Sodium-ion battery positive electrode material sodium ferric sulfate and preparation method and application thereof

Through sol-gel method and multi-site co-doping technology, a high-performance sodium ion battery positive electrode material, sodium sulfate, was prepared, which solved the problems of low conductivity and poor rate performance of existing materials, and achieved higher electrochemistry Performance and productivity.

CN119008886APending Publication Date: 2024-11-22JINGHE NEW TOWN SHAANXI COAL TECH RES INST NEW ENERGY MATERIALS CO LTD
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411085097.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing sodium ion battery sodium sulfate positive electrode materials have low electronic conductivity and poor rate performance, making it difficult to meet the needs of the energy storage field.

Method used

Sol-gel method is used to prepare sodium ion battery positive electrode material sodium sulfate. By uniformly doping trace elements at the molecular level, particle size and morphology regulation are achieved. Multi-site co-doping and carbon coating technology are used to improve the material's Cyclic stability and rate performance.

Benefits of technology

The conductivity and rate performance of the material is significantly improved, the production process is simplified, the cost is reduced, and the wetting and migration capacity of the electrolyte is improved through carbon cladding, improving the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008886A_ABST
    Figure CN119008886A_ABST
Patent Text Reader

Abstract

The invention discloses a sodium ion battery positive electrode material sodium ferric sulfate as well as a preparation method and application thereof, and the preparation method specifically comprises the following steps: step 1, adding a sodium source, an iron source, an additive and an antioxidant into deionized water, and dissolving to obtain a mixed solution; step 2, adding a thickening agent into the mixed solution, and uniformly stirring to obtain gel; step 3, dehydrating and drying the gel to obtain dry gel; and 4, crushing the dried gel, and sintering to obtain the sodium ferric sulfate powder of the sodium ion battery positive electrode material, which is applied as the sodium ion battery positive electrode material. According to the sodium-ion battery positive electrode material sodium ferric sulfate, the conductivity and the rate capability of the sodium ferric sulfate positive electrode material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of positive electrode materials for sodium ion batteries, and specifically relates to sodium ferric sulfate, a positive electrode material for sodium ion batteries, a preparation method of the sodium ferric sulfate, a positive electrode material for sodium ion batteries, and an application of the sodium ferric sulfate, a positive electrode material for sodium ion batteries. Background Art

[0002] At present, most of the most advanced energy storage systems use lithium-ion battery technology. However, with the fluctuation of lithium-ion battery prices, especially the consumption and future shortage of lithium resources, sodium-ion batteries have attracted people's attention again in recent years and are considered to be a promising next-generation secondary battery system that can replace lithium-ion batteries for large-scale energy storage.

[0003] The cathode material of sodium-ion batteries is a key factor in battery performance. The current mainstream material routes are mainly divided into: layered oxide materials, Prussian blue materials and polyanion materials. Among the three major routes of sodium-ion battery cathode materials, polyanion cathode materials have attracted much attention due to their unique advantages. Polyanion compounds have the characteristics of stable structure, long cycle life, high thermal stability, and high operating voltage, and are particularly suitable for the field of energy storage. Compared with other polyanion materials, iron-based sulfate has a high Fe content. 3+ / Fe 2+ Reversible redox couple and SO4 2- The strong electronegativity of the group has the advantage of high working voltage (3.0-3.8V). However, the crystal structure of sodium iron sulfate determines that it has inherent defects as a positive electrode material for sodium ion batteries, such as low electronic conductivity and poor rate performance. Summary of the invention

[0004] The first purpose of the present invention is to provide sodium ferric sulfate, a positive electrode material for sodium ion batteries, which solves the problems of low conductivity and poor rate performance of existing sodium ferric sulfate positive electrode materials for sodium ion batteries.

[0005] The second object of the present invention is to provide a method for preparing sodium ferric sulfate, a positive electrode material for sodium ion batteries.

[0006] The third object of the present invention is to provide the application of sodium ferric sulfate, a positive electrode material for sodium ion batteries, as a positive electrode material for sodium ion batteries.

[0007] The first technical solution adopted by the present invention is that the positive electrode material of the sodium ion battery is sodium ferric sulfate, and the molecular formula of the positive electrode material of the sodium ion battery is Na 2.5-x M1 x Fe 1.75-y M2 y (SO4)3M3 z@C, 0<x≤0.03, 0<y≤0.1, 0<z≤0.05, and the values ​​of x, y, and z satisfy the charge balance of the chemical formula.

