Sodium battery positive electrode material with gradient distribution of nickel, precursor, preparation and application
By using nickel gradient distribution and lanthanum and iodine shell coating technology in sodium battery positive electrode materials, the stability and performance problems of the material during recycling are solved, and higher rate performance and longer battery life are achieved, while reducing the number of times. The cost.
Patent Information
- Application Number
- CN202411125899.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
The existing sodium battery positive electrode materials are prone to rupture and side reactions during recycling, resulting in unstable performance, and the mixed discharge of Ni and Na metals is serious, affecting the rate performance and life of the battery.
The precursor of the positive electrode material of the sodium battery with a nickel gradient distribution is used to coat the lanthanum shell and the iodine shell on the outside of the nickel-ferromanganese ternary material core to control the reduction of nickel content gradient, enhance material stability and cyclic performance, and pass through the atomic layer. Deposition technology controls shell thickness and reduces costs.
It effectively reduces the mixing of Ni and Na metals, improves the rate performance and stability of the positive electrode material, extends the cycle life of the battery, and reduces the preparation cost.
Smart Images

Figure BDA0004996403440000221 
Figure BDA0004996403440000231
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of batteries, and relates to a precursor of a positive electrode material of a sodium battery with a nickel gradient distribution, and in particular to a positive electrode material of a sodium battery with a nickel gradient distribution, a precursor, and preparation and application thereof. Background Art
[0002] In today's era, the research and development of lithium-ion batteries and their core materials has become a key focus of global science and technology and industrial development. However, due to the limited reserves and uneven distribution of global lithium resources, the widespread application of lithium-ion batteries in the field of energy storage is severely restricted. In particular, the price fluctuations of lithium resources have a direct impact on the battery industry.
[0003] The research and development and industrialization of sodium-ion batteries are expected to alleviate the development constraints of energy storage batteries caused by the shortage of lithium resources to a certain extent. In the composition of batteries, positive electrode materials play a vital role. However, during the battery cycle, positive electrode materials are very prone to rupture, and continuous side reactions will occur between them and the electrolyte. These factors seriously affect the cycle life and rate performance of the battery. Surface coating of positive electrode materials can effectively reduce stress, improve the wettability of liquid electrolytes, and reduce the resistance of interfacial charge transfer, thereby reducing side reactions and optimizing the performance of positive electrode materials.
[0004] CN114639822A discloses a nickel-cobalt-manganese ternary MOF cathode material precursor with element gradient distribution and its preparation method. The invention realizes the preparation of MOF material by adding a complexing agent, and successfully prepares an in-situ conductive carbon array in the subsequent treatment to improve the internal electronic conductivity. In addition, the gradient distribution of metal elements in the ternary MOF cathode material is successfully achieved by using a method of mixing solutions at different temperatures at a constant speed. On the one hand, a built-in electric field is constructed inside the material to improve the electronic conductivity. On the other hand, the generation of structural defects is conducive to improving the transmission path of Na ions, further improving the ionic conductivity and reducing polarization.
[0005] CN117430171A discloses a nickel-cobalt-manganese positive electrode precursor material doped with both anions and cations, and its preparation method and application. The nickel-cobalt-manganese positive electrode precursor material includes a precursor matrix material and a doping element doped in the precursor matrix material; the doping element includes phosphorus and lanthanum, and the phosphorus doping is phosphate doping. The nickel-cobalt-manganese positive electrode precursor material provided by the invention realizes homogeneous doping of anions and cations through the synergistic doping of phosphate ions and lanthanum, effectively stabilizes the lanthanum and phosphorus elements in nickel-cobalt-manganese, and improves the structural stability of the positive electrode material, thereby improving the electrochemical performance of the positive electrode material.
[0006] The precursors of the sodium battery positive electrode materials disclosed in the prior art have certain defects. The sodium battery positive electrode materials prepared by them have high metal content, which easily leads to the mixing of Ni and Na metal in the positive electrode materials, and the positive electrode materials are unstable and prone to rupture during battery recycling, and continuous side reactions occur between the electrolyte. Therefore, it is very important to develop and design a new type of sodium battery positive electrode material, precursor, preparation and application with nickel gradient distribution. Summary of the invention
[0007] In view of the deficiencies in the prior art, the object of the present invention is to provide a sodium battery positive electrode material with a nickel gradient distribution, a precursor, and preparation and application. In the precursor of the sodium battery positive electrode material with a nickel gradient distribution provided by the present invention, along the radial direction of the nickel-iron-manganese ternary material core, the nickel content in the nickel-iron-manganese ternary material core gradually decreases from the inside to the outside, while ensuring the volume energy density of the positive electrode material prepared from the precursor, reducing the mixing of Ni and Na metals in the positive electrode material, and reducing the cost; in addition, the outer coating of the nickel-iron-manganese ternary material core has a lanthanum shell layer that improves the material rate, increases the system stability, and increases the cycle performance, and the iodine shell layer that increases the material stability is also coated on the outside of the lanthanum shell layer, thereby further improving the rate performance and stability of the positive electrode material prepared from the precursor.
[0008] To achieve this object, the present invention adopts the following technical solutions:
[0009] In a first aspect, the present invention provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, the precursor comprising a nickel-iron-manganese ternary material core, and a lanthanum shell layer and an iodine shell layer sequentially coated on the outside of the nickel-iron-manganese ternary material core; along the radial direction of the nickel-iron-manganese ternary material core, the nickel content in the nickel-iron-manganese ternary material core gradually decreases from the inside to the outside.
[0010] After the nickel-iron-manganese ternary material core described in the present invention is coated, the coating layer can prevent the positive electrode material from contacting the electrolyte, and the metal ions coated on the surface can reduce the mixing of cations to improve the stability of the material, and can also increase the spacing of the Na layer and increase the transmission rate of sodium ions, thereby improving the rate performance of the positive electrode material prepared by the precursor.
[0011] The precursor of the present invention includes a lanthanum shell layer, and the positive electrode material prepared by the precursor will form a La-O bond. Since the bond strength of the La-O bond is relatively large, La plays a supporting role, adjusts the TM-O (transition metal-oxygen) and Na-O bond lengths, and stabilizes the structure; in addition, the La-O bond can bring more valence electrons to nearby oxygen, thereby increasing the bond energy of the Mn-O ion, which not only ensures the stability of the lattice oxygen skeleton and the reversibility of redox, but also optimizes the oxygen local electronic structure generated by the mixing of the 5d orbital of La and the 2p orbital of O due to the charge transfer from the 2p orbital of O to the 5d orbital of La, so that O exhibits better resistance to over-oxidation under high pressure. Therefore, the presence of the lanthanum shell layer improves the rate performance of the positive electrode material prepared by the precursor, increases the system stability, and enhances the cycle performance.
[0012] The precursor of the present invention includes an iodine shell layer, and the advantage of the iodine shell layer is mainly to strengthen the stability of each bond of Ni-O, Mn-O and Fe-O, thereby improving the stability of the positive electrode material prepared by the precursor.
[0013] In the precursor of the sodium battery positive electrode material with nickel gradient distribution provided by the present invention, along the radial direction of the nickel-iron-manganese ternary material core, the nickel content in the nickel-iron-manganese ternary material core gradually decreases from the inside to the outside, while ensuring the volume energy density of the positive electrode material prepared by the precursor, reducing the mixing of Ni and Na metals in the positive electrode material, and reducing the cost; in addition, the nickel-iron-manganese ternary material core is coated with a lanthanum shell layer that improves the material rate, increases the system stability, and increases the cycle performance, and an iodine shell layer that increases the material stability is also coated on the outside of the lanthanum shell layer, thereby further improving the rate performance and stability of the positive electrode material prepared by the precursor.
