Overcurrent protection element
By using fluoropolymers and carbon black materials in overcurrent protection elements to adjust the resistance start-up temperature, the problem of insufficient thermal stability in the prior art is solved, and delaying current cutoff and effective protection of automotive electronics in high temperature environments is achieved. Effect of components.
Patent Information
- Application Number
- CN202310654856.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-16
- Filing Date
- 2023-06-05
- Publication Date
- 2024-11-22
AI Technical Summary
The existing overcurrent protection components are insufficient thermal stability in high temperature environments and cannot meet the protection needs of automotive electronic components. Especially at normal operating temperatures of 150℃ to 160℃, it is easy to cut off the current too early, causing the electronic components to stop. run.
Using fluoropolymer in polymer substrate as the material of the thermistor layer, adjust the resistance start-up temperature to between 184°C and 192°C, and reach the highest resistance value when it is higher than 208°C, combining carbon black and Metal compounds act as conductive fillers to form an efficient thermistor layer to delay current cutoff.
Improve the thermal stability and resistance stability of overcurrent protection components, ensure that the automotive electronic components operate normally in high temperature environments, avoid premature cutoff current and solder softening problems, and effectively cut off current at high temperature to meet high temperature overheating Protection needs.
Smart Images

Figure CN119008150A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an overcurrent protection element, and more particularly to an overcurrent protection element with high operating temperature and low volume resistivity. Background Art
[0002] The resistance of existing conductive composite materials with positive temperature coefficient (PTC) characteristics is very sensitive to changes in specific temperature. They can be used as materials for current sensing elements and are currently widely used in overcurrent protection elements or circuit elements. Specifically, the resistance of PTC conductive composite materials can be maintained at an extremely low value at normal temperature, allowing the circuit or battery to operate normally. However, when the circuit or battery has an overcurrent (over-current) or overtemperature (over-temperature) phenomenon, its resistance value will instantly increase to a high resistance state (at least 10 4 Ω or more), which is called a trip, and the overcurrent is cut off to protect the battery or circuit components.
[0003] The most basic structure of an overcurrent protection element is composed of a PTC material layer and metal electrodes attached to both sides of it. The PTC material layer will at least include a substrate and a conductive filler. The substrate is composed of a high molecular polymer, and the conductive filler is dispersed in the high molecular polymer as a conductive path. According to the type of high molecular polymer, it can be further divided into low operating temperature and high operating temperature polymers according to the operating temperature. The operating temperature is also called the resistor trip temperature, which refers to the time when the resistance value begins to rise sharply (between about 10 -1 Ω and 10 1 Ω). At this stage, the commonly used low operating temperature polymer is high-density polyethylene, and the high operating temperature polymer is polyvinylidene fluoride. However, the operating temperatures of the two are approximately 120°C and 160°C, respectively, which do not meet the needs of the automotive market for high-temperature overheat protection. The reason is that the normal operating temperature of several electronic components included in automotive electronic modules can reach about 150°C to 160°C. If the operating temperature of the overcurrent protection element is lower than or around 160°C, it means that the current of the overcurrent protection element will be gradually or completely cut off before the temperature rises to this temperature, causing the automotive electronic components that were originally able to operate normally to stop operating.
[0004] In summary, there is still considerable room for improvement in the operating temperature and thermal stability of existing overcurrent protection devices. Summary of the invention
[0005] The present invention provides a high temperature resistant overcurrent protection element, which is particularly suitable as a protection element for automotive components. The overcurrent protection element has a thermistor layer showing a positive temperature coefficient characteristic, and the thermistor layer has a high molecular polymer substrate and a low volume resistivity type conductive filler (i.e., a combination of carbon black and metal compounds). It should be particularly noted that the high molecular polymer substrate of the present invention is mainly composed of a fluorine-containing polymer. This fluorine-containing polymer has a higher resistance starting temperature, which means that the temperature starting point at which the resistance begins to rise sharply is higher. Under appropriate proportions, the resistance starting temperature of the overcurrent protection element can be adjusted to a specific temperature range (between about 184°C and 192°C). In other words, the resistance value of the overcurrent protection element will begin to rise sharply in the aforementioned temperature range, and will only rise to the highest value at a temperature higher than this temperature range (above about 208°C).
[0006] According to one embodiment of the present invention, an overcurrent protection element comprises an electrode layer and a thermistor layer. The electrode layer comprises an upper metal layer and a lower metal layer. The thermistor layer contacts the upper metal layer and the lower metal layer and is stacked therebetween. The thermistor layer has a positive temperature coefficient characteristic and comprises a polymer matrix and a conductive filler. The polymer matrix comprises a first fluorine-containing polymer and enables the overcurrent protection element to have a resistance trip temperature between 184°C and 192°C. The conductive filler comprises carbon black and a metal compound filler dispersed in the polymer matrix to form a conductive path of the thermistor layer.
[0007] According to some embodiments, the polymer matrix does not include polyvinylidene fluoride, and the overcurrent protection element has a resistance peak temperature greater than 208°C.
[0008] According to some embodiments, the first fluoropolymer has a melting point below 240°C.
[0009] According to some embodiments, the first fluorine-containing polymer is ethylene-tetrafluoroethylene copolymer, and the overcurrent protection element has a resistance peak temperature greater than 208°C.
[0010] According to some embodiments, based on 100% of the volume of the thermistor layer, the volume percentage of the ethylene-tetrafluoroethylene copolymer is 42% to 49%.
[0011] According to some embodiments, based on 100% of the volume of the thermistor layer, the volume percentage of the metal compound is 33% to 40%.
[0012] According to some embodiments, the polymer matrix further comprises a second fluorine-containing polymer. The second fluorine-containing polymer is selected from the group consisting of polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, perfluorocarbon oxide-modified tetrafluoroethylene, difluoroethylene-tetrafluoroethylene polymer, tetrafluoroethylene-perfluorodioxole copolymer, difluoroethylene-hexafluoropropylene copolymer, difluoroethylene-hexafluoropropylene-tetrafluoroethylene terpolymer, and mixtures or copolymers of any combination thereof. Based on the volume of the thermistor layer being 100%, the volume percentage of the second fluorine-containing polymer is 4% to 6%.
[0013] According to some embodiments, the polymer matrix does not include poly(chlorotrifluorotetrafluoroethylene).