[0008] The second technical solution adopted by the present invention is a method for preparing sodium iron sulfate, a positive electrode material for a sodium ion battery, which is specifically implemented according to the following steps:

[0009] Step 1, adding a sodium source, an iron source, an additive, and an antioxidant into deionized water and dissolving them to obtain a mixed solution;

[0010] Step 2, adding a thickener to the mixed solution obtained in step 1, stirring evenly to obtain a gel;

[0011] Step 3, dehydrating and drying the gel obtained in step 2 to obtain a dry gel;

[0012] Step 4, crushing the dry gel obtained in step 3 and sintering it to obtain sodium iron sulfate powder, which is a positive electrode material for sodium ion batteries.

[0013] The present invention is also characterized in that:

[0014] In step 1, the sodium source is anhydrous sodium sulfate or sodium sulfate decahydrate; the iron source is one of anhydrous ferrous sulfate, ferrous sulfate monohydrate or ferrous sulfate heptahydrate; the antioxidant is one of ascorbic acid, citric acid, tea polyphenols or sodium sulfite;

[0015] The additives include M1, M2 and M3; wherein M1 is one of Li sulfate, Li sulfate hydrate, Li acetate, K sulfate, K sulfate hydrate, K acetate, Mg sulfate, Mg sulfate hydrate, Mg acetate, Ca sulfate, Ca sulfate hydrate, and Ca acetate; M2 is Cu sulfate, Cu sulfate hydrate, Cu oxalate, Ni sulfate, Ni sulfate, etc. Salt hydrate, oxalate of Ni element, sulfate of Zn element, sulfate hydrate of Zn element, oxalate of Zn element, sulfate of Zr element, sulfate hydrate of Zr element, oxalate of Zr element, sulfate of Mn element, sulfate hydrate of Mn element, oxalate of Mn element, sulfate of Ti element, sulfate hydrate of Ti element, oxalate of Ti element; M3 is a phosphorus source or a fluorine source, specifically one of sodium dihydrogen phosphate, ammonium dihydrogen phosphate, potassium dihydrogen phosphate, sodium phosphate, sodium pyrophosphate, potassium pyrophosphate or sodium fluoride.

[0016] In step 1, the mass concentration of the mixed solution is 10% to 20%.

[0017] In step 1, the mass ratio of the antioxidant to the ferrous sulfate in the iron source is 1:3-12.

[0018] In step 2, the thickener is one or more of methyl cellulose, ethyl cellulose, carboxymethyl cellulose, sodium carboxymethyl cellulose, hydroxypropyl methyl cellulose, acrylic copolymer, polyurethane thickener, polyethylene glycol, polyvinyl alcohol, and starch. The amount of thickener added is that the carbon content provided by the thickener accounts for 3-18% of the total mass of the sodium source, the iron source, and the additives, and the mass of the thickener corresponding to the carbon content is the amount of thickener added.

[0019] In step 2, the viscosity of the gel is 1000 mPa·s to 10000 mPa·s.

[0020] In step 3, the dehydration and drying is one of spray drying, low-temperature drying in a nitrogen atmosphere, vacuum drying or freeze drying.

[0021] In step 4, the sintering temperature is 300° C. to 400° C., the holding time is 20 h to 48 h, and the atmosphere is nitrogen or argon.

[0022] The third technical solution adopted by the present invention is to use the sodium iron sulfate powder obtained by the above preparation method as a positive electrode material for a sodium ion battery.

[0023] The beneficial effects of the present invention are:

[0024] (1) The preparation method of the present invention adopts the sol-gel method, which can achieve uniform mixing of reactants at the molecular level compared to the micron-level diffusion of solid-phase reaction, and can evenly and quantitatively incorporate trace elements through solution reaction to achieve uniform doping at the molecular level. At the same time, the preparation method can achieve particle size and morphology control and optimize material performance;

[0025] (2) The preparation method of the present invention adopts a one-pot process to directly obtain the carbon-coated sodium iron sulfate positive electrode material. Compared with the material prepared by sintering once, the carbon coating process of the secondary sintering simplifies the production process, improves production efficiency and reduces costs;

