance value begins to rise sharply. At this temperature, the resistance value of the overcurrent protection element 10 has not yet risen to the highest, but is the starting point for the sudden rise. Then, as the temperature continues to rise to about 220° C. to 230° C., the overcurrent protection element 10 will present a high resistance state (resistance value exceeds 10 4 Ω).
[0044] It should be noted that when the car is running, its internal core temperature can be as high as 180°C, so automotive electronic components can generally operate normally between 150°C and 160°C. In addition, with the development trend of the automotive market, the normal operating temperature of automotive electronic components will be further increased in the future, that is, exceeding 160°C, or even reaching 180°C. Therefore, the resistor tripping temperature of the overcurrent protection element 10 needs to be adjusted to a higher temperature accordingly, but it cannot be unlimited. For example, when the resistor tripping temperature is lower than 200°C, the starting point of the sudden increase in the resistance value of the overcurrent protection element 10 is too close to the temperature at which the automotive electronic components can operate normally. This will increase the possibility of the overcurrent protection element 10 cutting off the current prematurely. Furthermore, before the temperature reaches the resistor tripping temperature, although the resistance value of the overcurrent protection element 10 has not risen sharply, it has begun to rise slowly. Therefore, the low resistor tripping temperature has already affected the normal operation of automotive electronic components.
[0045] If the resistor tripping temperature is higher than 210°C, there will be a problem of tin melting. In more detail, the melting point of the solder used when the overcurrent protection element 10 is assembled to the circuit board (or other supporting objects) is generally lower than 260°C, and it begins to soften and undergo a phase change at about 230°C. If the resistor tripping temperature of the overcurrent protection element 10 is too close to 230°C, it will cause the current to be completely cut off too late, causing the temperature to rise too high. This high temperature may cause the solder to soften or even melt, thereby causing the overcurrent protection element 10 to fall off the circuit board (or other supporting objects).
[0046] In addition, please note that the resistor starting temperature of the present invention is at least 200°C, which means that the main component of the polymer matrix must also have a melting point higher than this temperature. Therefore, in the present invention, the polymer matrix does not use polyvinylidene fluoride (melting point of about 177°C) with a relatively low melting point, but uses a fluorine-containing copolymer. The fluorine-containing copolymer is preferably an ethylene-tetrafluoroethylene copolymer. It should be understood that, depending on the polymerization method, the ethylene-tetrafluoroethylene copolymer may have different melting points, which may be as high as 280°C or above, or as low as 240°C or below. The present invention selects a low-melting-point ethylene-tetrafluoroethylene copolymer, in addition to the reasons for the aforementioned resistor starting temperature, also considering the process processing problem. If the melting point of the ethylene-tetrafluoroethylene copolymer is higher than 240°C, the structure of the material after the polymer matrix and the conductive filler are mixed at high temperatures will be too stable, resulting in difficulties in hot pressing. In one embodiment, the melting point of the ethylene-tetrafluoroethylene copolymer is preferably 220°C to 230°C. In this way, the overcurrent protection element 10 can have better thermal stability while not being so stable as to affect the mixing process.
[0047] In addition, the thermistor layer 11 of the present invention may further include a nucleating agent selected from the group consisting of polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, perfluorocarbon oxide-modified tetrafluoroethylene, difluoroethylene-tetrafluoroethylene polymer, tetrafluoroethylene-perfluorodioxole copolymer, difluoroethylene-hexafluoropropylene copolymer, difluoroethylene-hexafluoropropylene-tetrafluoroethylene terpolymer and any combination thereof. The melting point of the fluorinated copolymer is lower than the melting point of the nucleating agent, and the melting point of the fluorinated copolymer is preferably 110° C. to 140° C. different from the melting point of the nucleating agent, such as 110° C., 115° C., 120° C., 125° C., 130° C., 135° C. or 140° C. When the ambient temperature is higher than the melting point of the fluorinated copolymer and lower than the melting point of the nucleating agent, the fluorinated copolymer will melt while the nucleating agent will not. Accordingly, the nucleating agent can present solid particles uniformly dispersed in the thermistor layer 11 and serve as the nucleation center when the fluorine-containing copolymer recrystallizes, which is conducive to the formation of crystals. Alternatively, based on the high melting point characteristics of the nucleating agent, the deformation degree of the nucleating agent is small at high temperatures, thereby effectively stabilizing the structural form of the thermistor layer 11 without excessive deformation. In one embodiment, ethylene-tetrafluoroethylene copolymer is used as the main component of the polymer matrix (i.e., the fluorine-containing copolymer), and polytetrafluoroethylene is used as the secondary component of the polymer matrix (i.e., the nucleating agent); therefore, based on the volume of the thermistor layer as 100%, the volume percentage of ethylene-tetrafluoroethylene copolymer is 48% to 60%, and the volume percentage