[0014] According to some embodiments, the second fluoropolymer is polytetrafluoroethylene.
[0015] According to some embodiments, the first fluoropolymer has a melt flow index between 20 g / 10 min and 30 g / 10 min at a temperature of 297° C.
[0016] According to some embodiments, the overcurrent protection element has a peak resistance equal to or greater than 1×10 7 Ω.
[0017] According to some embodiments, the peak resistance is 1×10 7 Ω to 3×10 7 Ω.
[0018] According to some embodiments, after being triggered for the first time and cooled back to room temperature, the overcurrent protection element has a volume resistivity of 0.02 Ω·cm to 0.09 Ω·cm.
[0019] According to some embodiments, under the conditions of the first cycle life test, the overcurrent protection element has a resistance jump rate of 2.1 to 2.5. The first cycle life test includes performing a specific number of cycles of applied power, wherein the applied power is 24V / 40A and the specific number of cycles is 200 times. The resistance jump rate is defined as the post-trigger resistance value divided by the initial resistance value, wherein the overcurrent protection element has the initial resistance value at room temperature when not triggered, and the overcurrent protection element has the post-trigger resistance value after the first cycle life test and cooled to room temperature.
[0020] According to some embodiments, the resistance jump ratio is 2.4 to 2.5.
[0021] According to some embodiments, the overcurrent protection element can be subjected to a second cycle life test without burning out. The second cycle life test includes performing a specific number of cycles of applied power, wherein the applied power is 24V / 40A and the specific number of cycles is 500 times.
[0022] According to some embodiments, the overcurrent protection element can be subjected to a third cycle life test without burning out. The third cycle life test includes performing a specific number of cycles of applied power, wherein the applied power is 30V / 30A and the specific number of cycles is 100 times.
[0023] According to some embodiments, the overcurrent protection element has a first thermal drop ratio of 0.51 to 0.66. The first thermal drop ratio is defined as the required trigger current of the overcurrent protection element at 23°C divided by the required trigger current of the overcurrent protection element at -40°C.
[0024] According to some embodiments, the overcurrent protection device has a second thermal drop ratio of 0.63 to 0.73. The second thermal drop ratio is defined as the trigger current required by the overcurrent protection device at 125°C divided by the trigger current required by the overcurrent protection device at 85°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A cross-sectional view showing an overcurrent protection element according to an embodiment of the present invention;
[0026] Figure 2 show Figure 1 a top view of an overcurrent protection element; and
[0027] Figure 3 and Figure 4 Displays the resistance value-temperature curve of the overcurrent protection element.
[0028] The reference numerals are described as follows:
[0029] 10: Overcurrent protection element
[0030] 11: Thermistor layer
[0031] 12: Upper metal layer
[0032] 13: Lower metal layer
[0033] A: Length
[0034] A0: Intersection point
[0035] A1, A2, A3: Resistance starting points
[0036] A1', A2', A3': highest resistance points
[0037] B: Width
[0038] L1: First tangent
[0039] L2: Second tangent DETAILED DESCRIPTION
[0040] In order to make the above and other technical contents, features and advantages of the present invention more clearly understood, relevant embodiments are given below and described in detail with reference to the accompanying drawings.
[0041] Please refer to Figure 1 , showing the basic state of the overcurrent protection element of the present invention. The overcurrent protection element 10 includes a thermistor layer 11 and an electrode layer. The thermistor layer 11 has an upper surface and a lower surface, and the electrode layer has an upper metal layer 12 and a lower metal layer 13 respectively attached to the upper surface and the lower surface of the thermistor layer 11. In this way, the thermistor layer 11 is physically in direct contact with the upper metal layer 12 and the lower metal layer 13, and is stacked between the two. In one embodiment, the upper metal layer 12 and the lower metal layer 13 can be composed of nickel-plated copper foil or other conductive metals. In addition, the thermistor layer 11 includes a polymer substrate and a conductive filler. The polymer substrate is an insulator that is easily expanded by heat, and the conductive filler is a conductor, whereby the thermistor layer 11 has a positive temperature coefficient characteristic. When the overcurrent protection element 10 is not activated, the conductive filler is evenly dispersed in the polymer matrix and connected in series to form a conductive path; when the overcurrent protection element 10 is affected by high temperature, the polymer matrix will expand rapidly, causing the conductive filler particles to be pulled apart from each other, resulting in the truncation of the conductive path.
[0042] In other words, the type of polymer matrix and its ratio relative to the conductive filler roughly determine the positive temperature coefficient characteristics of the thermistor layer 11. Accordingly, the polymer matrix of the present invention includes a specific fluorinated polymer (hereinafter referred to as the first fluorinated polymer). Through appropriate proportion adjustment, the first fluorinated polymer can make the resistance trip temperature of the overcurrent protection element 10 fall within the first temperature range of 184°C to 192°C. Considering the influence of reproducibility errors, the resistance trip temperature in the present invention can be adjusted to 186°C to 190°C. The resistance trip temperature refers to the starting temperature point corresponding to when the resistance value begins to rise sharply. At this temperature, the resistance value of the overcurrent protection element 10 has not yet risen to the highest, but it is the starting point for the sudden rise. Then, as the temperature continues to rise and exceeds 208°C, the overcurrent protection element 10 will present a stable high resistance state (that is, the resistance value is about 10 7 Ω or more), and has the highest resistance value in the second temperature range. The aforementioned highest resistance value is also called the resistance peak value, and the temperature point corresponding to the resistance peak value is called the resistance peak temperature, which falls within the range of the second temperature range. In the present invention, the resistance peak value is 1×10 7 Ω to 3×10 7 Ω, and the resistance peak temperature is between 208℃ and 218℃.
[0043] It should be noted that when the car is running, its internal core temperature can be as high as 180°C, so automotive electronic components can generally operate normally between 150°C and 160°C. Therefore, the resistor trip temperature of the overcurrent protection element 10 needs to be adjusted to a higher temperature accordingly, but it cannot be unlimited. For example, when the resistor trip temperature is lower than 184°C, the starting point where the resistance value of the overcurrent protection element 10 begins to rise sharply is too close to the temperature at which the automotive electronic components can operate normally. This greatly increases the possibility that the overcurrent protection element 10 cuts off the current prematurely. Furthermore, before the temperature reaches the resistor trip temperature, although the resistance value of the overcurrent protection element 10 has not risen sharply, it has begun to rise slowly. Therefore, the resistor trip temperature is too close to 150°C to 160°C, which has already affected the normal operation of automotive electronic components.