[0026] (3) The preparation method of the present invention is through multi-site co-doping, wherein Na doping stabilizes the material structure while increasing Na + Diffusion kinetics, metal cation doping on Fe site can activate transition metal redox and improve material specific capacity, SO4 2- The substitution of the sites and the use of mixed polyanion groups can enhance the inductive effect, increase the voltage of the material, and utilize the synergistic effect of the doping elements at each site in the system to greatly improve the cycle stability and rate performance of the material;

[0027] (4) The preparation method of the present invention uses high molecular weight organic matter and relies on the decomposition of the organic matter in an inert environment to form a carbon coating layer. This type of material has a certain viscosity after melting and is easily coated on the surface of the active material. After carbonization, loose amorphous carbon is obtained, which is conducive to the infiltration and migration of the electrolyte. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 XRD diagram of sodium iron sulfate powder, a positive electrode material for a sodium ion battery prepared in Example 1 of the present invention;

[0029] Figure 2 This is a SEM image of sodium iron sulfate powder, a positive electrode material for a sodium ion battery prepared in Example 1 of the present invention;

[0030] Figure 3 This is a SEM image of sodium iron sulfate powder, a positive electrode material for a sodium ion battery prepared in Example 2 of the present invention;

[0031] Figure 4 This is an EDS image of sodium iron sulfate powder, a positive electrode material for a sodium ion battery prepared in Example 2 of the present invention;

[0032] Figure 5 The 0.1C charge-discharge capacity curve of sodium iron sulfate powder, a positive electrode material for a sodium ion battery prepared in Example 2 of the present invention;

[0033] Figure 6 This is a SEM image of sodium iron sulfate powder, a positive electrode material for a sodium ion battery prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0034] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0035] The sodium ion battery positive electrode material of the present invention is sodium iron sulfate, the molecular formula is Na 2.5-x M1 x Fe 1.75-y M2 y (SO4)3M3 z @C, 0<x≤0.03, 0<y≤0.1, 0<z≤0.05, and the values ​​of x, y, and z satisfy the charge balance of the chemical formula.

[0036] The preparation method of sodium ferric sulfate, a positive electrode material for a sodium ion battery of the present invention, is specifically implemented according to the following steps:

[0037] Step 1, adding a sodium source, an iron source, an additive, and an antioxidant into deionized water and dissolving them to obtain a mixed solution, wherein the mass concentration of the mixed solution is 10% to 20%;

[0038] The mass ratio of the antioxidant to the ferrous sulfate in the iron source is 1:3-12;

[0039] The molar ratio of sodium source, iron source and additive is described by the molecular formula of sodium iron sulfate, the cathode material of sodium ion battery;

[0040] The sodium source is anhydrous sodium sulfate or sodium sulfate decahydrate;

[0041] The iron source is one of anhydrous ferrous sulfate, ferrous sulfate monohydrate or ferrous sulfate heptahydrate;

[0042] The antioxidant is one of ascorbic acid, citric acid, tea polyphenols or sodium sulfite;

[0043] Additives include M1, M2 and M3;

[0044] M1 is one of a sulfate of the Li element, a sulfate hydrate of the Li element, an acetate of the Li element, a sulfate of the K element, a sulfate hydrate of the K element, an acetate of the K element, a sulfate of the Mg element, a sulfate hydrate of the Mg element, an acetate of the Mg element, a sulfate of the Ca element, a sulfate hydrate of the Ca element, and an acetate of the Ca element;

[0045] M2 is one of a sulfate of Cu element, a sulfate hydrate of Cu element, an oxalate of Cu element, a sulfate of Ni element, a sulfate hydrate of Ni element, an oxalate of Ni element, a sulfate of Zn element, a sulfate hydrate of Zn element, an oxalate of Zn element, a sulfate of Zr element, a sulfate hydrate of Zr element, an oxalate of Zr element, a sulfate of Mn element, a sulfate hydrate of Mn element, an oxalate of Mn element, a sulfate of Ti element, a sulfate hydrate of Ti element, and an oxalate of Ti element;

[0046] M3 is a phosphorus source or a fluorine source, specifically one of sodium dihydrogen phosphate, ammonium dihydrogen phosphate, potassium dihydrogen phosphate, sodium phosphate, sodium pyrophosphate, potassium pyrophosphate or sodium fluoride;