[0014] Preferably, the chemical formula of the nickel-iron-manganese ternary material core includes but is not limited to Ni x Fe y Mn 1-x-y (OH)2, wherein 0.1≤x<0.45, 0.1≤y<0.45, 0.1≤1-xy<0.40, the value of x can be, for example, 0.1, 0.2, 0.3, 0.4 or 0.45, but is not limited to the listed values, and other values not listed within the numerical range are equally applicable; the value of y can be, for example, 0.1, 0.2, 0.3, or 0.4, but is not limited to the listed values, and other values not listed within the numerical range are equally applicable.
[0015] Preferably, the average particle size of the nickel-iron-manganese ternary material core is 4 to 8 μm, for example, it can be 4 μm, 4.5 μm, 5 μm, 5.5 μm, 6 μm, 6.5 μm, 7 μm, 7.5 μm or 8 μm, but is not limited to the listed values, and other unlisted values within this numerical range are also applicable.
[0016] Preferably, the molar ratio of the sum of metal ions in the nickel-iron-manganese ternary material core to the sum of lanthanum in the lanthanum shell and iodine in the iodine shell is (95-99.7):(0.3-5), for example, it can be 95:5, 95.5:4.5, 96:4, 96.5:3.5, 97:3, 97.5:2.5, 98:2, 98.5:1.5, 99:1, 99.5:0.5 or 99.7:0.3, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0017] Preferably, the molar ratio of lanthanum in the lanthanum shell layer to iodine in the iodine shell layer is 1:(0.5-2), for example, it can be 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9, 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4, 1:1.5, 1:1.6, 1:1.7, 1:1.8, 1:1.9 or 1:2, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0018] In a second aspect, the present invention provides a method for preparing the precursor according to the first aspect, the preparation method comprising:
[0019] (1) adding a nickel-iron-manganese mixed salt solution, a precipitant solution and a complexing agent solution to a reaction base solution in stages to carry out a coprecipitation reaction to obtain a nickel-iron-manganese ternary material core;
[0020] Wherein, the staged method comprises at least two stages, and the nickel concentration in the nickel-iron-manganese mixed salt solution added in each previous stage is higher than the nickel concentration in the nickel-iron-manganese mixed salt solution added in the adjacent next stage;
[0021] (2) Depositing a lanthanum shell layer and an iodine shell layer in sequence on the surface of the obtained nickel-iron-manganese ternary material core to obtain the precursor.
[0022] The nickel-iron-manganese mixed salt solution of the present invention is obtained by mixing nickel salt, iron salt, manganese salt and solvent; the nickel salt, iron salt and manganese salt independently include but are not limited to any one of sulfate, chloride or nitrate or a combination of at least two, and typical but non-limiting combinations include a combination of sulfate and chloride, and a combination of chloride and nitrate; the solvent includes water.
[0023] The preparation method of the present invention utilizes a simple hydroxide co-precipitation reaction, and by regulating the nickel concentration in the nickel-iron-manganese mixed salt solution added at different stages during the co-precipitation process, a nickel-iron-manganese ternary material core is prepared, in which the nickel content in the nickel-iron-manganese ternary material core decreases gradually along the radial direction. After coating the outside of the nickel-iron-manganese ternary material core with a lanthanum shell layer and an iodine shell layer, the precursor is obtained.
[0024] Preferably, the staged process of step (1) comprises three stages, and the nickel concentration in the nickel-iron-manganese mixed salt solution added in the first stage, the second stage and the third stage decreases successively.
[0025] Preferably, in the first stage, the first nickel-iron-manganese mixed salt solution, the precipitant solution and the complexing agent solution are added to the reaction base solution in parallel to carry out a first coprecipitation reaction to obtain a primary mixed solution containing a precipitate.
[0026] Preferably, the total concentration of metal ions in the first nickel-iron-manganese mixed salt solution in the first stage is 1-20 mol / L, and the concentration ratio of nickel ions, iron ions and manganese ions is (35-45):(22-32):(28-38).
[0027] The total concentration of metal ions in the first nickel-iron-manganese mixed salt solution in the first stage of the present invention is 1 to 20 mol / L, for example, it can be 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, 13 mol / L, 14 mol / L, 15 mol / L, 16 mol / L, 17 mol / L, 18 mol / L, 19 mol / L, or 20 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0028] In the present invention, the ratio of the concentration of nickel ions to iron ions in the first nickel-iron-manganese mixed salt solution in the first stage is (35-45):(22-32), for example, it can be 35:22, 35:23, 35:27, 35:29, 35:31, 35:32, 37:22, 37:23, 37:27, 37:29, 37:31, 37:32, 41:22, 41:23, 41:27, 41:29, 41:31, 41:32, 45:22, 45:23, 45:27, 45:29, 45:31 or 45:32, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0029] In the present invention, the concentration ratio of nickel ions to manganese ions in the first nickel-iron-manganese mixed salt solution in the first stage is (35-45):(28-38), for example, it can be 35:28, 35:31, 35:33, 35:37, 35:38, 37:28, 37:31, 37:33, 37:37, 37:38, 41:28, 41:31, 41:33, 41:37, 41:38, 45:28, 45:31, 45:33, 45:37 or 45:38, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0030] Preferably, the addition rate of the first nickel-iron-manganese mixed salt solution in the first stage is 1 to 100 L / h, for example, it can be 1 L / h, 3 L / h, 5 L / h, 10 L / h, 15 L / h, 20 L / h, 30 L / h, 50 L / h, 70 L / h or 100 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0031] Preferably, the pH of the first coprecipitation reaction is 10.5-11.5, and the ammonia concentration is 5-200 g / L.
[0032] The pH of the first coprecipitation reaction in the present invention is 10.5-11.5, for example, it can be 10.5, 10.6, 10.7, 10.8, 10.9, 11.0, 11.1, 11.2, 11.3, 11.4 or 11.5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0033] The ammonia concentration of the first coprecipitation reaction of the present invention is 5 to 200 g / L, for example, it can be 5 g / L, 10 g / L, 20 g / L, 40 g / L, 60 g / L, 80 g / L, 100 g / L, 120 g / L, 140 g / L, 160 g / L, 180 g / L or 200 g / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0034] Preferably, the duration of the first stage is 2 to 48 hours, for example, it can be 2h, 4h, 6h, 10h, 15h, 20h, 25h, 30h, 35h, 40h, 45h or 48h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0035] Preferably, in the first stage, the addition rate of the precipitant solution is 1 to 200 L / h, and the addition rate of the complexing agent solution is 0.5 to 50 L / h.
[0036] The addition rate of the precipitant solution in the first stage of the present invention is 1 to 200 L / h, for example, 1 L / h, 3 L / h, 5 L / h, 10 L / h, 15 L / h, 20 L / h, 30 L / h, 40 L / h, 60 L / h, 80 L / h, 100 L / h, 120 L / h, 160 L / h or 200 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0037] The addition rate of the complexing agent solution in the first stage of the present invention is 0.5 to 50 L / h, for example, it can be 0.5 L / h, 1 L / h, 3 L / h, 5 L / h, 10 L / h, 15 L / h, 20 L / h, 30 L / h, 40 L / h or 50 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0038] Preferably, in the first stage, the concentration of the precipitant solution is 5-15 mol / L, and the concentration of the complexing agent solution is 5-10 mol / L.