[0044] If the resistor tripping temperature is higher than 192°C, there will be a problem of tin melting. In more detail, the melting point of the solder used when the overcurrent protection element 10 is assembled to the circuit board (or other supporting objects) is generally lower than 260°C, and it begins to soften and undergo a phase change at about 230°C. If the resistor tripping temperature of the overcurrent protection element 10 is too close to 230°C, it will take too long to completely cut off the current, causing the temperature to rise too high. This high temperature may cause the solder to soften or even melt, causing the overcurrent protection element 10 to fall off the circuit board (or other supporting objects).
[0045] In addition, considering the demand for high-temperature overheat protection in the automotive market, the polymer substrate of the present invention does not use polyvinylidene fluoride (melting point of about 177°C) with a relatively low melting point. As for the first fluorine-containing polymer in the polymer substrate of the present invention, an ethylene-tetrafluoroethylene copolymer with a melting point below 240°C can be used. It should be understood that, depending on the polymerization method, the ethylene-tetrafluoroethylene copolymer may have different melting points, which may be as high as above 280°C or as low as below 240°C. In addition to the reasons for the aforementioned resistance starting temperature, the present invention selects a low-melting-point ethylene-tetrafluoroethylene copolymer, also taking into account the problem of process processing. If the melting point of the ethylene-tetrafluoroethylene copolymer is higher than 240°C, the structure of the material after the polymer substrate and the conductive filler are mixed will be too stable at high temperatures, resulting in difficulties in hot pressing. In one embodiment, the melting point of the ethylene-tetrafluoroethylene copolymer is preferably 220°C to 230°C; and according to the standard specification of ASTM D3159, at a temperature of 297°C, the ethylene-tetrafluoroethylene copolymer has a melt flow index between 20g / 10min and 30g / 10min. The aforementioned melt flow index may also be referred to as melt flow rate, which refers to the number of grams of melt that flows through a standard capillary per ten minutes, and can be used to evaluate the fluidity of the polymer in a molten state. The higher the melt flow index, the better the melt fluidity. Conversely, the lower the melt flow index, the worse the melt fluidity. Generally speaking, the ethylene-tetrafluoroethylene copolymer with a melting point above 240°C has a melt flow index below 20g / 10min, and has poor fluidity during hot pressing.
[0046] In addition, the thermistor layer 11 of the present invention may further include a second fluoropolymer (hereinafter referred to as the second fluoropolymer), which is also used as the composition of the polymer matrix of the thermistor layer 11. The conductive filler is dispersed in the polymer matrix composed of the first fluoropolymer and the second fluoropolymer to form the conductive path of the thermistor layer 11. The second fluoropolymer is selected from the group consisting of a mixture or copolymer of polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, perfluorocarbon oxide modified tetrafluoroethylene, difluoroethylene-tetrafluoroethylene polymer, tetrafluoroethylene-perfluorodioxole copolymer, difluoroethylene-hexafluoropropylene copolymer, difluoroethylene-hexafluoropropylene-tetrafluoroethylene terpolymer and any combination thereof. For example, the second fluoropolymer can be selected from polytetrafluoroethylene. Therefore, in the present invention, the first fluoropolymer can use ethylene-tetrafluoroethylene copolymer as the main component of the polymer matrix, and the second fluoropolymer can use polytetrafluoroethylene as the secondary component of the polymer matrix. That is, in the polymer matrix, the content of ethylene-tetrafluoroethylene copolymer is higher than that of polytetrafluoroethylene; therefore, based on the volume of the thermistor layer as 100%, the volume percentage of ethylene-tetrafluoroethylene copolymer is 42% to 49%, while polytetrafluoroethylene accounts for 4% to 6%. In one embodiment, based on the volume of the thermistor layer 11 as 100%, ethylene-tetrafluoroethylene copolymer accounts for 42%, 43%, 44%, 45%, 46%, 47%, 48% or 49%. In one embodiment, based on the volume of the thermistor layer 11 as 100%, polytetrafluoroethylene accounts for 4%, 4.5%, 5%, 5.5% or 6%. The melting point of polytetrafluoroethylene (about 320°C to 335°C) is much higher than that of ethylene-tetrafluoroethylene copolymer. Considering the needs of automotive components, the content of polytetrafluoroethylene in the aforementioned ratio range will not be so high as to affect the resistor tripping temperature of the overcurrent protection element 10, but at the same time it can fine-tune the overall thermal stability of the polymer matrix. It should also be mentioned that, based on process considerations, the present invention does not use poly(chlorotri-fluorotetrafluoroethylene) as the second fluorine-containing polymer. That is, the polymer matrix does not contain poly(chlorotri-fluorotetrafluoroethylene). When poly(chlorotri-fluorotetrafluoroethylene) is closely kneaded with other materials (ethylene-tetrafluoroethylene copolymer and other fillers), it is easy to break, crack or produce smoke, so it is not suitable for the present invention.
[0047] As for the conductive filler, the present invention uses metal compounds as the main component and carbon black as the secondary component to improve the conductivity of the overcurrent protection element 10. The conductive filler includes carbon black and metal compound fillers dispersed in a high molecular polymer matrix to form a conductive path of the thermistor layer 11. Moreover, based on the volume of the thermistor layer as 100%, the volume percentage of the metal compound is 33% to 40%. The metal compound is selected from the group consisting of tungsten carbide, titanium carbide, vanadium carbide, zirconium carbide, niobium carbide, tantalum carbide, molybdenum carbide, hafnium carbide, titanium boride, vanadium boride, zirconium boride, niobium boride, molybdenum boride, hafnium boride, zirconium nitride and any combination thereof. In one embodiment, in order to make the overcurrent protection element 10 have better withstand voltage characteristics, the conductive filler may also include a small amount of carbon black. For example, based on the volume of the thermistor layer as 100%, the conductive filler further includes about 2% to 8% of carbon black. In addition, the present invention has observed that in the combination of conductive fillers, the use of metal carbides (especially tungsten carbide) and carbon black can enable the overcurrent protection element 10 to maintain a low volume resistivity while having better voltage resistance characteristics.