[0047] Step 2, adding a thickener to the mixed solution obtained in step 1, stirring evenly to obtain a gel, wherein the viscosity of the gel is 1000 mPa·s to 10000 mPa·s;

[0048] Wherein, the thickener is one or more of methyl cellulose, ethyl cellulose, carboxymethyl cellulose, sodium carboxymethyl cellulose, hydroxypropyl methyl cellulose, acrylic copolymer, polyurethane thickener, polyethylene glycol, polyvinyl alcohol, and starch;

[0049] The amount of thickener added is that the carbon content provided by the thickener accounts for 3-18% of the total mass of the sodium source, the iron source and the additives, and the mass of the thickener corresponding to the carbon content is the amount of thickener added.

[0050] Step 3, dehydrating and drying the gel obtained in step 2 to obtain a dry gel;

[0051] The dehydration drying is one of spray drying, nitrogen atmosphere low temperature drying (temperature is 80℃~200℃), vacuum drying or freeze drying.

[0052] Step 4, crushing the dry gel obtained in step 3 into powder and then sintering it, the sintering temperature is 300°C to 400°C, the insulation time is 20h to 48h, the atmosphere is nitrogen or argon atmosphere, and sodium iron sulfate powder, a positive electrode material for a sodium ion battery, is obtained.

[0053] Application of the sodium iron sulfate powder obtained by the above preparation method in positive electrode materials of sodium ion batteries.

[0054] Example 1

[0055] Step 1, adding 353.68 g of anhydrous sodium sulfate, 478.18 g of ferrous sulfate heptahydrate, 1.74 g of potassium sulfate, 7.02 g of titanium oxalate, 2.40 g of sodium dihydrogen phosphate, and 21.77 g of ascorbic acid into 3022.5 g of deionized water and dissolving them to obtain a mixed solution;

[0056] Step 2, adding 161.97 g of acrylic copolymer to the mixed solution obtained in step 1, stirring evenly to obtain a gel, the viscosity of the gel is 10000 mPa·s;

[0057] Step 3, vacuum drying the gel obtained in step 2 to obtain a dry gel;

[0058] Step 4, crushing the dry gel obtained in step 3 into powder and placing it in a nitrogen atmosphere tube furnace, sintering at 350°C for 24 hours to obtain sodium iron sulfate powder, a positive electrode material for sodium ion batteries, with a molecular formula of Na 2.49 K 0.01 Fe 1.72 Ti 0.03 (SO4)3(PO4) 0.02 @C.

[0059] like Figure 1 As shown in the figure, the prepared sodium iron sulfate powder of the sodium ion battery positive electrode material belongs to the alumina-magnesium-type Na2Fe2(SO4)3 structure, and its sharp diffraction peak indicates the high crystallinity of the material; Figure 2 As shown, the prepared sodium iron sulfate powder of the sodium ion battery positive electrode material is irregular particles with good overall dispersion.

[0060] Example 2

[0061] Step 1, adding 350.84 g of anhydrous sodium sulfate, 259.76 g of anhydrous ferrous sulfate, 5.29 g of calcium acetate, 9.99 g of copper sulfate pentahydrate, 1.15 g of ammonium dihydrogen phosphate, and 25.98 g of citric acid into 4325.7 g of deionized water and dissolving them to obtain a mixed solution;

[0062] Step 2, adding 129.88 g of starch to the mixed solution obtained in step 1, stirring evenly to obtain a colloidal solution, the viscosity of the colloidal solution is 1000 mPa·s;

[0063] Step 3, spray drying the colloidal solution obtained in step 2 to obtain a powder material;

[0064] Step 4: Place the powder material obtained in step 3 in an argon atmosphere tube furnace and sinter at 380° C. for 20 h to obtain sodium ferric sulfate powder, a positive electrode material for sodium ion batteries, with a molecular formula of Na 2.47 Ca 0.03 Fe 1.71 Cu 0.04 (SO4)3(PO4) 0.01 @C.

[0065] like Figure 3 and Figure 4 As shown in FIG. 1 , the sodium iron sulfate powder particles of the sodium ion battery positive electrode material prepared by spray drying are spherical as a whole, with D50=3.53 μm, and the doped elements Ca, Cu, P and the coated carbon are evenly distributed; Figure 5 As shown, at 2.0-4.5V, the material's 0.1C discharge capacity is 93.42mAh / g, and the first efficiency is 95.89%.