[0039] The concentration of the precipitant solution in the first stage of the present invention is 5 to 15 mol / L, for example, it can be 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, 13 mol / L, 14 mol / L or 15 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0040] The concentration of the complexing agent solution in the first stage of the present invention is 5 to 10 mol / L, for example, it can be 5 mol / L, 5.5 mol / L, 6 mol / L, 6.5 mol / L, 7 mol / L, 7.5 mol / L, 8 mol / L, 8.5 mol / L, 9 mol / L, 9.5 mol / L or 10 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0041] Preferably, in the second stage, the second nickel-iron-manganese mixed salt solution, the precipitant solution and the complexing agent solution are added in parallel to the primary mixed solution containing the precipitate to perform a second coprecipitation reaction to obtain a remixed solution containing the precipitate.
[0042] Preferably, the total concentration of metal ions in the second nickel-iron-manganese mixed salt solution in the second stage is 1-20 mol / L, and the concentration ratio of nickel ions, iron ions and manganese ions is (25-35):(32-42):(28-38).
[0043] The total concentration of metal ions in the second nickel-iron-manganese mixed salt solution in the second stage of the present invention is 1 to 20 mol / L, for example, it can be 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, 13 mol / L, 14 mol / L, 15 mol / L, 16 mol / L, 17 mol / L, 18 mol / L, 19 mol / L, or 20 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0044] The ratio of the concentration of nickel ions to iron ions in the second nickel-iron-manganese mixed salt solution in the second stage of the present invention is (25-35): (32-42), for example, it can be 25:32, 25:37, 25:39, 25:41, 25:42, 27:32, 27:37, 27:39, 27:41, 27:42, 29:32, 29:37, 29:39, 29:41, 29:42, 32:32, 32:37, 32:39, 32:41 or 32:42, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0045] The ratio of the concentration of nickel ions to manganese ions in the second nickel-iron-manganese mixed salt solution in the second stage of the present invention is (25-35): (28-38), for example, it can be 32:28, 32:31, 32:33, 32:37, 32:38, 27:28, 27:31, 27:33, 27:37, 27:38, 31:28, 31:31, 31:33, 31:37, 31:38, 33:28, 33:31, 33:37, 33:38, 38:28, 38:31, 38:33 or 38:37, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0046] Preferably, the addition rate of the second nickel-iron-manganese mixed salt solution in the second stage is 1 to 100 L / h, for example, it can be 1 L / h, 2 L / h, 5 L / h, 10 L / h, 20 L / h, 30 L / h, 40 L / h, 50 L / h, 60 L / h, 70 L / h, 80 L / h, 90 L / h or 100 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0047] Preferably, the pH of the second coprecipitation reaction is 10.5-11.5, and the ammonia concentration is 5-200 g / L.
[0048] The pH of the second coprecipitation reaction in the present invention is 10.5-11.5, for example, it can be 10.5, 10.6, 10.7, 10.8, 10.9, 11.0, 11.1, 11.2, 11.3, 11.4 or 11.5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0049] The ammonia concentration of the second coprecipitation reaction of the present invention is 5 to 200 g / L, for example, it can be 5 g / L, 10 g / L, 20 g / L, 40 g / L, 60 g / L, 80 g / L, 100 g / L, 120 g / L, 140 g / L, 160 g / L, 180 g / L or 200 g / L, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0050] Preferably, the duration of the second stage is 2 to 48 hours, for example, it can be 2 hours, 6 hours, 10 hours, 15 hours, 20 hours, 25 hours, 30 hours, 35 hours, 40 hours, 45 hours or 48 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0051] Preferably, in the second stage, the precipitant solution is added at a rate of 1 to 200 L / h, and the complexing agent solution is added at a rate of 0.5 to 50 L / h.
[0052] In the present invention, the addition rate of the precipitant solution in the second stage is 1 to 200 L / h, for example, it can be 1 L / h, 3 L / h, 5 L / h, 10 L / h, 15 L / h, 20 L / h, 30 L / h, 40 L / h, 60 L / h, 80 L / h, 100 L / h, 120 L / h, 160 L / h or 200 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0053] The addition rate of the complexing agent solution in the second stage of the present invention is 0.5 to 50 L / h, for example, it can be 0.5 L / h, 1 L / h, 3 L / h, 5 L / h, 10 L / h, 15 L / h, 20 L / h, 30 L / h, 40 L / h or 50 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0054] Preferably, in the second stage, the concentration of the precipitant solution is 5-15 mol / L, and the concentration of the complexing agent solution is 5-10 mol / L.
[0055] The concentration of the precipitant solution in the second stage of the present invention is 5 to 15 mol / L, for example, it can be 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, 13 mol / L, 14 mol / L or 15 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0056] The concentration of the complexing agent solution in the second stage of the present invention is 5 to 10 mol / L, for example, it can be 5 mol / L, 5.5 mol / L, 6 mol / L, 6.5 mol / L, 7 mol / L, 7.5 mol / L, 8 mol / L, 8.5 mol / L, 9 mol / L, 9.5 mol / L or 10 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0057] Preferably, in the third stage, the third nickel-iron-manganese mixed salt solution, the precipitant solution and the complexing agent solution are added in parallel to the remixed liquid containing the precipitate to carry out a third co-precipitation reaction to obtain a final mixed liquid containing the nickel-iron-manganese ternary material core.
[0058] Preferably, the total concentration of metal ions in the third nickel-iron-manganese mixed salt solution in the third stage is 1-20 mol / L, and the concentration ratio of nickel ions, iron ions and manganese ions is (15-25):(42-52):(28-38).
[0059] The total concentration of metal ions in the third nickel-iron-manganese mixed salt solution in the third stage of the present invention is 1 to 20 mol / L, for example, 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, 13 mol / L, 14 mol / L, 15 mol / L, 16 mol / L, 17 mol / L, 18 mol / L, 19 mol / L, or 20 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0060] The concentration ratio of nickel ions to iron ions in the third nickel-iron-manganese mixed salt solution in the third stage of the present invention is (15-25):(42-52), for example, it can be 15:42, 15:46, 15:49, 15:52, 17:42, 17:46, 17:49, 17:52, 23:42, 23:46, 23:49, 23:52, 25:42, 25:46, 25:49 or 25:52, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0061] The concentration ratio of nickel ions to manganese ions in the third nickel-iron-manganese mixed salt solution in the third stage of the present invention is (15-25): (28-38), for example, it can be 15:28, 15:31, 15:34, 15:37, 15:38, 17:28, 17:31, 17:34, 17:37, 17:38, 23:28, 23:31, 23:34, 23:37, 23:38, 25:28, 25:31, 25:34, 25:37 or 25:38, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0062] Preferably, the addition rate of the third nickel-iron-manganese mixed salt solution in the third stage is 1 to 100 L / h, for example, it can be 1 L / h, 3 L / h, 5 L / h, 10 L / h, 15 L / h, 20 L / h, 30 L / h, 50 L / h, 70 L / h or 100 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0063] Preferably, the pH of the third coprecipitation reaction is 10.5-11.5, and the ammonia concentration is 5-200 g / L.