[0048] As mentioned above, Figure 1 The overcurrent protection element 10 is only the most basic state and can be processed arbitrarily later. The processing process often involves high temperature, which leads to the triggering of the overcurrent protection element 10. After the overcurrent protection element 10 is triggered, even if it is cooled back to room temperature, its resistance value will increase and cannot be restored to the initial resistance value. The better the resistance stability of the overcurrent protection element 10, the easier it is for its resistance value to recover to a low resistance state as the temperature gradually decreases. The present invention has observed that the thermistor layer 11 composed of the above-mentioned materials can not only accurately control the resistance starting temperature, but also enhance the resistance stability of the overcurrent protection element 10. For example, the overcurrent protection element 10 can be welded with pins on the upper metal layer 12 and the lower metal layer 13 respectively. The high temperature of welding will cause the overcurrent protection element 10 to be triggered for the first time. In the present invention, the overcurrent protection element 10 has a volume resistivity of 0.02 Ω·cm to 0.09 Ω·cm when it is first triggered and cooled back to room temperature, which is much smaller than the volume resistivity of conventional overcurrent protection elements for high temperatures (about 0.2 Ω·cm to 0.4 Ω·cm). Obviously, after processing, the overcurrent protection element 10 of the present invention can maintain good conductive properties when not in operation, and will not affect the normal operation of other electronic components. In one embodiment, the overcurrent protection element 10 preferably has a volume resistivity of 0.02 Ω·cm to 0.06 Ω·cm, for example, 0.0297 Ω·cm to 0.0535 Ω·cm.
[0049] In addition, the overcurrent protection element 10 of the present invention further includes several other electrical characteristics. The following is an explanation of three cycle life tests and two thermal derating tests. The cycle life test is divided into a first cycle life test, a second cycle life test, and a third cycle life test according to different test conditions. The thermal derating test is divided into a first thermal derating test and a second thermal derating test according to different test conditions.
[0050] Under the conditions of the first cycle life test, the overcurrent protection element 10 has a resistance jump rate of 2.1 to 2.5. More specifically, the conditions of the first cycle life test are that after the voltage / current of 24V / 40A is applied for 10 seconds, it is closed for 60 seconds as one cycle. In this way, 200 cycles are repeated. The resistance jump rate is defined as the resistance value after the overcurrent protection element 10 is triggered divided by the initial resistance value of the overcurrent protection element 10. The overcurrent protection element 10 has an initial resistance value at room temperature when it is not triggered, and has a post-trigger resistance value after the first cycle life test and cooled to room temperature. The resistance jump rate can be used to evaluate the resistance stability of the overcurrent protection element 10. In all embodiments of the present invention, the resistance jump rate can be stably maintained at 2.1 to 2.5. In contrast, the traditional overcurrent protection element for high temperature is likely to fail to pass the first cycle life test due to insufficient voltage resistance. Even if it can pass the first cycle life test, its volume resistivity is too high and does not meet the application requirements. In one embodiment, the resistance jump rate of the over-current protection element 10 of the present invention is preferably 2.4 to 2.5.
[0051] Under the conditions of the second cycle life test, the overcurrent protection element 10 of the present invention has better withstand voltage characteristics without burning. The second cycle life test differs from the first cycle life test only in the number of cycles. The second cycle life test increases the number of cycles to 500 times to observe whether the overcurrent protection element 10 can withstand more high-energy impacts. Although the overcurrent protection element used for low temperature overheating protection can pass the second cycle life test, it cannot pass the second cycle life test when it is traditionally improved to meet the requirements of high temperature overheating protection applications (for example: using polyvinylidene fluoride as the main component of the polymer substrate).
[0052] Under the conditions of the third cycle life test, the overcurrent protection element 10 of the present invention also has better withstand voltage characteristics without burning. The applied power and number of cycles of the third cycle life test are changed to observe the situation of the overcurrent protection element 10 under different powers and different numbers of cycles. More specifically, the conditions of the third cycle life test are 30V / 30A voltage / current applied for 10 seconds, and then closed for 60 seconds as a cycle. In this way, 100 cycles are repeated. Under this power and number of cycles, the overcurrent protection element 10 of the present invention can still operate normally without burning. In comparison, the traditional overcurrent protection element used for high-temperature overheating protection is likely to fail to pass the third cycle life test. Even if it can pass the third cycle life test, its volume resistivity is too high to meet the application requirements.
[0053] The thermal drop test is used to compare the difference in the trigger current of the overcurrent protection element 10 under different ambient temperatures, thereby evaluating the impact of high temperature on operability. Ideally, it is expected that the trigger current of the overcurrent protection element 10 can be maintained at the same value under various temperatures, stabilized at the preset trigger current to play a protective role, and facilitate operation. The ambient temperatures used for comparison in the first thermal drop test are 23°C and -40°C, while the ambient temperatures used for comparison in the second thermal drop test are 125°C and 85°C.
[0054] In the first thermal drop test, the overcurrent protection element 10 has a first thermal drop ratio of 0.51 to 0.66. The first thermal drop ratio is defined as the trigger current required by the overcurrent protection element 10 in an environment of 23°C divided by the trigger current required by the overcurrent protection element 10 in an environment of -40°C. In the second thermal drop test, the overcurrent protection element 10 has a second thermal drop ratio of 0.63 to 0.73. The second thermal drop ratio is defined as the trigger current required by the overcurrent protection element 10 in an environment of 125°C divided by the trigger current required by the overcurrent protection element in an environment of 85°C. As can be seen from the foregoing, the first thermal drop ratio shows the thermal drop of the overcurrent protection element 10 in a low temperature range, while the second thermal drop ratio shows the thermal drop of the overcurrent protection element 10 in a high temperature range. In the low temperature range, the overcurrent protection element 10 of the present invention is not much different from the traditional overcurrent protection element; but in the high temperature range, the second thermal drop ratio of the overcurrent protection element 10 of the present invention is much higher than the second thermal drop ratio of the traditional overcurrent protection element. The second heat drop ratio of the overcurrent protection element 10 of the present invention can even reach about 0.73, but the second heat drop ratio of the conventional overcurrent protection element is about 0.55 or less. It can be seen that compared with the conventional overcurrent protection element, the thermal stability of the overcurrent protection element 10 of the present invention is greatly improved, and its operability is less susceptible to high temperature.