of polytetrafluoroethylene is 4% to 6%. In one embodiment, the volume percentage of ethylene-tetrafluoroethylene copolymer is 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%, 56%, 57%, 58%, 59% or 60% based on the volume of the thermistor layer 11 being 100%. In one embodiment, the volume percentage of polytetrafluoroethylene is 4%, 4.5%, 5%, 5.5% or 6% based on the volume of the thermistor layer 11 being 100%. In a preferred embodiment, the volume percentage of ethylene-tetrafluoroethylene copolymer is 48% to 57%, and the volume percentage of polytetrafluoroethylene is 5% based on the volume of the thermistor layer 11 being 100%. Considering the needs of automotive components, the content of polytetrafluoroethylene in the aforementioned ratio range will not be so high as to affect the resistance tripping temperature of the overcurrent protection element 10, but at the same time it can fine-tune the overall thermal stability of the polymer substrate. It should also be mentioned that, based on process considerations, the present invention does not use poly(chlorotrifluorotetrafluoroethylene) as a nucleating agent. That is, the polymer matrix does not contain poly(chlorotrifluorotetrafluoroethylene). Poly(chlorotrifluorotetrafluoroethylene) is prone to break, crack or produce smoke when mixed with other materials (ethylene-tetrafluoroethylene copolymer and other fillers), so it is not suitable for the present invention.
[0048] As for the conductive filler, the conductive filler of the present invention does not include metal materials. The metal material is, for example, tungsten carbide, titanium carbide, vanadium carbide, zirconium carbide, niobium carbide, tantalum carbide, molybdenum carbide, hafnium carbide, titanium boride, vanadium boride, zirconium boride, niobium boride, molybdenum boride, hafnium boride or zirconium nitride. As mentioned above, the conductive filler of the present invention is composed of carbon black, so that the thermistor layer 11 can be made thinner to achieve the ability to withstand high voltage. In one embodiment, the volume percentage of the conductive filler (i.e., carbon black) is 27% to 34% based on the volume of the thermistor layer as 100%.
[0049] In addition, the over-current protection element 10 of the present invention further includes several other electrical characteristics, which are described below using a thermal derating effect test of a trigger current and a cycle life test of a specific power.
[0050] For the thermal derating effect test, the overcurrent protection element 10 is placed in several different ambient temperatures, and the current required for its triggering can be measured at each ambient temperature. In a low temperature environment, the overcurrent protection element 10 has a lower resistance value, and the current required for triggering will be relatively large. In a high temperature environment, the overcurrent protection element 10 has a higher resistance value, and the current required for triggering will be relatively small. In other words, the increase in temperature will reduce the current required for triggering, which is the thermal derating effect of the triggering current. The thermal derating effect test is used to compare the difference in the triggering current of the overcurrent protection element 10 under different ambient temperatures, thereby evaluating the impact of high temperature on operability. Ideally, it is expected that the triggering current of the overcurrent protection element 10 can be maintained at the same value under various temperatures, stabilized at the preset triggering current to play a protective role, and facilitate operation. The overcurrent protection element 10 of the present invention has a triggering current thermal derating ratio in three temperature sections (hereinafter referred to as the first temperature section, the second temperature section, and the third temperature section). In the first temperature section (25°C to 85°C), the overcurrent protection element has a first trigger current thermal drop ratio of 65% to 79%. The first trigger current thermal drop ratio is defined as the trigger current required by the overcurrent protection element in an environment of 85°C divided by the trigger current required by the overcurrent protection element in an environment of 25°C, and converted into a percentage. In the second temperature section (25°C to 125°C), the overcurrent protection element has a second trigger current thermal drop ratio of 53% to 60%. The second trigger current thermal drop ratio is defined as the trigger current required by the overcurrent protection element in an environment of 125°C divided by the trigger current required by the overcurrent protection element in an environment of 25°C, and converted into a percentage. In the third temperature section (85°C to 125°C), the overcurrent protection element has a third trigger current thermal drop ratio of 69% to 82%. The third trigger current thermal drop ratio is defined as the trigger current required by the overcurrent protection element in an environment of 125°C divided by the trigger current required by the overcurrent protection element in an environment of 85°C, and converted into a percentage. It should be understood that the heat drop ratio of the trigger current of the conventional overcurrent protection element, regardless of the above temperature range, generally falls between 30% and 60%. However, the heat drop ratio of the trigger current of the overcurrent protection element 10 of the present invention in the above three temperature ranges can reach up to 80% or more, indicating that the current required for triggering is less affected by temperature. The overcurrent protection element 10 of the present invention can be stabilized at the preset trigger current to play a protective role, which is convenient for operation.