[0064] The pH of the third coprecipitation reaction in the present invention is 10.5-11.5, for example, it can be 10.5, 10.6, 10.7, 10.8, 10.9, 11.0, 11.1, 11.2, 11.3, 11.4 or 11.5, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0065] The ammonia concentration of the third coprecipitation reaction of the present invention is 5 to 200 g / L, for example, it can be 5 g / L, 10 g / L, 20 g / L, 40 g / L, 60 g / L, 80 g / L, 100 g / L, 120 g / L, 140 g / L, 160 g / L, 180 g / L or 200 g / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0066] Preferably, in the third stage, the precipitant solution is added at a rate of 1 to 200 L / h, and the complexing agent solution is added at a rate of 0.5 to 50 L / h.
[0067] The addition rate of the precipitant solution in the third stage of the present invention is 1 to 200 L / h, for example, 1 L / h, 3 L / h, 5 L / h, 10 L / h, 15 L / h, 20 L / h, 30 L / h, 40 L / h, 60 L / h, 80 L / h, 100 L / h, 120 L / h, 160 L / h or 200 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are equally applicable.
[0068] The addition rate of the complexing agent solution in the third stage of the present invention is 0.5 to 50 L / h, for example, it can be 0.5 L / h, 1 L / h, 3 L / h, 5 L / h, 10 L / h, 15 L / h, 20 L / h, 30 L / h, 40 L / h or 50 L / h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0069] Preferably, in the third stage, the concentration of the precipitant solution is 5 to 15 mol / L, and the concentration of the complexing agent solution is 5 to 10 mol / L.
[0070] The concentration of the precipitant solution in the third stage of the present invention is 5 to 15 mol / L, for example, it can be 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, 13 mol / L, 14 mol / L or 15 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0071] The concentration of the complexing agent solution in the third stage of the present invention is 5-10 mol / L, for example, it can be 5 mol / L, 6 mol / L, 7 mol / L, 8 mol / L, 9 mol / L, 10 mol / L, 11 mol / L, 12 mol / L, 13 mol / L, 14 mol / L or 15 mol / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0072] Preferably, the reaction base liquid in step (1) is composed of a solvent, a precipitant and a complexing agent, the pH of the reaction base liquid is 8.5 to 11.7, and the ammonia concentration is 3 to 70 g / L.
[0073] The pH of the reaction base solution of the present invention is 8.5-11.7, for example, it can be 8.5, 8.7, 9, 9.5, 10, 10.5, 11, 11.5 or 11.7, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0074] The ammonia concentration of the reaction base solution of the present invention is 3 to 70 g / L, for example, it can be 3 g / L, 6 g / L, 10 g / L, 20 g / L, 30 g / L, 40 g / L, 50 g / L, 60 g / L or 70 g / L, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0075] Preferably, step (1) is carried out in a protective atmosphere, and the temperature of the coprecipitation reaction is controlled to be 30-70°C, for example, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C or 70°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0076] Preferably, the lanthanum shell layer and the iodine shell layer in step (2) are both deposited by atomic layer deposition.
[0077] The present invention adopts atomic layer deposition to achieve effective control of the thickness and quality of the lanthanum shell layer and the iodine shell layer.
[0078] Preferably, the raw material for depositing the lanthanum shell layer in step (2) includes any one of lanthanum sulfate, lanthanum chloride or lanthanum nitrate, or a combination of at least two of them. Typical but non-limiting combinations include a combination of lanthanum sulfate and lanthanum chloride, a combination of lanthanum chloride and lanthanum nitrate, or a combination of lanthanum sulfate, lanthanum chloride and lanthanum nitrate.
[0079] Preferably, the raw material for the iodine shell deposition in step (2) includes any one of iodine water, sodium iodide, manganese iodide, barium iodide, copper iodide or magnesium iodide, or a combination of at least two of them. Typical but non-limiting combinations include a combination of iodine water and sodium iodide, a combination of manganese iodide and barium iodide, a combination of copper iodide and magnesium iodide, or a combination of iodine water, sodium iodide and manganese iodide.
[0080] In the present invention, the raw materials for the deposition of the lanthanum shell layer and the raw materials for the deposition of the iodine shell layer are both low-cost materials, replacing the expensive LaI2, thereby further reducing the cost of the preparation method.
[0081] Preferably, the preparation method further comprises aging, solid-liquid separation, washing and drying carried out in sequence after the coprecipitation reaction in step (1) to obtain the nickel-iron-manganese ternary material core.
[0082] In a third aspect, the present invention provides a sodium battery positive electrode material with a nickel gradient distribution, wherein the sodium battery positive electrode material is prepared from the precursor described in the first aspect.
[0083] In a fourth aspect, the present invention provides a process for preparing the positive electrode material for a sodium battery according to the third aspect, the preparation process comprising:
[0084] The precursor is mixed with a sodium source and sintered in an oxygen atmosphere to obtain the sodium battery positive electrode material.
[0085] Preferably, the molar ratio of the precursor to the sodium source is (1-1.2):1, for example, it can be 1:1, 1.02:1, 1.04:1, 1.06:1, 1.08:1, 1.1:1, 1.12:1, 1.14:1, 1.16:1, 1.18:1 or 1.2:1, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0086] Preferably, the sintering temperature is 400-1000° C. and the sintering time is 4-30 hours.
[0087] The sintering temperature in the present invention is 400-1000°C, for example, it can be 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, 950°C or 1000°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0088] The sintering time in the present invention is 4 to 30 hours, for example, it can be 4h, 6h, 8h, 10h, 12h, 14h, 16h, 18h, 20h, 22h, 24h, 26h, 28h or 30h, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0089] Preferably, the preparation process further comprises grinding and screening performed in sequence after the sintering.
[0090] In a fifth aspect, the present invention provides a sodium ion battery, wherein the sodium ion battery comprises the sodium battery positive electrode material described in the third aspect.