[0055] Please continue to refer to Figure 2 ,for Figure 1 The overcurrent protection element 10 has a length A and a width B, and the area "A×B" is also equal to the area of the thermistor layer 11. The thermistor layer 11 may have a top view area of 4mm depending on the product model. 2 Up to 72mm 2 For example, the area "A x B" can be 2 x 2 mm 2 , 5×5mm 2 、5.1×6.1mm 2 , 5×7mm 2 、7.62×7.62mm 2 、8.2×7.15mm 2 、7.3×9.5mm 2 or 7.62×9.35mm 2 In addition, the overall thickness of the overcurrent protection element 10 (i.e., the sum of the thicknesses of the upper metal layer 12, thermistor layer 11, and the lower metal layer 13) is between 0.5 mm and 0.6 mm. For example, the top surface area of the overcurrent protection element 10 may be 35 mm. 2 (ie 5×7mm 2 ), and the thickness is 0.55 mm. In another embodiment, the top surface area of the overcurrent protection element 10 may be 25 mm 2 (ie 5×5mm 2 ), and the thickness is 0.5 mm. It should be understood that the overcurrent protection element 10 of the present invention has the same effect when applied to the above dimensions.
[0056] As described above, the present invention can make the overcurrent protection element 10 have good electrical characteristics at high temperatures. The following Tables 1 to 6 further illustrate the actual verification data.
[0057] Table 1. Main polymers of polymer matrix
[0058] polymer Melt flow index (g / 10min) Melting point(℃) ETFE 25 225 PVDF-1 3 168 PVDF-2 1.1 185 HDPE 1 134
[0059] Table 2. Formula ratio of thermistor layer 11 (vol%)
[0060] Group ETFE PVDF-1 PVDF-2 HDPE PTFE <![CDATA[Mg(OH)2]]> CB WC E1 45 5 5 833 E2 48 5 6 734 E3 46 5 8 536 E4 43 5 10 240 C1 43 5 10 240 C2 43 5 10 240 C3 56 540
[0061] As shown in Table 1, the main types of polymers used in high molecular polymer substrates are ethylene-tetrafluoroethylene copolymer (ETFE), two types of polyvinylidene difluoride (PVDF) and high density polyethylene (HDPE). The melt flow index is measured according to different specifications depending on the polymer. The melt flow index of polytetrafluoroethylene is measured according to the standard specification of ASTM D3159, while the melt flow index of polyvinylidene fluoride and high density polyethylene is measured according to the standard specification of ASTMD1238. As can be seen from Table 1, polytetrafluoroethylene has the highest melting point, and it still has a stable shape and structure above 185°C, and has good fluidity at high temperatures, which will not cause difficulties in the dense mixing and hot pressing process.
[0062] Continuing to refer to Table 2, Table 2 shows the formula ingredients of thermistor layer 11 of each embodiment of the present invention (group E1 to group E4) and comparative examples (group C1 to group C3) in volume percentage. The first column shows each group from top to bottom, namely, embodiment E1 to comparative example C3. The first row shows the various material ingredients in thermistor layer 11 from left to right, which are ethylene-tetrafluoroethylene copolymer (ETFE), polyvinylidene fluoride (PVDF-1 and PVDF-2), high-density polyethylene, polytetrafluoroethylene (Polytetrafluoroethylene, PTFE), magnesium hydroxide (Magnesium hydroxide, Mg(OH)2), carbon black (Carbon black, CB) and tungsten carbide (Tungsten carbide, WC). In addition, each group uses magnesium hydroxide as a flame retardant. As for the conductive filler, in order to improve the conductivity of the element, tungsten carbide is mainly used, and carbon black is secondary. Therefore, the combination of tungsten carbide and carbon black can be generally called a low volume resistivity conductive filler.
[0063] In the embodiments E1 to E4 of the present invention, the main component of the high molecular polymer matrix is ETFE, and the secondary component is PTFE. Since PTFE has a melting point much higher than that of ETFE (about 330°C), the proportion of PTFE should not be too large to avoid affecting the protection temperature (such as the resistor tripping temperature and the resistor peak temperature) and other triggering characteristics of the overcurrent protection element. In other words, the relative proportion of ETFE and PTFE must be appropriately adjusted. Specifically, the volume percentage of ETFE:PTFE is about 89:11 to 91:9. That is, when the total volume of ETFE and PTFE is 100%, the volume percentage of ETFE is 89% to 91%, and the volume percentage of PTFE is 9% to 11%. It should also be noted that the volume percentage of the high molecular polymer matrix (i.e., ETFE and PTFE) in the thermistor layer 11 also needs to be adjusted within an appropriate range. If it is too low, the current cannot be completely cut off when triggered, and if it is too high, the conductivity will be poor. In this formulation, the volume percentage of the polymer matrix in the thermistor layer 11 is 48% to 53%. Considering the influence of the error and the results of practical applications, the volume percentage of the polymer matrix is 45% to 55% and can achieve the same technical effect.
[0064] In Comparative Examples C1 and C2, the main component of the polymer substrate is PVDF, and the minor component is PTFE. Traditionally, different polyvinylidene fluorides are used to adjust the high-temperature stability of the overcurrent protection element, so two commonly used polyvinylidene fluorides are selected for comparison in Table 2. PVDF-1 in Comparative Example C1 has a lower melting point and a higher melt flow index, while PVDF-2 in Comparative Example C2 has a higher melting point and a lower melt flow index. Subsequent experiments will show that the electrical properties of both cannot meet the needs of the automotive market. As for Comparative Example C3, the polymer substrate is composed of HDPE. It is known that HDPE has a low melting point and a lower trigger temperature. Traditionally, Comparative Example 3 is an overcurrent protection element for low-temperature overheat protection, which is used to show that it cannot be used in automotive market applications for high-temperature overheat protection.