[0051] As for the cycle life test, the overcurrent protection element 10 of the present invention can still withstand a high voltage of 24V when the thickness of the thermistor layer 11 is about 0.12mm to 0.15mm. More specifically, in a preferred embodiment, the thermistor layer 11 further includes a flame retardant in a specific proportion. The flame retardant is selected from a group consisting of zinc oxide, antimony oxide, aluminum oxide, silicon oxide, calcium carbonate, magnesium sulfate or barium sulfate, magnesium hydroxide, aluminum hydroxide, calcium hydroxide and barium hydroxide. Taking the volume of the thermistor layer 11 as 100%, the present invention adjusts the volume percentage of the flame retardant to be much greater than 5% (for example, adjusted to a range of 9% to 13%). By virtue of the ability of the flame retardant to reduce flammability, the overcurrent protection element 10 can pass the cycle life test of higher voltage or high power (such as 24V / 40A) without burning. In addition, the overcurrent protection element can withstand a power per unit area of 1W / mm at 125°C. 2 Up to 1.5W / mm 2 The upper limit is much higher than the power that the traditional overcurrent protection element can withstand at a high temperature of 125°C (1W / mm 2 the following).
[0052] Please continue to refer to Figure 2 ,for Figure 1 The overcurrent protection element 10 has a length A and a width B, and the area "A×B" is also equal to the area of the thermistor layer 11. The thermistor layer 11 may have a top view area of 4mm depending on the product model. 2 Up to 72mm 2 For example, the area "A x B" can be 2 x 2 mm 2 , 5×5mm 2 、5.1×6.1mm 2 , 5×7mm 2 、7.62×7.62mm 2 、7.8×8.15mm 2 、7.3×9.5mm 2 or 7.62×9.35mm 2 In addition, the overall thickness of the overcurrent protection element 10 (i.e., the sum of the thicknesses of the upper metal layer 12, thermistor layer 11, and the lower metal layer 13) is between 0.19 mm and 0.22 mm. For example, the top surface area of the overcurrent protection element 10 may be 63.57 mm 2 (i.e. 7.8×8.15mm 2 ), and the thickness is 0.22 mm. In another embodiment, the top view area of the overcurrent protection element 10 may be 58.06 mm 2 (i.e. 7.62×7.62mm 2), and the thickness is 0.19 mm. It should be understood that the overcurrent protection element 10 of the present invention has the same effect when applied to the above dimensions.
[0053] As described above, the present invention can make the overcurrent protection element 10 have good electrical characteristics at high temperatures. The following Tables 1 to 6 further illustrate the actual verification data.
[0054] Table 1. Formula ratio of thermistor layer 11 (vol%)
[0055] Group ETFE PVDF PTFE <![CDATA[Mg(OH)2]]> CB E1 58.0 5.0 5.0 32.0 E2 60.0 5.0 3.0 32.0 E3 57.0 5.0 11.0 27.0 E4 57.0 5.0 9.0 29.0 E5 48.0 5.0 13.0 34.0 C1 58.0 5.0 3.0 34.0
[0056] Table 1 shows the formula ingredients of thermistor layer 11 of each embodiment of the present invention (group E1 to group E5) and comparative example (group C1) in volume percentage. The first column shows each group from top to bottom, namely embodiment E1 to comparative example C1. The first row shows the various material ingredients in thermistor layer 11 from left to right, namely ethylene-tetrafluoroethylene copolymer (ETFE), polyvinylidene difluoride (PVDF), polytetrafluoroethylene (PTFE), magnesium hydroxide (Mg(OH)2) and carbon black (CB). In addition, each group uses magnesium hydroxide as a flame retardant. As for the conductive filler, in order to improve the voltage resistance characteristics, it is composed only of carbon black.