[0091] Compared with the prior art, the present invention has the following beneficial effects:
[0092] In the precursor of the sodium battery positive electrode material with nickel gradient distribution provided by the present invention, along the radial direction of the nickel-iron-manganese ternary material core, the nickel content in the nickel-iron-manganese ternary material core gradually decreases from the inside to the outside, while ensuring the volume energy density of the positive electrode material prepared by the precursor, reducing the mixing of Ni and Na metals in the positive electrode material, and reducing the cost; in addition, the nickel-iron-manganese ternary material core is coated with a lanthanum shell layer that improves the material rate, increases the system stability, and increases the cycle performance, and an iodine shell layer that increases the material stability is also coated on the outside of the lanthanum shell layer, thereby further improving the rate performance and stability of the positive electrode material prepared by the precursor. DETAILED DESCRIPTION
[0093] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0094] Example 1
[0095] This embodiment provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, the precursor comprising a nickel-iron-manganese ternary material core with an average particle size of 5 μm, and a lanthanum shell layer and an iodine shell layer sequentially coated on the outside of the nickel-iron-manganese ternary material core; along the radial direction of the nickel-iron-manganese ternary material core, the nickel content in the nickel-iron-manganese ternary material core gradually decreases from the inside to the outside;
[0096] The molar ratio of the sum of metal ions in the nickel-iron-manganese ternary material core to the sum of lanthanum in the lanthanum shell and iodine in the iodine shell is 99:1; the molar ratio of lanthanum in the lanthanum shell and iodine in the iodine shell is 1:0.5;
[0097] The preparation method of the precursor comprises:
[0098] (1) The first stage: In a protective atmosphere, a first nickel-iron-manganese mixed salt solution (the ratio of nickel ion, iron ion and manganese ion concentration is 35:30:35) with a total metal ion concentration of 10 mol / L is added to the reaction bottom liquid at a rate of 40 L / h in parallel with a sodium hydroxide solution with a concentration of 10 mol / L and an ammonia solution with a concentration of 5 mol / L, the reaction pH is controlled to be 11 and the ammonia concentration is 20 g / L, and a first coprecipitation reaction is carried out at 58° C. for 25 h to obtain a primary mixed solution containing a precipitate;
[0099] The first coprecipitation reaction base liquid is composed of a solvent, a precipitant and a complexing agent, the pH of the reaction base liquid is 10, and the ammonia concentration is 10g / L;
[0100] (2) Second stage: In a protective atmosphere, a second nickel-iron-manganese mixed salt solution (the ratio of nickel ion, iron ion and manganese ion concentration is 25:38:37) with a total metal ion concentration of 10 mol / L is added at a rate of 40 L / h to the primary mixed solution containing the precipitate obtained in step (1) in parallel with a sodium hydroxide solution with a concentration of 10 mol / L and an ammonia solution with a concentration of 5 mol / L, the pH is controlled to be 11 and the ammonia concentration is 20 g / L, and a second coprecipitation reaction is carried out at 58° C. for 25 h to obtain a remixed solution containing the precipitate;
[0101] (3) The third stage: in a protective atmosphere, a third nickel-iron-manganese mixed salt solution having a total metal ion concentration of 10 mol / L (the ratio of nickel ion, iron ion and manganese ion concentration is 15:50:35) is added at a rate of 40 L / h to the remixed solution obtained in step (2) containing the precipitate, and the reaction pH is controlled to be 11 and the ammonia concentration is 20 g / L. A third coprecipitation reaction is carried out at 58° C. to obtain a final mixed solution containing the nickel-iron-manganese ternary material core, and aging, solid-liquid separation, washing and drying are carried out in sequence to obtain the nickel-iron-manganese ternary material core;
[0102] (4) using atomic layer deposition technology, the surface of the nickel-iron-manganese ternary material core obtained in step (3) is first coated with a lanthanum shell using lanthanum sulfate as a lanthanum source, and then coated with an iodine shell using sodium bromide as a bromine source, and then aging to remove sulfate and impurity elements, centrifugally washing and drying at 150° C. to obtain the precursor.
[0103] Example 2
[0104] This embodiment provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, the precursor comprising a nickel-iron-manganese ternary material core with an average particle size of 8 μm, and a lanthanum shell layer and an iodine shell layer sequentially coated on the outside of the nickel-iron-manganese ternary material core; along the radial direction of the nickel-iron-manganese ternary material core, the nickel content in the nickel-iron-manganese ternary material core gradually decreases from the inside to the outside;
[0105] The molar ratio of the sum of metal ions in the nickel-iron-manganese ternary material core to the sum of lanthanum in the lanthanum shell and iodine in the iodine shell is 98:2; the molar ratio of lanthanum in the lanthanum shell and iodine in the iodine shell is 1:0.8;
[0106] The preparation method of the precursor comprises:
[0107] (1) The first stage: In a protective atmosphere, a first nickel-iron-manganese mixed salt solution (the ratio of nickel ion, iron ion and manganese ion concentration is 30:32:38) with a total metal ion concentration of 5 mol / L is added to the reaction bottom liquid at a rate of 80 L / h in parallel with a sodium hydroxide solution with a concentration of 4 mol / L and an ammonia solution with a concentration of 10 mol / L, the reaction pH is controlled to be 11.2 and the ammonia concentration is 15 g / L, and a first coprecipitation reaction is carried out at 55° C. for 20 h to obtain a primary mixed solution containing a precipitate;
[0108] The first coprecipitation reaction base liquid is composed of a solvent, a precipitant and a complexing agent, the pH of the reaction base liquid is 10.5, and the ammonia concentration is 5 g / L;
[0109] (2) Second stage: In a protective atmosphere, a second nickel-iron-manganese mixed salt solution (the ratio of nickel ion, iron ion and manganese ion concentration is 25:40:35) with a total metal ion concentration of 5 mol / L is added at a rate of 80 L / h to the primary mixed solution containing the precipitate obtained in step (1) in parallel with a 4 mol / L sodium hydroxide solution and a 10 mol / L ammonia solution, the pH is controlled to be 11.2 and the ammonia concentration is 15 g / L, and a second coprecipitation reaction is carried out at 55° C. for 20 h to obtain a remixed solution containing the precipitate;
[0110] (3) The third stage: in a protective atmosphere, a third nickel-iron-manganese mixed salt solution having a total metal ion concentration of 5 mol / L (the ratio of nickel ion, iron ion and manganese ion concentration is 15:50:35) is added at a rate of 80 L / h to the remixed solution obtained in step (2) containing the precipitate, in parallel with a sodium hydroxide solution having a concentration of 4 mol / L and an ammonia solution having a concentration of 10 mol / L, the reaction pH is controlled to be 11.2 and the ammonia concentration is 15 g / L, a third coprecipitation reaction is carried out at 55° C. to obtain a final mixed solution containing the nickel-iron-manganese ternary material core, and aging, solid-liquid separation, washing and drying are carried out in sequence to obtain the nickel-iron-manganese ternary material core;
[0111] (4) using atomic layer deposition technology, the surface of the nickel-iron-manganese ternary material core obtained in step (3) is first coated with a lanthanum shell using lanthanum sulfate as a lanthanum source, and then coated with an iodine shell using sodium bromide as a bromine source, and then aging to remove sulfate and impurity elements, centrifugally washing and drying at 120° C. to obtain the precursor.