[0066] Example 3

[0067] Step 1, adding 352.26 g of anhydrous sodium sulfate, 480.96 g of ferrous sulfate heptahydrate, 2.41 g of magnesium sulfate, 4.68 g of titanium oxalate, 3.28 g of sodium phosphate, and 87.60 g of ascorbic acid into 6912.1 g of deionized water and dissolving them to obtain a mixed solution;

[0068] Step 2, adding 71.30 g of sodium carboxymethyl cellulose to the mixed solution obtained in step 1, stirring evenly to obtain a gel having a viscosity of 2000 mPa·s;

[0069] Step 3, drying the gel obtained in step 2 in a nitrogen atmosphere to obtain a dry gel;

[0070] Step 4, crushing the dry gel obtained in step 3 into powder and placing it in an argon atmosphere tube furnace, sintering at 300°C for 48h to obtain sodium iron sulfate powder, a positive electrode material for sodium ion batteries, with a molecular formula of Na 2.48 Mg 0.02Fe 1.73 Ti 0.02 (SO4)3(PO4) 0.02 @C.

[0071] like Figure 6 As shown, the prepared sodium iron sulfate powder, a positive electrode material for sodium ion batteries, has a parallelepiped morphology of nano primary particles stacked together, and has good particle integrity and dispersibility.

[0072] Example 4

[0073] The difference from Example 1 is that: Step 1, 352.26 g of anhydrous sodium sulfate, 458.72 g of ferrous sulfate heptahydrate, 2.20 g of lithium sulfate, 28.34 g of zirconium sulfate, 6.00 g of sodium pyrophosphate, 25.06 g of ascorbic acid, and 3114.5 g of deionized water are dissolved to obtain a mixed solution;

[0074] Step 2, adding 166.13 g of acrylic copolymer to the mixed solution obtained in step 1, stirring evenly to obtain a gel;

[0075] In step 4, sodium iron sulfate powder, a positive electrode material for sodium ion batteries, is obtained, and the molecular formula is Na 2.48 Li 0.02 Fe 1.65 Zr 0.1 (SO4)3(P2O7) 0.05 @C.

[0076] The rest of the process is exactly the same as in Example 1.

[0077] Example 5

[0078] The difference from Example 2 is that: Step 1, 799.03 g of sodium sulfate decahydrate, 478.18 g of ferrous sulfate heptahydrate, 3.52 g of calcium acetate, 7.89 g of nickel sulfate hexahydrate, 6.00 g of sodium pyrophosphate, 32.66 g of citric acid, and 3735.5 g of deionized water are dissolved to obtain a mixed solution;

[0079] Step 2, adding 132.07 g of starch to the mixed solution obtained in step 1, stirring evenly to obtain a gel;

[0080] In step 4, sodium iron sulfate powder, a positive electrode material for sodium ion batteries, is obtained, and the molecular formula is Na 2.48 Ca 0.02 Fe 1.72 Ni 0.03 (SO4)3(P2O7) 0.005 @C.

[0081] The rest of the process is exactly the same as in Example 2.

[0082] Example 6

[0083] The difference from Example 3 is that: Step 1, 352.26 g of anhydrous sodium sulfate, 258.24 g of anhydrous ferrous sulfate, 2.41 g of magnesium sulfate, 11.70 g of titanium oxalate, 4.08 g of potassium pyrophosphate, 43.04 g of ascorbic acid, and 6717.3 g of deionized water are dissolved to obtain a mixed solution;

[0084] Step 2, adding 67.17 g of sodium carboxymethyl cellulose to the mixed solution obtained in step 1, stirring evenly to obtain a gel;

[0085] In step 4, sodium iron sulfate powder, a positive electrode material for sodium ion batteries, is obtained, and the molecular formula is Na 2.48 Mg 0.02 Fe 1.7 Ti 0.05 (SO4)3(P2O7) 0.03 @C.

[0086] The rest of the process is exactly the same as in Example 3.