[0057] In the embodiments E1 to E4 of the present invention, the main component of the polymer substrate is ETFE, and the secondary component is PTFE. Since PTFE has a melting point much higher than that of ETFE (about 330°C), the proportion of PTFE should not be too large to avoid affecting the protection temperature and other triggering characteristics of the overcurrent protection element. In addition, considering the function of PTFE as a nucleating agent, the melting point of ETFE and the melting point of PTFE must differ by at least 110°C, preferably by about 110°C to 140°C. If the melting point difference is too low, both will soften or melt at the same time at a specific temperature; in this way, the nucleating agent will lose its significance as a nucleation center and a stable structure. If the melting point difference is too high, the proportion of the nucleating agent in the content will be difficult to control, because a slight change in its proportion will significantly affect the thermal stability of the thermistor layer 11. That is, if the melting point difference is higher than 140°C, the nucleating agent will be too sensitive to the thermal stability of the thermistor layer 11, so the error tolerance during the deployment is too small. It should also be noted that the volume percentage of the polymer matrix (i.e., ETFE and PTFE) in the thermistor layer 11 must also be adjusted within an appropriate range. If it is too low, the current cannot be completely cut off when triggered, and if it is too high, the conductivity will be poor. In this formulation, the volume percentage of the polymer matrix in the thermistor layer 11 is 53% to 65%. Considering the impact of errors and the results of actual applications, the volume percentage of the polymer matrix in the thermistor layer 11 can achieve the same technical effect at 51% to 67%.
[0058] In Comparative Example C1, the main component of the polymer substrate is PVDF, and the secondary component is PTFE. Traditionally, polymer substrates based on PVDF are often used to make overcurrent protection components with high temperature resistance and high temperature overheat protection. Through subsequent test verification, it can be shown that Examples E1 to E4 have better high temperature overheat protection applicability than Comparative Example C1.
[0059] The preparation process of the overcurrent protection element of Example E1 to Example E5 and Comparative Example C1 is described as follows. First, based on the formula presented in Table 1, the materials in the formula are added to a twin-screw mixer produced by HAAKE for mixing. The mixing temperature of the embodiment is 240°C, while the mixing temperature of the comparative example is 215°C. The premixing time is 3 minutes, and the mixing time is 15 minutes. After the mixing is completed, a conductive polymer can be obtained, and a hot press is used at high temperature (250°C for the embodiment and 210°C for the comparative example) and 150kg / cm 2 The sheets were then cut into squares of about 20 cm x 20 cm. Next, the sheets were pressed into thin sheets using a hot press at high temperature (250°C for the example and 210°C for the comparative example) and 150 kg / cm 2The two nickel-plated copper foils are pressed onto the two sides of the conductive polymer sheet with a pressure of 100° to form a three-layer plate. Finally, a punch is used to punch out multiple chips from the plate, which are the overcurrent protection components. The length and width of the overcurrent protection component are 7.8mm and 8.15mm respectively (i.e., the top surface area is 63.57mm). 2 ), and the thickness is 0.22 mm. Then, the chips prepared in the embodiment and the comparative example were irradiated with a light dose of 50 kGy (the light dose can be adjusted according to the needs and is not a limiting condition of the present invention), and 15 chips were taken as test samples for subsequent experiments.
[0060] It should be noted that the resistance stability of the conventional overcurrent protection element is poor in the low temperature range, and its operating temperature does not meet the requirements of the automotive market. Therefore, two resistance-temperature tests (resistance-temperature test 1 and resistance-temperature test 2) are performed below to illustrate that compared with the conventional overcurrent protection element, the present invention has improved resistance stability and operating temperature.
[0061] Regarding the resistance-temperature test 1, the temperature conditions are: in the temperature range of 40℃ to 130℃, the heating rate is 5℃ / min, and each temperature point is kept at temperature for 15 minutes. The aforementioned holding time allows the overcurrent protection element to more accurately reflect its resistance value at a specific temperature. In more detail, staying at each temperature point in the environment for 15 minutes allows the overcurrent protection element to absorb heat and make its overall temperature rise to each temperature point, which is the same as the ambient temperature. This is conducive to analyzing its resistance state before it is triggered.
[0062] Table 2. Resistance-Temperature Test 1
[0063]
[0064] R 40℃ , refers to the resistance value of the overcurrent protection element at 40℃.
[0065] R 130℃ , refers to the resistance value of the overcurrent protection element at 130℃.