[0112] Example 3
[0113] This embodiment provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, the precursor comprising a nickel-iron-manganese ternary material core with an average particle size of 4 μm, and a lanthanum shell layer and an iodine shell layer sequentially coated on the outside of the nickel-iron-manganese ternary material core; along the radial direction of the nickel-iron-manganese ternary material core, the nickel content in the nickel-iron-manganese ternary material core gradually decreases from the inside to the outside;
[0114] The molar ratio of the sum of metal ions in the nickel-iron-manganese ternary material core to the sum of lanthanum in the lanthanum shell and iodine in the iodine shell is 97:3; the molar ratio of lanthanum in the lanthanum shell and iodine in the iodine shell is 1:1;
[0115] The preparation method of the precursor comprises:
[0116] (1) The first stage: In a protective atmosphere, a first nickel-iron-manganese mixed salt solution (the ratio of nickel ion, iron ion and manganese ion concentration is 40:30:30) with a total metal ion concentration of 20 mol / L is added to the reaction bottom liquid at a rate of 20 L / h in parallel with a sodium hydroxide solution with a concentration of 16 mol / L and an ammonia solution with a concentration of 8 mol / L, the reaction pH is controlled to be 11.5 and the ammonia concentration is 5 g / L, and a first coprecipitation reaction is carried out at 55° C. for 30 h to obtain a primary mixed solution containing a precipitate;
[0117] The first coprecipitation reaction base liquid is composed of a solvent, a precipitant and a complexing agent, the pH of the reaction base liquid is 10.2, and the ammonia concentration is 8 g / L;
[0118] (2) Second stage: In a protective atmosphere, a second nickel-iron-manganese mixed salt solution (the ratio of nickel ion, iron ion and manganese ion concentration is 26:38:36) with a total metal ion concentration of 20 mol / L is added at a rate of 20 L / h to the primary mixed solution containing the precipitate obtained in step (1) in parallel with a sodium hydroxide solution with a concentration of 16 mol / L and an ammonia solution with a concentration of 8 mol / L, the pH is controlled to be 11.5 and the ammonia concentration is 5 g / L, and a second coprecipitation reaction is carried out at 55° C. for 30 h to obtain a remixed solution containing the precipitate;
[0119] (3) The third stage: in a protective atmosphere, a third nickel-iron-manganese mixed salt solution having a total metal ion concentration of 20 mol / L (the ratio of nickel ion, iron ion and manganese ion concentration is 15:50:35) is added at a rate of 20 L / h to the remixed solution containing the precipitate obtained in step (2) in parallel with a sodium hydroxide solution having a concentration of 16 mol / L and an ammonia solution having a concentration of 8 mol / L, the reaction pH is controlled to be 11.5 and the ammonia concentration is 5 g / L, a third coprecipitation reaction is carried out at 55° C. to obtain a final mixed solution containing the nickel-iron-manganese ternary material core, and aging, solid-liquid separation, washing and drying are carried out in sequence to obtain the nickel-iron-manganese ternary material core;
[0120] (4) using atomic layer deposition technology, the surface of the nickel-iron-manganese ternary material core obtained in step (3) is first coated with a lanthanum shell using lanthanum sulfate as a lanthanum source, and then coated with an iodine shell using sodium bromide as a bromine source, and then aging to remove sulfate and impurity elements, centrifugally washing and drying at 120° C. to obtain the precursor.
[0121] Example 4
[0122] This embodiment provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, the precursor comprising a nickel-iron-manganese ternary material core with an average particle size of 6.5 μm, and a lanthanum shell layer and an iodine shell layer sequentially coated on the outside of the nickel-iron-manganese ternary material core; along the radial direction of the nickel-iron-manganese ternary material core, the nickel content in the nickel-iron-manganese ternary material core gradually decreases from the inside to the outside;
[0123] The molar ratio of the sum of metal ions in the nickel-iron-manganese ternary material core to the sum of lanthanum in the lanthanum shell and iodine in the iodine shell is 98.5:1.5; the molar ratio of lanthanum in the lanthanum shell and iodine in the iodine shell is 1:2;
[0124] The preparation method of the precursor comprises:
[0125] (1) The first stage: In a protective atmosphere, a first nickel-iron-manganese mixed salt solution (the ratio of nickel ion, iron ion and manganese ion concentration is 42:30:28) with a total metal ion concentration of 100 mol / L is added to the reaction base liquid at a rate of 4 L / h, a sodium hydroxide solution with a concentration of 100 mol / L and an ammonia solution with a concentration of 9 mol / L, the reaction pH is controlled to be 11.2 and the ammonia concentration is 15 g / L, and a first coprecipitation reaction is carried out at 45° C. for 8 h to obtain a primary mixed solution containing a precipitate;
[0126] The first coprecipitation reaction base liquid is composed of a solvent, a precipitant and a complexing agent, the pH of the reaction base liquid is 8.5, and the ammonia concentration is 20 g / L;
[0127] (2) Second stage: In a protective atmosphere, a second nickel-iron-manganese mixed salt solution (the ratio of nickel ion, iron ion and manganese ion concentration is 25:37:38) with a total metal ion concentration of 100 mol / L is added at a rate of 4 L / h to the primary mixed solution containing the precipitate obtained in step (1) in parallel with a sodium hydroxide solution with a concentration of 100 mol / L and an ammonia solution with a concentration of 9 mol / L, the pH is controlled to be 11.2 and the ammonia concentration is 15 g / L, and a second coprecipitation reaction is carried out at 45° C. for 8 h to obtain a remixed solution containing the precipitate;
[0128] (3) The third stage: in a protective atmosphere, a third nickel-iron-manganese mixed salt solution with a total metal ion concentration of 100 mol / L (the ratio of nickel ion, iron ion and manganese ion concentration is 17:52:31) is added at a rate of 4 L / h to the remixed solution obtained in step (2) containing the precipitate, in parallel with a sodium hydroxide solution with a concentration of 100 mol / L and an ammonia solution with a concentration of 9 mol / L, the reaction pH is controlled to be 11.2 and the ammonia concentration is 15 g / L, a third coprecipitation reaction is carried out at 45° C. to obtain a final mixed solution containing the nickel-iron-manganese ternary material core, and aging, solid-liquid separation, washing and drying are carried out in sequence to obtain the nickel-iron-manganese ternary material core;
[0129] (4) using atomic layer deposition technology, the surface of the nickel-iron-manganese ternary material core obtained in step (3) is first coated with a lanthanum shell using lanthanum sulfate as a lanthanum source, and then coated with an iodine shell using sodium bromide as a bromine source, and then aging to remove sulfate and impurity elements, centrifugally washing and drying at 170° C. to obtain the precursor.
[0130] Example 5
[0131] This embodiment provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, which is the same as Example 1 except that the average particle size of the nickel-iron-manganese ternary material core is 3.5 μm, that is, the time of the third coprecipitation reaction in the preparation method is shortened.
[0132] Example 6
[0133] This embodiment provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, which is the same as Example 1 except that the average particle size of the nickel-iron-manganese ternary material core is 10 μm, that is, the time of the third coprecipitation reaction in the preparation method is extended.
[0134] Example 7
[0135] The present embodiment provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, which is the same as Example 1 except that the molar ratio of the sum of metal ions in the nickel-iron-manganese ternary material core to the sum of lanthanum in the lanthanum shell and iodine in the iodine shell is 94:6, and the molar ratio of lanthanum in the lanthanum shell and iodine in the iodine shell remains unchanged.
[0136] Example 8
[0137] The present embodiment provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, which is the same as Example 1 except that the molar ratio of the sum of metal ions in the nickel-iron-manganese ternary material core to the sum of lanthanum in the lanthanum shell and iodine in the iodine shell is 99.9:0.1.
[0138] Example 9
[0139] This embodiment provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, which is the same as that of Embodiment 1 except that the molar ratio of lanthanum in the lanthanum shell layer and iodine in the iodine shell layer is 1:6.
[0140] Example 10
[0141] This embodiment provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, which is the same as that of Embodiment 1 except that the molar ratio of lanthanum in the lanthanum shell layer to iodine in the iodine shell layer is 1:0.3.
[0142] Comparative Example 1
[0143] This comparative example provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, which is the same as Example 1 except that the positions of the lanthanum shell layer and the iodine shell layer are swapped, that is, in step (4) of the preparation method, the iodine shell layer is first deposited on the outside of the nickel-iron-manganese ternary material core and then coated with the lanthanum shell layer.
[0144] Comparative Example 2
[0145] This comparative example provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, which is the same as Example 1 except that the lanthanum shell layer is omitted, that is, the step (4) of depositing the lanthanum shell layer by atomic layer deposition in the preparation method is omitted.