[0065] The preparation process of the overcurrent protection elements of Examples E1 to E4 and Comparative Examples C1 to C3 is described as follows. First, based on the formula presented in Table 1, the materials in the formula are added to a twin-screw mixer produced by HAAKE for mixing. The mixing temperature of the embodiment is 240°C, while the mixing temperature of the comparative example is 215°C. The premixing time is 3 minutes, and the mixing time is 15 minutes. After the mixing is completed, a conductive polymer can be obtained, and a hot press is used at high temperature (250°C for the embodiment and 210°C for the comparative example) and 150kg / cm 2The sheets were then cut into squares of about 20 cm x 20 cm. Next, the sheets were pressed into thin sheets using a hot press at high temperature (250°C for the example and 210°C for the comparative example) and 150 kg / cm 2 The two nickel-plated copper foils are pressed onto the two sides of the conductive polymer sheet with a pressure of 100° to form a three-layer plate. Finally, a punch is used to punch out multiple chips from the plate, which are the overcurrent protection components. The length and width of the overcurrent protection component are 5mm and 7mm respectively (i.e., the top surface area is 35mm). 2 ), and the thickness is 0.55 mm. Then, the chips prepared in the embodiment and the comparative example were irradiated with a light dose of 50 kGy (the light dose can be adjusted according to the needs and is not a limiting condition of the present invention), and 15 chips were taken as test samples for subsequent experiments.
[0066] It should be noted again that the selection of polymer substrates is not based solely on their physical properties at high temperatures (such as the melt flow index and melting point in Table 1), but also on the compatibility between polymers (such as ETFE and PTFE) and between polymers and fillers (such as Mg(OH)2, CB and WC). Based on the aforementioned physical properties and compatibility, it is necessary to adjust the appropriate ratio so that the electrical properties of the overcurrent protection element 10 meet the application requirements. Tables 3 to 6 further illustrate the electrical properties of the overcurrent protection element 10.
[0067] Table 3. Trigger temperature and its resistance peak value
[0068] Group Resistance tripping temperature (℃) Resistance peak temperature (℃) Peak resistance(Ω) E1 188 212 <![CDATA[1×10 7 ]]> E2 188 212 <![CDATA[1×10 7 ]]> E3 188 212 <![CDATA[3×10 7 ]]> E4 188 212 <![CDATA[2×10 7 ]]> C1 150 160 <![CDATA[3×10 5 ]]> C2 168 174 <![CDATA[1×10 6 ]]> C3 124 130 <![CDATA[1×10 8 ]]>
[0069] Please also refer to Table 3. Figure 3 and Figure 4 . Figure 3 The resistance value-temperature curve of the overcurrent protection element 10 is shown. The Y axis shows the resistance value, and the X axis shows the temperature. More specifically, the present invention performs a resistance-temperature test on the overcurrent protection element 10. Under the condition of a heating rate of 5°C / min, a resistance-temperature curve of the overcurrent protection element 10 is obtained. It should be noted that Figure 3 and Figure 4 The Y axis of the embodiment adopts a logarithmic scale, so the curves of the embodiments E1 to E4 are almost overlapped. Figure 3 In the figure, a single curve is used to present the average values of all the examples. In addition, the polymer substrates of Comparative Examples C1 and C2 both use the same main polymer (i.e., PVDF). To make the layout simpler, cleaner, and easier to explain, only the curve of Comparative Example C2 is presented. Figure 3Point A1, point A2 and point A3 are the starting points where the resistance is about to rise suddenly, that is, the resistance jump point. The temperature point corresponding to the resistance jump point is the resistance jump temperature (℃) in Table 1. Point A1', point A2' and point A3' are the apex where the resistance rises suddenly to the highest point, that is, the highest point of resistance. The temperature and resistance value corresponding to the highest point of resistance are the resistance peak temperature (℃) and resistance peak value (Ω) in Table 1, respectively. In Example E1 to Example E4, the resistance jump temperature is 188℃, and the resistance peak temperature is 212℃, which just meets the temperature requirements of automotive components. That is to say, in the temperature range (about 150℃ to 160℃) in which automotive components can operate normally, the overcurrent protection element 10 of Example E1 to Example E4 will not start to work. Before reaching the melting point of solder, the resistance value of the overcurrent protection element 10 of Example E1 to Example E4 will jump to the highest at around 212℃, that is, about 1×10 7 Ω to 3×10 7 Ω resistance peak; at this time, the current will be completely cut off without the problem of tin melting. In contrast, the resistor tripping temperature of Comparative Examples C1 and C2 is about 150℃ to 168℃, and they will start to operate at the normal operating temperature of the automotive components, affecting the normal operation of the automotive components; and if there is an unexpected incident that causes the temperature to rise to 200℃ in a short period of time (the time when the protection function has no time to react), Comparative Examples C1 and C2 are actually prone to rupture due to the poor thermal stability of the overcurrent protection components. As for Comparative Example 3, it will start to operate at a relatively low temperature (124℃), causing the automotive components to be unable to operate normally, which is completely incompatible with the temperature requirements of the automotive market.
[0070] Please continue to refer to Figure 4, further illustrating the definition of the resistor tripping temperature in embodiments E1 to E4 of the present invention. In the low resistance state before the overcurrent protection element 10 is triggered, this curve will show a straight linear climb in a certain temperature section in the low resistance state, so the tangent L1 can be drawn from this linear climb section. During the period from the overcurrent protection element 10 being triggered to the high resistance state, this curve will show a sharp linear climb in a certain temperature section, so the tangent L2 can also be drawn from this linear climb section. Each point on the tangent L1 conforms to the formula: y=0.002302x+0.005387; and each point on the tangent L2 conforms to the formula: y=9124x-1769929. That is to say, in the linear climb section, the slope of the tangent L1 is 0.002302 (hereinafter referred to as the "lowest slope"); and the slope of the tangent L2 is 9124 (hereinafter referred to as the "highest slope"). The tangent line L1 with the lowest slope and the tangent line L2 with the highest slope intersect at the intersection A0. The temperature point of the intersection A0 corresponding to the X-axis is the switching point between the low resistance state and the high resistance state, that is, the resistance tripping temperature. Therefore, the intersection A0 will overlap with the resistance tripping point A1 when it is vertically translated upward along the Y-axis. According to the formula of the thermistor layer 11 adjusted by the present invention, the resistance tripping temperature under this definition can be accurately controlled within the range of 184°C and 192°C.
[0071] Next, the voltage resistance characteristics of the overcurrent protection element 10 are evaluated through a cycle life test. The cycle life test is based on a certain power applied for 10 seconds and turned off for 60 seconds as one cycle. In the following experiments, the cycle life test is divided into three conditions (hereinafter referred to as the first cycle life test, the second cycle life test and the third cycle life test). The conditions of the first cycle life test are 24V / 40A voltage / current and 200 cycles; the conditions of the second cycle life test are 24V / 40A voltage / current and 500 cycles; and the conditions of the third cycle life test are 30V / 30A voltage / current and 100 cycles.