[0066] R 130℃ / R 40℃ , is R 130℃ and R 40℃ The ratio of high temperature to low temperature resistance jump rate is the ratio of high temperature to low temperature resistance jump rate. The lower this value is, the less the resistance is affected by temperature, and the stable low resistance state can be maintained. Therefore, the resistance jump rate can be used to evaluate the electrical conduction ability of the overcurrent protection element before it is triggered.
[0067] Please also refer to Table 2 and Figure 3 . Figure 3In the graph, the Y axis shows the resistance value, and the X axis shows the temperature. From 40°C to 130°C, the resistance value of Example E3 only increases from 0.0218Ω to 0.0267Ω, and its resistance jump rate (R 130℃ / R 40℃ ) is 1.23. The resistance jump rate (R 130℃ / R 40℃ ) is very close to 1, so the curve is quite stable from 40℃ to 130℃, and the resistance value is kept at about 0.02Ω. In contrast, the resistance value of Comparative Example C1 increases significantly from 0.0167Ω to 0.0683Ω in the temperature range of 40℃ to 130℃, and the resistance jump rate (R 130℃ / R 40℃ ) is 4.10. The resistance jump rate (R 130℃ / R 40℃ ) is much greater than 1, so its Figure 3 The above results show that the overcurrent protection element 10 of the present invention can maintain a stable low resistance state when not triggered, and does not affect the normal operation of the protected electronic element.
[0068] Next is the resistance-temperature test 2, the temperature condition of which is: in the temperature range of 40°C to 230°C, the temperature is continuously increased from 40°C to 230°C at a rate of 5°C / min. This test is used to observe the resistance bounce (triggering) of the overcurrent protection element.
[0069] Table 3. Resistance-temperature test 2
[0070]
[0071] Please refer to Table 3 and Figure 4 . Figure 4 In the diagram, the Y axis shows the resistance value, and the X axis shows the temperature. Figure 4 The Y-axis of the embodiment adopts a logarithmic scale, so the curves of the embodiments E1 to E5 are almost overlapped. Figure 4 The average value of all embodiments is presented in a single curve. Point A1 and point A2 are the starting points for the sudden rise of resistance, that is, the resistance jump point. The temperature point corresponding to the resistance jump point is the resistance jump temperature (℃) in Table 3. The resistance peak value is the highest point of resistance after the overcurrent protection element is triggered. In embodiments E1 to E5, the resistance jump temperature is 205℃, which meets the high operating temperature requirements of the automotive market. In addition, considering the problem of tin melting, the resistance jump temperature of embodiments E1 to E5 will not be too high to cause too late jump, so it can climb to 4.04×10 4Ω high resistance state. In contrast, the resistor tripping temperature of Comparative Example C1 is 165°C, which will start to work at the normal operating temperature of the vehicle components, affecting the normal operation of the vehicle components. Moreover, if an unexpected incident causes the temperature to rise to 200°C in a short period of time (the time when the protection function has no time to react), Comparative Example C1 is actually prone to rupture due to the poor thermal stability of the overcurrent protection component.
[0072] Please continue to refer to Figure 5 , further illustrating the definition of the resistor tripping temperature in embodiments E1 to E5 of the present invention. In the low resistance state before the overcurrent protection element 10 is triggered, a certain temperature section of this curve in the low resistance state will show a straight and slow linear climb, so a tangent L1 can be drawn from this linear climb section. During the period from the overcurrent protection element 10 being triggered to the high resistance state, a certain temperature section of this curve will show a sharp linear climb, so a tangent L2 can also be drawn from this linear climb section. Each point on the tangent L1 conforms to the formula: y=0.000006x+0.0858; and each point on the tangent L2 conforms to the formula: y=60.145x-12713. That is to say, in the linear climb section, the slope of the tangent L1 is 0.000006 (hereinafter referred to as the "lowest slope"); and the slope of the tangent L2 is 60.145 (hereinafter referred to as the "highest slope"). The tangent line L1 with the lowest slope and the tangent line L2 with the highest slope intersect at the intersection A0. The temperature point of the intersection A0 corresponding to the X-axis is the switching point between the low resistance state and the high resistance state, that is, the resistance starting temperature. Therefore, the intersection A0 will overlap with the resistance starting point A1 when it is vertically translated upward along the Y-axis. According to the formula of the thermistor layer 11 adjusted by the present invention, the resistance starting temperature under this definition can be accurately controlled within the range of 200°C and 210°C.