[0146] Comparative Example 3
[0147] This comparative example provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, which is the same as Example 1 except that the iodine shell layer is omitted, that is, the iodine shell layer is deposited by atomic layer deposition in step (4) of the preparation method is omitted.
[0148] Comparative Example 4
[0149] This comparative example provides a precursor of a sodium battery positive electrode material with a nickel gradient distribution, which is the same as Example 1 except that the lanthanum shell layer and the iodine shell layer are omitted, that is, step (4) is omitted.
[0150] Comparative Example 5
[0151] This comparative example provides a precursor for a positive electrode material for a sodium ion battery, which is the same as Example 1 except that along the radial direction of the nickel-iron-manganese ternary material core, the nickel content in the nickel-iron-manganese ternary material core first decreases and then increases from the inside to the outside, that is, the first nickel-iron-manganese mixed salt solution in step (1) of the preparation method is exchanged with the second nickel-iron-manganese mixed salt solution in step (2).
[0152] Comparative Example 6
[0153] This comparative example provides a precursor for a positive electrode material for a sodium ion battery, wherein the nickel content in the nickel-iron-manganese ternary material core remains unchanged along the radial direction of the nickel-iron-manganese ternary material core, that is, the second nickel-iron-manganese mixed salt solution in step (2) and the third nickel-iron-manganese mixed salt solution in step (3) in the preparation method are replaced by the first nickel-iron-manganese mixed salt solution in step (1), and the rest are the same as Example 1.
[0154] Comparative Example 7
[0155] This comparative example provides a precursor for a positive electrode material for a sodium ion battery, wherein the nickel content in the nickel-iron-manganese ternary material core remains unchanged along the radial direction of the nickel-iron-manganese ternary material core, and the lanthanum shell layer and the iodine shell layer are omitted, that is, the second nickel-iron-manganese mixed salt solution in step (2) and the third nickel-iron-manganese mixed salt solution in step (3) in the preparation method are replaced by the first nickel-iron-manganese mixed salt solution in step (1), and step (4) is omitted, and the rest is the same as Example 1.
[0156] The precursors provided in the above examples and comparative examples are mixed with sodium carbonate to obtain a mixture, wherein the molar ratio of the precursor to sodium carbonate is 1:1, and then calcined at 600° C. for 15 hours, and then ground and sieved to obtain a sodium battery positive electrode material;
[0157] At 25°C, the obtained sodium battery positive electrode material was used as the positive electrode main material, and the metal sodium sheet was used as the negative electrode to assemble into CR2032 button batteries. Then, charge and discharge tests were carried out in the voltage range of 1.0 to 4.5 V, and the initial discharge specific capacity and rate performance were obtained as shown in Table 1. Then, the battery was cycled 300 times at 1C / 5C, and the capacity retention rate after 500 cycles at 1C and the capacity retention rate after 500 cycles at 5C were obtained as shown in Table 1.
[0158] Table 1
[0159]
[0160]
[0161] From Table 1, we can get:
[0162] (1) The positive electrode material prepared by the precursor prepared in Examples 1 to 4 of the present invention, and the sodium ion battery prepared by the obtained positive electrode material have a higher initial discharge specific capacity, show higher rate performance at 1C and 5C, and show higher capacity retention rate after 300 cycles at 1C / 5C;
[0163] (2) By comparing Example 1 with Examples 5 and 6, it can be seen that the average particle size of the nickel-iron-manganese ternary material core in the present invention will affect the performance of the prepared precursor, thereby affecting the performance of the sodium ion battery; when the average particle size of the nickel-iron-manganese ternary material core is low, the capacity retention rate after 300 cycles at 1C and 5C will be reduced. This is because small-particle materials are prone to particle agglomeration, structural disintegration and side reactions during long-term cycles, resulting in a decrease in capacity retention rate; when the average particle size of the nickel-iron-manganese ternary material core is high, the first discharge specific capacity will be reduced, and the larger particle size reduces the specific surface area, limiting the embedding and de-embedding of sodium ions;
[0164] (3) By comparing Example 1 with Examples 7 and 8, it can be seen that the molar ratio of the sum of the metal ions in the core of the nickel-iron-manganese ternary material to the sum of the lanthanum in the lanthanum shell and the iodine in the iodine shell will affect the performance of the prepared precursor, thereby affecting the performance of the sodium ion battery; when the molar ratio is low, the capacity retention rate after 300 cycles at 1C and 5C will decrease. This is because the structural stability of the material is affected by the low molar ratio during the long-term cycle, resulting in a decrease in the capacity retention rate; when the molar ratio is high, the first discharge specific capacity will decrease, and more metal ions will be present in the core, which reduces the ratio of lanthanum and iodine in the shell, thereby reducing the specific surface area and ion transfer efficiency of the material, and the rate performance at 1C and 5C will decrease;
[0165] (4) By comparing Example 1 with Examples 9 and 10, it can be seen that the molar ratio of lanthanum in the lanthanum shell layer and iodine in the iodine shell layer will affect the performance of the prepared precursor, thereby affecting the performance of the sodium ion battery; when the molar ratio of La:I is low, the capacity retention rate after 300 cycles at 1C and 5C will be reduced. This is because the lower La:I molar ratio affects the structural stability of the material during long-term cycles, resulting in a decrease in the capacity retention rate; when the La:I molar ratio is high, the first discharge specific capacity will be reduced. A higher La:I molar ratio means that the shell contains relatively more lanthanum, which reduces the ionic conductivity of the material, thereby reducing the sodium ion insertion and deinsertion efficiency, and the rate performance at 1C and 5C is reduced;
[0166] (5) By comparing Example 1 with Comparative Example 1, it can be seen that the order of the lanthanum shell layer and the iodine shell layer coated on the outside of the nickel-iron-manganese ternary material core will affect the performance of the prepared precursor, thereby affecting the performance of the sodium ion battery; when the positions of the lanthanum shell layer and the iodine shell layer are swapped, the initial discharge specific capacity will be reduced, the rate performance at 1C and 5C will be reduced, and the capacity retention rate after 300 cycles at 1C and 5C will be reduced. This is because when the positions of the lanthanum shell layer and the iodine shell layer are swapped, the order of the shell layers will significantly affect the surface properties and ion transport path of the material. The specific arrangement of lanthanum and iodine on the surface of the material plays a key role in the electrochemical properties of the material. After the order is adjusted, the ion insertion / deinsertion efficiency and the material structure stability will change, thereby affecting the overall performance of the battery;
[0167] (6) By comparing Example 1 with Comparative Examples 2 and 4, it can be seen that the precursor of the present invention includes a lanthanum shell layer, and the positive electrode material prepared by the precursor will form a La-O bond. Since the bond strength of the La-O bond is relatively large, La plays a supporting role, adjusts the TM-O (transition metal-oxygen) and Na-O bond lengths, and stabilizes the structure; in addition, the La-O bond can bring more valence electrons to nearby oxygen, thereby increasing the bond energy of the Mn-O ion, which not only ensures the stability of the lattice oxygen skeleton and the reversibility of oxygen redox, but also optimizes the oxygen local electronic structure generated by the mixing of the 5d orbital of La and the 2p orbital of O due to the charge transfer from the 2p orbital of O to the 5d orbital of La, so that O exhibits better resistance to over-oxidation under high pressure. Therefore, the presence of the lanthanum shell layer improves the rate performance of the positive electrode material prepared by the precursor, increases the system stability, and enhances the cycle performance;
[0168] (7) By comparing Example 1 with Comparative Examples 3 and 4, it can be seen that the precursor in the present invention includes an iodine shell layer. The advantage of the iodine shell layer is mainly to strengthen the stability of each bond of Ni-O, Mn-O and Fe-O, thereby improving the stability of the positive electrode material prepared by the precursor;
[0169] (8) By comparing Example 1 with Comparative Examples 5 to 7, it can be seen that in the precursor of the sodium battery positive electrode material with a nickel gradient distribution provided by the present invention, the nickel content in the nickel-iron-manganese ternary material core gradually decreases from the inside to the outside along the radial direction of the nickel-iron-manganese ternary material core, while ensuring the volume energy density of the positive electrode material prepared from the precursor, reducing the mixing of Ni and Na metals in the positive electrode material and reducing the cost.