[0087] Example 7

[0088] The difference from Example 1 is that: Step 1, 350.84 g of anhydrous sodium sulfate, 471.23 g of ferrous sulfate heptahydrate, 5.23 g of potassium sulfate, 5.85 g of titanium oxalate, 2.10 g of sodium fluoride, 21.46 g of ascorbic acid, and 3002.5 g of deionized water are dissolved to obtain a mixed solution;

[0089] Step 2, adding 160.81 g of acrylic copolymer to the mixed solution obtained in step 1, stirring evenly to obtain a gel;

[0090] In step 4, sodium iron sulfate powder, a positive electrode material for sodium ion batteries, is obtained, and the molecular formula is Na 2.47 K 0.03 Fe 1.695 Ti 0.025 (SO4)3F 0.05 @C.

[0091] The rest of the process is exactly the same as in Example 1.

[0092] Example 8

[0093] The difference from Example 2 is that: Step 1, 353.68 g of anhydrous sodium sulfate, 458.72 g of ferrous sulfate heptahydrate, 1.20 g of magnesium sulfate, 16.90 g of manganese sulfate monohydrate, 0.42 g of sodium fluoride, 50.13 g of citric acid, and 4264.6 g of deionized water are dissolved to obtain a mixed solution;

[0094] Step 2, adding 134.23 g of starch to the mixed solution obtained in step 1, stirring evenly to obtain a gel;

[0095] In step 4, sodium iron sulfate powder, a positive electrode material for sodium ion batteries, is obtained, and the molecular formula is Na 2.49 Mg 0.01 Fe 1.65 Mn 0.1 (SO4)3F 0.01 @C.

[0096] The rest of the process is exactly the same as in Example 2.

[0097] Example 9

[0098] The difference from Example 3 is that: Step 1, 802.25 g of sodium sulfate decahydrate, 483.74 g of ferrous sulfate heptahydrate, 1.76 g of calcium acetate, 2.83 g of zirconium sulfate, 1.26 g of sodium fluoride, 26.43 g of ascorbic acid, and 5834.8 g of deionized water are dissolved to obtain a mixed solution;

[0099] Step 2, adding 65.03 g of sodium carboxymethyl cellulose to the mixed solution obtained in step 1, stirring evenly to obtain a gel;

[0100] In step 4, sodium iron sulfate powder, a positive electrode material for sodium ion batteries, is obtained, and the molecular formula is Na 2.49 Ca 0.01 Fe 1.74 Zr 0.01 (SO4)3F 0.03 @C.

[0101] The rest of the process is exactly the same as in Example 3.

[0102] Comparative Example 1

[0103] The difference from Example 1 is:

[0104] Step 1, adding 353.68 g of anhydrous sodium sulfate, 478.18 g of ferrous sulfate heptahydrate, and 21.77 g of ascorbic acid to 3022.5 g of deionized water and dissolving them to obtain a mixed solution;

[0105] Step 2, spray drying the mixed solution obtained in step 1, placing the dried powder material in a nitrogen atmosphere tubular furnace, and sintering it at 350° C. for 24 hours to obtain sodium iron sulfate powder, a positive electrode material for a sodium ion battery, namely NFS-KB1.

[0106] Comparative Example 2

[0107] The difference from Example 1 is that 353.68 g of anhydrous sodium sulfate, 478.18 g of ferrous sulfate heptahydrate, and 21.77 g of ascorbic acid are mixed by ball milling and then sintered to obtain sodium ferric sulfate powder, a positive electrode material for a sodium ion battery, which is recorded as NFS-KB2.

[0108] Comparative Example 3

[0109] The difference from Example 1 is that step 2 and step 3 in Example 1 are removed, and the mixed solution obtained in step 1 is spray-dried to obtain sodium iron sulfate powder, a positive electrode material for a sodium ion battery, which is recorded as NFS-DB1.

[0110] Comparative Example 4

[0111] The difference from Example 1 is that: Step 1, 353.68 g of anhydrous sodium sulfate, 478.18 g of ferrous sulfate heptahydrate, and 21.77 g of ascorbic acid are added to 3022.5 g of deionized water and dissolved to obtain a mixed solution;

[0112] Finally, a carbon-coated sodium iron sulfate positive electrode material was obtained, which was recorded as NFS-DB2.

[0113] The rest of the process is exactly the same as in Example 1.