[0073] Subsequently, the voltage withstand characteristics of the overcurrent protection element 10 are evaluated by a cycle life test. The cycle life test is based on a cycle of applying a certain power for 10 seconds and shutting down for 60 seconds. In the following experiments, the cycle life test is divided into two conditions (hereinafter referred to as the first cycle life test and the second cycle life test). The conditions of the first cycle life test are 16V / 50A voltage / current and 500 cycles. The conditions of the second cycle life test are 24V / 40A voltage / current and 500 cycles.
[0074] Table 4. Cycle life test
[0075]
[0076] As shown in Table 4, the first column shows the verification items from left to right.
[0077] R i, refers to the initial resistance value of the overcurrent protection element at room temperature. In addition, according to the volume resistivity formula ρ=R×A / L, R is the resistance value, L is the thickness, and A is the area. i The volume resistivity is calculated as ρ.
[0078] R 16V / 50A_500C , refers to the resistance value measured when the overcurrent protection element is cooled to room temperature after the first cycle life test. Based on this, the resistance jump rate of the first cycle life test (i.e. R 16V / 50A_500C / R i ), the lower the ratio (i.e. the closer it is to 1), the better the ability of the overcurrent protection element to recover to a low resistance state or the resistance recovery. Similarly, R 24V / 40A_500C , refers to the resistance value measured when the overcurrent protection element is cooled to room temperature after the second cycle life test. Based on this, the resistance jump rate of the second cycle life test (i.e. R 24V / 40A_500C / R i ).
[0079] In Examples E1 to E5, the initial resistance value (R i ) generally fall within the range of 0.01Ω to 0.014Ω, which are all lower than 0.019Ω of Comparative Example C1. That is, the initial resistance values (R i ) is about 0.010Ω to about 0.014Ω, and its corresponding volume resistivity (ρ) is about 0.30Ω·cm to 0.41Ω·cm. However, it should be noted that although Example E3 has a slightly higher initial resistance value, its resistance jump rate (R 16V / 50A_500C / R i ) is the lowest among all the examples E1 to E5, which is 1.9. Moreover, the example E3 can pass the second cycle life test without burning, and has a resistance jump rate (R 24V / 40A_500C / R i The resistance jump rate (R 24V / 40A_500C / R i ) is 1.2, which is very close to 1, which means that the resistance does not change much before and after the trigger. Example E3 shows its advantage of stable resistance under higher voltage and high power conditions. In addition, Example E1 and Example E2 will burn out in the second cycle life test, so their R values are not shown in Table 4. 24V / 40A_500C and R 24V / 40A_500C / R i data.
[0080] Table 5. Trigger current and withstand power
[0081]
[0082] Table 6. Trigger current thermal drop percentage
[0083] Group <![CDATA[I-T 85℃ / I-T 25℃ ]]> <![CDATA[I-T 125℃ / I-T 25℃ ]]> <![CDATA[I-T 125℃ / I-T 85℃ <!-- 10 -->]]> E1 73.5% 56.4% 76.7% E2 75.8% 57.9% 76.4% E3 65.4% 53.2% 81.4% E4 73.5% 59.7% 81.3% E5 78.3% 54.2% 69.3% C1 63.6% 35.3% 55.6%
[0084] Please refer to Table 5 first. The first row shows several verification items from left to right.
[0085] IT 25℃ 、IT 85℃ and IT 125℃ , refers to the trigger current of the overcurrent protection element under 25℃, 85℃ and 125℃ environments respectively.
[0086] IT 25℃ / area and 25℃ withstand power can be obtained by IT 25℃ IT 25℃ / area refers to the trigger current per unit area of the overcurrent protection element at 25°C. The 25°C withstand power refers to the power per unit area of the overcurrent protection element at 25°C. The 125°C withstand power can be calculated by IT 125℃ The value obtained is the power that the overcurrent protection element can withstand per unit area in an environment of 125°C.
[0087] In the embodiments E1 to E5, the power that the overcurrent protection element 10 can withstand under a 25° C. environment is generally 1.9 W / mm. 2 Up to 2.7W / mm 2 The maximum power it can withstand (i.e. 2.67W / mm 2 ) is only the same as the conventional overcurrent protection element (ie, comparative example C1). However, when the ambient temperature rises to 125°C, the power that the overcurrent protection element 10 of embodiments E1 to E5 can withstand generally falls below 1W / mm 2 Up to 1.5W / mm 2 The power of the conventional overcurrent protection element is higher than that of the conventional overcurrent protection element (i.e., 0.94W / mm2 of the comparative example C1). 2 ). It can be seen that as the temperature increases, the advantages of the overcurrent protection element 10 of the present invention gradually emerge. That is, at 125° C., the overcurrent protection element 10 of the present invention can withstand the application of higher power without burning out, and has better high temperature stability.