[0170] The above description is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A precursor of a sodium battery positive electrode material with a nickel gradient distribution, characterized in that: The precursor includes a nickel-iron-manganese ternary material core, and a lanthanum shell layer and an iodine shell layer sequentially coated on the outside of the nickel-iron-manganese ternary material core; along the radial direction of the nickel-iron-manganese ternary material core, the nickel content in the nickel-iron-manganese ternary material core gradually decreases from the inside to the outside.
2. The precursor according to claim 1, characterized in that The average particle size of the nickel-iron-manganese ternary material core is 4 to 8 μm.
3. The precursor according to claim 1 or 2, characterized in that The molar ratio of the sum of metal ions in the nickel-iron-manganese ternary material core to the sum of lanthanum in the lanthanum shell and iodine in the iodine shell is (95-99.7): (0.3-5); Preferably, the molar ratio of lanthanum in the lanthanum shell layer to iodine in the iodine shell layer is 1:(0.5-2).
4. A method for preparing the precursor according to any one of claims 1 to 3, characterized in that: The preparation method comprises: (1) adding a nickel-iron-manganese mixed salt solution, a precipitant solution and a complexing agent solution to a reaction base solution in stages to carry out a coprecipitation reaction to obtain a nickel-iron-manganese ternary material core; Wherein, the staged method comprises at least two stages, and the nickel concentration in the nickel-iron-manganese mixed salt solution added in each previous stage is higher than the nickel concentration in the nickel-iron-manganese mixed salt solution added in the adjacent next stage; (2) Depositing a lanthanum shell layer and an iodine shell layer in sequence on the surface of the obtained nickel-iron-manganese ternary material core to obtain the precursor.
5. The preparation method according to claim 4, characterized in that: The step (1) comprises three stages, wherein the nickel concentration in the nickel-iron-manganese mixed salt solution added in the first stage, the second stage and the third stage is reduced successively; Preferably, in the first stage, the first nickel-iron-manganese mixed salt solution, the precipitant solution and the complexing agent solution are added to the reaction base solution in parallel to perform a first coprecipitation reaction to obtain a primary mixed solution containing a precipitate; Preferably, in the first stage, the total concentration of metal ions in the first nickel-iron-manganese mixed salt solution is 1-20 mol / L, and the concentration ratio of nickel ions, iron ions and manganese ions is (35-45):(22-32):(28-38); Preferably, the addition rate of the first nickel-iron-manganese mixed salt solution in the first stage is 1 to 100 L / h; Preferably, the pH of the first coprecipitation reaction is 10.5 to 11.5, and the ammonia concentration is 5 to 200 g / L; Preferably, the duration of the first stage is 2 to 48 hours; Preferably, the concentration of the precipitant solution is 5 to 15 mol / L, and the concentration of the complexing agent solution is 5 to 10 mol / L; Preferably, in the second stage, the second nickel-iron-manganese mixed salt solution, the precipitant solution and the complexing agent solution are added in parallel to the primary mixed solution containing the precipitate to perform a second coprecipitation reaction to obtain a remixed solution containing the precipitate; Preferably, in the second stage, the total concentration of metal ions in the second nickel-iron-manganese mixed salt solution is 1-20 mol / L, and the concentration ratio of nickel ions, iron ions and manganese ions is (25-35):(32-42):(28-38); Preferably, the addition rate of the second nickel-iron-manganese mixed salt solution in the second stage is 1 to 100 L / h; Preferably, the pH of the second coprecipitation reaction is 10.5-11.5, and the ammonia concentration is 5-200 g / L; Preferably, the duration of the second stage is 2 to 48 hours; Preferably, the concentration of the precipitant solution in the second stage is 5 to 15 mol / L, and the concentration of the complexing agent solution is 5 to 10 mol / L; Preferably, in the third stage, a third nickel-iron-manganese mixed salt solution, a precipitant solution and a complexing agent solution are added in parallel to the remixed solution containing the precipitate to perform a third coprecipitation reaction to obtain a final mixed solution containing the nickel-iron-manganese ternary material core; Preferably, in the third stage, the total concentration of metal ions in the third nickel-iron-manganese mixed salt solution is 1-20 mol / L, and the concentration ratio of nickel ions, iron ions and manganese ions is (15-25):(42-52):(28-38); Preferably, the addition rate of the third nickel-iron-manganese mixed salt solution in the third stage is 1 to 100 L / h; Preferably, the pH of the third coprecipitation reaction is 10.5-11.5, and the ammonia concentration is 5-200 g / L; Preferably, in the third stage, the concentration of the precipitant solution is 5 to 15 mol / L, and the concentration of the complexing agent solution is 5 to 10 mol / L.
6. The preparation method according to claim 4 or 5, characterized in that: The reaction base liquid in step (1) is composed of a solvent, a precipitant and a complexing agent, the pH of the reaction base liquid is 8.5 to 11.7, and the ammonia concentration is 3 to 70 g / L; Preferably, step (1) is carried out in a protective atmosphere, and the temperature of the coprecipitation reaction is controlled to be 30 to 70° C.; Preferably, the deposition methods of the lanthanum shell layer and the iodine shell layer in step (2) are both atomic layer deposition; Preferably, the raw material for depositing the lanthanum shell layer in step (2) comprises any one of lanthanum sulfate, lanthanum chloride or lanthanum nitrate, or a combination of at least two thereof; Preferably, the raw material for the iodine shell deposition in step (2) comprises any one of iodine water, sodium iodide, manganese iodide, barium iodide, copper iodide or magnesium iodide, or a combination of at least two thereof; Preferably, the preparation method further comprises aging, solid-liquid separation, washing and drying carried out in sequence after the coprecipitation reaction in step (1) to obtain the nickel-iron-manganese ternary material core.
7. A sodium battery positive electrode material with nickel gradient distribution, characterized in that: The sodium battery positive electrode material is prepared from the precursor according to any one of claims 1 to 3.
8. A process for preparing the positive electrode material for a sodium battery according to claim 7, characterized in that: The preparation process comprises: The precursor is mixed with a sodium source and sintered in an oxygen atmosphere to obtain the sodium battery positive electrode material.
9. The preparation process according to claim 8, characterized in that: The molar ratio of the precursor to the sodium source is (1-1.2):1; Preferably, the sintering temperature is 400-1000°C and the sintering time is 4-30h; Preferably, the preparation process further comprises grinding and screening performed in sequence after the sintering.
10. A sodium ion battery, characterized in that: The sodium ion battery comprises the sodium battery positive electrode material according to claim 7.