[0072] Table 4. Cycle life test
[0073]
[0074] As shown in Table 4, the first column shows the verification items from left to right.
[0075] R i , refers to the initial resistance value of the overcurrent protection element at room temperature.
[0076] R1 refers to the resistance value measured after the overcurrent protection element is triggered once and then cooled to room temperature. Specifically, the overcurrent protection element is welded to the pins, and the high temperature of welding will cause the overcurrent protection element to be triggered for the first time. In addition, according to the formula of volume resistivity ρ=R×A / L, R is the resistance value, L is the thickness, and A is the area. Based on this, the volume resistivity can be calculated as ρ by R1.
[0077] R 200C , refers to the resistance value measured when the overcurrent protection element is cooled to room temperature after the first cycle life test. Based on this, the resistance jump rate (i.e. R 200C / R i ), the lower the ratio (i.e., the closer it is to 1), the better the ability of the overcurrent protection element to recover to a low resistance state or the resistance recovery. In other words, the resistance jump rate can be used to evaluate the resistance stability.
[0078] 500C and 100C are the device states of the second cycle life test and the third cycle life test, respectively. "Pass" means that the overcurrent protection device is not burned, while "Fail" means that the overcurrent protection device is burned.
[0079] First, please pay attention to R1 and the corresponding ρ. The overcurrent protection element 10 is only the most basic state, and it is often processed later. In actual use, the overcurrent protection element 10 is usually triggered at least once. In other words, R1 and ρ can better reflect the resistance of the overcurrent protection element assembled in the electronic device. In Example E1 to Example E4, the resistance value (R1) of the overcurrent protection element 10 after the first trigger is 0.0047Ω to 0.0138Ω, and the volume resistivity (ρ) is 0.0297Ω·cm to 0.0876Ω·cm, which are much lower than the resistance value (R1) and volume resistivity (ρ) after the first trigger of Comparative Example C1 and Comparative Example C2. In other words, compared with the traditional overcurrent protection element for high-temperature overheating protection, the present invention can maintain good conductive properties when it is not actuated. As for Comparative Example C3, although it can maintain a similar low post-trigger resistance value (R1) and volume resistivity (ρ), as mentioned above, it cannot be applied to devices that require high-temperature overheating protection.
[0080] As for the resistance jump rate (R 200C / R i ), Examples E1 to E4 are all stable and maintained in the approximate range of 2.199 to 2.466. Comparative Example C1 was not obtained due to the burnout of the component. Although Comparative Example C2 has a lower resistance jump rate (R 200C / R i), but its resistance value (R1) and volume resistivity (ρ) are too high (0.0339Ω and 0.2154Ω·cm, respectively) when it is first used in an electronic device. In other words, during the initial normal operation of an electronic device, the amount of current flowing through it is small and the conductive properties are poor. Finally, for comparative example C3, its resistance jump rate (R 200C / R i ) is 3.103, which is much higher than 2.199 to 2.466 of Examples E1 to E4. The overcurrent protection element of Comparative Example C3 not only fails to meet the requirements of high temperature overheating protection, but also has poor resistance stability.
[0081] Under the same power, the present invention further verifies the limit of the number of cycles that the overcurrent protection 10 can withstand by the second cycle life test. The applied power of the second cycle life test is the same as that of the first cycle life test, but the second cycle life test increases the number of cycles from 200 to 500. As can be seen from Table 4, among Examples E1 to E4, only Example E1 can withstand 500 cycles and has the best withstand voltage characteristics. Comparative Examples C1 and C2 both burn out, indicating that the conventional overcurrent protection element used for high-temperature overheating protection has poor withstand voltage characteristics. Finally, the third cycle life test is further used to verify the limits of voltage and power that the overcurrent protection 10 can withstand. Similarly, among Examples E1 to E4, only Example E1 can pass the third cycle life test without burning. Although Comparative Example C2 can pass the third cycle life test, it will burn out in the second cycle life test and its conductive properties are not good, and its performance is not as good as Example E1. It should be noted that although Comparative Example C3 can pass the above three cycle life tests, it is only applicable to low-temperature overheat protection devices and is not suitable for use in high-temperature overheat protection automotive market applications.
[0082] The last test is the thermal drop test, which can show the ability of the overcurrent protection element 10 to resist thermal decay in the triggering characteristics. Thermal drop test 1 is used to verify the thermal drop situation in the low temperature range (-40°C to 23°C), while thermal drop test 2 is used to verify the thermal drop situation in the high temperature range (85°C to 125°C). Details are as follows.
[0083] Table 5. Heat drop test 1
[0084]
[0085] Table 6. Heat drop test 2
[0086]
[0087]
[0088] As shown in Table 5, the first column shows several verification items from left to right.
[0089] IT -40℃ , refers to the trigger current of the overcurrent protection element in a -40℃ environment. Based on this, IT can be obtained -40℃ / area refers to the size of the trigger current per unit area of the overcurrent protection element in a -40°C environment.
[0090] IT 23℃ , refers to the trigger current of the overcurrent protection element at 23°C. Based on this, IT can be obtained 23℃ / area refers to the size of the trigger current per unit area of the overcurrent protection component under a 23°C environment.
[0091] IT 23℃ / IT -40℃ It is used to compare the thermal decay of the current required to trigger under different temperature environments. 23℃ / IT -40℃ Also known as the first thermal drop ratio, the closer it is to 1, the less the trigger current is affected by heat and the higher the thermal stability.
[0092] Table 6 IT 85℃ 、IT 85℃ / area、IT 125℃ 、IT 125℃ / area and IT 125℃ / IT 85℃ The definition of IT -40℃ 、IT -40℃ / area、IT 23℃ 、IT 23℃ / area and IT 23℃ / IT -40℃ Similar, no further praise here. In addition, IT 125℃ / IT 85℃ Also known as the second heat reduction ratio.