[0088] In addition, this experiment further integrates IT 25℃ 、IT 85℃ and IT 125℃ The data were analyzed and summarized in Table 6.
[0089] As mentioned above, the current required to trigger the overcurrent protection element will be different under different ambient temperatures. In a low temperature environment, the overcurrent protection element has a lower resistance value, and the current required to trigger it will be relatively large. In a high temperature environment, the overcurrent protection element has a higher resistance value, and the current required to trigger it will be relatively small. In this way, the impact of high temperature on the operability of the overcurrent protection element can be evaluated based on the heat drop effect.
[0090] IT 85℃ / IT 25℃ That is, the first trigger current heat drop ratio defined above; IT 125℃ / IT 25℃ That is the second trigger current heat drop ratio defined above; and IT 125℃ / IT 85℃ That is, the third trigger current heat drop ratio defined above. For the convenience of explanation, the ratios of the three are converted into percentages and presented in Table 6. If the percentage is 100%, it means that the trigger current does not change between high and low temperatures, and the overcurrent protection element has the most ideal operating stability. Therefore, the closer the trigger current heat drop ratio is to 100%, the smaller the degree of heat drop is, and the more ideal the operating stability is. In Examples E1 to E5, the first trigger current heat drop ratio (IT 85℃ / IT 25℃ ), the second trigger current heat drop ratio (IT 125℃ / IT 25℃ ) and the third trigger current thermal drop ratio (IT 125℃ / IT 85℃ ) are 65.4% to 78.3%, 53.2% to 59.7% and 69.3% to 81.4% respectively, which are much higher than the trigger current heat drop ratio corresponding to the comparative example C1 (63.6%, 35.3% and 55.6% respectively). It is particularly noted that this ratio is more significant when the temperature range is high.
[0091] More specifically, in the temperature range of 25°C to 125°C, 25°C to 85°C is a relatively low temperature section, while 85°C to 125°C is a relatively high temperature section. In the relatively low temperature section, the first trigger current thermal drop ratio (IT 85℃ / IT 25℃ ) is 65.4% to 78.3%, while the first trigger current heat drop ratio (IT 85℃ / IT 25℃ ) is 63.6%; that is, the difference between Examples E1 to E5 and Comparative Example C1 is at most 14.7%. However, in the relatively high temperature section, the third trigger current heat drop ratio (IT 125℃ / IT85℃ ) is 69.3% to 81.4%, while the third trigger current heat reduction ratio (IT 125℃ / IT 85℃ ) is 55.6%; on the contrary, the difference between Examples E1 to E5 and Comparative Example C1 is at least 14%, and can be as high as 25.8%. That is to say, in the high temperature section, the difference in the stability of the trigger current between Examples E1 to E5 and Comparative Example C1 is more obvious. Examples E1 to E5 are significantly better than Comparative Example C1, with a percentage closer to 100%. Comparative Example C1 not only has a significant gap with Examples E1 to E5, but also reduces the trigger current by nearly 50%, and the thermal drop effect is serious.
[0092] The technical content and technical features of the present invention have been disclosed as above, but a person skilled in the art with ordinary knowledge may still make various substitutions and modifications based on the teachings and disclosures of the present invention without departing from the spirit of the present invention. Therefore, the protection scope of the present invention should not be limited to those disclosed in the embodiments, but should include various substitutions and modifications without departing from the present invention, and be covered by the following claims.