[0093] Please pay special attention to the first heat reduction ratio (IT 23℃ / IT -40℃ ) and the second heat reduction ratio (IT 125℃ / IT 85℃). It should be understood that when the overcurrent protection element is placed in a high temperature environment, the resistance will be higher, and the current required for triggering will become smaller accordingly. However, if the current required for triggering varies too much with temperature, it will be detrimental to the operation of the overcurrent protection element. In other words, the smaller the amplitude of the overcurrent protection element's trigger current decreases with temperature, the better the thermal stability of the resistor is, which is conducive to operation. In Table 5, the first thermal drop ratio (IT) of Examples E1 to E4 is 23℃ / IT -40℃ ) is 0.516 to 0.663, which is approximately the same range as that of Comparative Examples C1 to C3. In Table 6, the second heat reduction ratio (IT) of Examples E1 to E4 125℃ / IT 85℃ ) is 0.633 to 0.725, which is much higher than Comparative Examples C1 to C3, where Comparative Example C3 has been activated (triggered) at 125°C and therefore has no data. It can be seen that although the thermal drop of Examples E1 to E4 in the low temperature range (-40°C to 23°C) is similar to that of Comparative Examples C1 to C3, as the temperature rises to the high temperature range (85°C to 125°C), its thermal stability advantage gradually emerges. Thus, the second thermal drop ratio (IT) of Examples E1 to E4 is 125℃ / IT 85℃ ) is still quite close to 1 in the high temperature range (85℃ to 125℃), indicating better thermal stability.
[0094] The technical content and technical features of the present invention have been disclosed as above, but a person skilled in the art with ordinary knowledge may still make various substitutions and modifications based on the teachings and disclosures of the present invention without departing from the spirit of the present invention. Therefore, the protection scope of the present invention should not be limited to those disclosed in the embodiments, but should include various substitutions and modifications without departing from the present invention, and be covered by the following claims.
Claims
1. An overcurrent protection element, comprising: an electrode layer having an upper metal layer and a lower metal layer; and A thermistor layer contacts the upper metal layer and the lower metal layer and is stacked therebetween, wherein the thermistor layer has a positive temperature coefficient characteristic and comprises: A high molecular polymer substrate, comprising a first fluorine-containing polymer, and enabling the overcurrent protection element to have a resistance tripping temperature between 184° C. and 192° C.; and A conductive filler, including carbon black and a metal compound filler, is dispersed in the high molecular polymer matrix to form a conductive channel of the thermistor layer. 2 . The overcurrent protection device according to claim 1 , wherein the polymer substrate does not contain polyvinylidene fluoride, and the overcurrent protection device has a resistance peak temperature greater than 208° C. 3 . 3 . The overcurrent protection device according to claim 1 , wherein the melting point of the first fluorine-containing polymer is lower than 240° C. 4 . 4 . The overcurrent protection device according to claim 3 , wherein the first fluorine-containing polymer is ethylene-tetrafluoroethylene copolymer, and the overcurrent protection device has a resistance peak temperature greater than 208° C. 5 . The overcurrent protection element according to claim 4 , wherein based on the volume of the thermistor layer being 100%, the volume percentage of the ethylene-tetrafluoroethylene copolymer is 42% to 49%. 6 . The overcurrent protection element according to claim 5 , wherein based on the volume of the thermistor layer being 100%, the volume percentage of the metal compound is 33% to 40%.
7. The overcurrent protection device according to claim 6, wherein the polymer substrate further comprises a second fluorine-containing polymer selected from the group consisting of polytetrafluoroethylene, tetrafluoroethylene-hexafluoropropylene copolymer, perfluorocarbon oxide-modified tetrafluoroethylene, difluoroethylene-tetrafluoroethylene polymer, tetrafluoroethylene-perfluorodioxole copolymer, difluoroethylene-hexafluoropropylene copolymer, difluoroethylene-hexafluoropropylene-tetrafluoroethylene terpolymer, and mixtures or copolymers of any combination thereof, and based on the volume of the thermistor layer being 100%, the volume percentage of the second fluorine-containing polymer is 4% to 6%. 8 . The overcurrent protection device according to claim 7 , wherein the high molecular polymer matrix does not contain poly(chlorotrifluorotetrafluoroethylene). 9 . The overcurrent protection device as claimed in claim 7 , wherein the second fluorine-containing polymer is polytetrafluoroethylene.
10. The overcurrent protection device according to claim 1 or 9, wherein at a temperature of 297°C, the first fluorine-containing polymer has a melt flow index between 20 g / 10 min and 30 g / 10 min. 11 . The over-current protection element according to claim 1 or 9 , wherein the over-current protection element has a resistance peak value equal to or greater than 1×10 7 Ω after being triggered. 12 . The overcurrent protection device according to claim 11 , wherein the resistance peak value is 1×10 7 Ω to 3×10 7 Ω. 13 . The overcurrent protection device according to claim 12 , wherein after being triggered for the first time and cooled back to room temperature, the overcurrent protection device has a volume resistivity of 0.02 Ω·cm to 0.09 Ω·cm.
14. The overcurrent protection device according to claim 13, wherein under a first cycle life test condition, the overcurrent protection device has a resistance jump rate of 2.1 to 2.5, wherein: The first cycle life test includes performing an applied power for a specific number of cycles, the applied power is 24V / 40A and the specific number of cycles is 200 times; and The resistance jump rate is defined as a post-trigger resistance value divided by an initial resistance value, wherein the overcurrent protection element has the initial resistance value at room temperature when not triggered, and the overcurrent protection element has the post-trigger resistance value after the first cycle life test and cooling to room temperature. The over-current protection device as claimed in claim 14 , wherein the resistance jump rate is 2.4 to 2.
5.
16. The overcurrent protection device according to claim 15, wherein the overcurrent protection device can pass a second cycle life test without burning out, wherein: The second cycle life test includes performing an applied power for a specific number of cycles, the applied power is 24V / 40A and the specific number of cycles is 500 times.
17. The overcurrent protection device according to claim 16, wherein the overcurrent protection device can pass a third cycle life test without burning out, wherein: The third cycle life test includes performing an applied power for a specific number of cycles, the applied power is 30V / 30A and the specific number of cycles is 100 times.
18. The overcurrent protection element according to claim 14, wherein the overcurrent protection element has a first thermal drop ratio of 0.51 to 0.66, wherein the first thermal drop ratio is defined as the trigger current required by the overcurrent protection element in an environment of 23°C divided by the trigger current required by the overcurrent protection element in an environment of -40°C.
19. The overcurrent protection element according to claim 18, wherein the overcurrent protection element has a second thermal drop ratio of 0.63 to 0.73, wherein the second thermal drop ratio is defined as the trigger current required by the overcurrent protection element in an environment of 125°C divided by the trigger current required by the overcurrent protection element in an environment of 85°C.