Claims
1. An overcurrent protection element, comprising: an electrode layer having an upper metal layer and a lower metal layer; and A thermistor layer contacts the upper metal layer and the lower metal layer and is stacked therebetween, wherein the thermistor layer has a positive temperature coefficient characteristic and comprises: A polymer matrix comprising a fluorine-containing copolymer, wherein the fluorine-containing copolymer is a copolymer of a fluorine-free olefin monomer and a fluorine-containing olefin monomer and has a melting point between 215° C. and 240° C.; and a conductive filler consisting of carbon black and dispersed in the high molecular polymer matrix for forming a conductive path of the thermistor layer; in, The over-current protection element has a resistance jump rate between 1.2 and 1.3 between 40° C. and 130° C. 2 . The over-current protection device according to claim 1 , wherein the resistance value of the over-current protection device at 130° C. is 0.02Ω to 0.03Ω. 3 . The over-current protection device as claimed in claim 2 , wherein the over-current protection device has a resistance tripping temperature between 200° C. and 210° C. 4 . The over-current protection element as claimed in claim 3 , wherein the over-current protection element has a resistance peak value greater than 4×10 4 Ω after being triggered. 5 . The overcurrent protection element according to claim 4 , wherein based on the volume of the thermistor layer being 100%, the volume percentage of the fluorine-containing copolymer is 48% to 60%. The overcurrent protection device according to claim 5 , wherein the fluorine-containing copolymer is ethylene-tetrafluoroethylene copolymer. 7 . The overcurrent protection device according to claim 6 , wherein based on the volume of the thermistor layer being 100%, the volume percentage of the conductive filler is 27% to 34%.
8. The overcurrent protection device according to claim 7, wherein the polymer substrate further comprises a nucleating agent selected from the group consisting of polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, perfluoroalkylene-modified tetrafluoroethylene, difluoroethylene-tetrafluoroethylene polymer, tetrafluoroethylene-perfluorodioxole copolymer, difluoroethylene-hexafluoropropylene copolymer, difluoroethylene-hexafluoropropylene-tetrafluoroethylene terpolymer, and mixtures or copolymers of any combination thereof, and based on the volume of the thermistor layer being 100%, the volume percentage of the nucleating agent is 4% to 6%. 9 . The overcurrent protection device according to claim 8 , wherein the high molecular polymer matrix does not contain poly(chlorotrifluorotetrafluoroethylene). 10 . The overcurrent protection device according to claim 8 , wherein the melting point of the fluorine-containing copolymer is lower than the melting point of the nucleating agent, and the melting point of the fluorine-containing copolymer differs from the melting point of the nucleating agent by 110° C. to 140° C. The overcurrent protection device according to claim 10 , wherein the thickness of the thermistor layer is 0.12 mm to 0.15 mm. 12 . The overcurrent protection device according to claim 11 , wherein the nucleating agent is polytetrafluoroethylene.
13. An overcurrent protection element according to claim 1 or 12, wherein the overcurrent protection element has a first trigger current thermal drop ratio of 65% to 79%, wherein the first trigger current thermal drop ratio is defined as the trigger current required by the overcurrent protection element in an environment of 85°C divided by the trigger current required by the overcurrent protection element in an environment of 25°C, and converted into a percentage.
14. The overcurrent protection element according to claim 13, wherein the overcurrent protection element has a second trigger current thermal drop ratio of 53% to 60%, wherein the second trigger current thermal drop ratio is defined as the trigger current required by the overcurrent protection element in an environment of 125°C divided by the trigger current required by the overcurrent protection element in an environment of 25°C, and converted into a percentage.
15. The overcurrent protection element according to claim 14, wherein the overcurrent protection element has a third trigger current thermal drop ratio of 69% to 82%, wherein the third trigger current thermal drop ratio is defined as the trigger current required by the overcurrent protection element in an environment of 125°C divided by the trigger current required by the overcurrent protection element in an environment of 85°C, and converted into a percentage.
16. The overcurrent protection element according to claim 15, wherein the thermistor layer further comprises a flame retardant selected from the group consisting of zinc oxide, antimony oxide, aluminum oxide, silicon oxide, calcium carbonate, magnesium sulfate or barium sulfate, magnesium hydroxide, aluminum hydroxide, calcium hydroxide and barium hydroxide, and the volume percentage of the flame retardant is 9% to 13% based on the volume of the thermistor layer as 100%.
17. The overcurrent protection device according to claim 16, wherein the flame retardant is magnesium hydroxide.
18. The overcurrent protection element according to claim 16, wherein the overcurrent protection element has a withstand voltage value of 24V, and can pass a cycle life test set with the withstand voltage value without burning out, wherein the cycle life test is applied with a power of 24V / 40A for 500 cycles.
19. The over-current protection device according to claim 18, wherein the over-current protection device has a power handling capacity per unit area of 1.9 W / mm at 25°C. 2 Up to 2.7W / mm 2 .
20. The overcurrent protection device according to claim 19, wherein the overcurrent protection device has a power tolerance per unit area of 1 W / mm at 125°C. 2 Up to 1.5W / mm 2 .