[0114] Sodium iron sulfate positive electrode material button battery performance test:

[0115] The sodium iron sulfate obtained in Examples 1 to 9 and Comparative Examples 1 to 4 was mixed evenly with conductive carbon black and binder PVDF in NMP (N-methylpyrrolidone) in a mass ratio of 85:10:5, and coated on an aluminum foil, dried, and pressed into a positive electrode sheet, and a metal sodium sheet was used as a negative electrode to assemble into a 2032-type button battery. The electrical performance was tested using a blue electric test system, and the test results are shown in Table 1.

[0116] Battery capacity test: In the voltage range of 2.0 to 4.5V, test the discharge specific capacity at 0.1C and 1C.

[0117] Cycle performance test: In the voltage range of 2.0 to 4.5 V, test the capacity retention rate after 100 cycles at 1C.

[0118] Table 1 Electrochemical performance parameters of button cell

[0119]

[0120] It can be seen from Table 1 that the sodium iron sulfate positive electrode material prepared by multi-site doping and carbon coating in various embodiments of the present invention has higher gram capacity and cycle retention rate, indicating that under the limitation of low-temperature sintering preparation of this material, the doping elements play a synergistic role with the sodium source and the iron source, promoting full reaction between the raw materials and improving the generation of active products. At the same time, the introduction of doping elements changes the size and morphology of the primary grains, making the surface of the formed secondary particle agglomerates denser, reducing the specific surface area of ​​the material, and improving the processing performance of the material. In addition, the polymer carbon source forms a uniform carbon coating layer after low-temperature carbonization, which improves the conductivity of the material. The combined effect of the doping elements and the carbon source greatly improves the electrochemical properties of the material.

Claims

1. Sodium iron sulfate, the positive electrode material of sodium ion battery, It is characterized in that The molecular formula of sodium iron sulfate, the positive electrode material of sodium ion battery, is Na 2.5-x M1 x Fe 1.75-y M2 y (SO 4 ) 3 M3 z @C, 0<x≤0.03, 0<y≤0.1, 0<z≤0.05, and the values ​​of x, y, and z satisfy the charge balance of the chemical formula.

2. Preparation method of sodium iron sulfate, a positive electrode material for sodium ion batteries, It is characterized in that Follow the steps below to implement it: Step 1, adding a sodium source, an iron source, an additive, and an antioxidant into deionized water and dissolving them to obtain a mixed solution; Step 2, adding a thickener to the mixed solution obtained in step 1, stirring evenly to obtain a gel; Step 3, dehydrating and drying the gel obtained in step 2 to obtain a dry gel; Step 4, crushing the dry gel obtained in step 3 and sintering it to obtain sodium iron sulfate powder, which is a positive electrode material for sodium ion batteries.

3. The method for preparing sodium iron sulfate as a positive electrode material for sodium ion batteries according to claim 2, It is characterized in that In step 1, the sodium source is anhydrous sodium sulfate or sodium sulfate decahydrate; the iron source is one of anhydrous ferrous sulfate, ferrous sulfate monohydrate or ferrous sulfate heptahydrate; the antioxidant is one of ascorbic acid, citric acid, tea polyphenols or sodium sulfite; The additives include M1, M2 and M3; wherein M1 is one of Li sulfate, Li sulfate hydrate, Li acetate, K sulfate, K sulfate hydrate, K acetate, Mg sulfate, Mg sulfate hydrate, Mg acetate, Ca sulfate, Ca sulfate hydrate, and Ca acetate; M2 is Cu sulfate, Cu sulfate hydrate, Cu oxalate, Ni sulfate, Ni sulfate, etc. Salt hydrate, oxalate of Ni element, sulfate of Zn element, sulfate hydrate of Zn element, oxalate of Zn element, sulfate of Zr element, sulfate hydrate of Zr element, oxalate of Zr element, sulfate of Mn element, sulfate hydrate of Mn element, oxalate of Mn element, sulfate of Ti element, sulfate hydrate of Ti element, oxalate of Ti element; M3 is a phosphorus source or a fluorine source, specifically one of sodium dihydrogen phosphate, ammonium dihydrogen phosphate, potassium dihydrogen phosphate, sodium phosphate, sodium pyrophosphate, potassium pyrophosphate or sodium fluoride.

4. The method for preparing sodium iron sulfate as a positive electrode material for sodium ion batteries according to claim 3, It is characterized in that In step 1, the mass concentration of the mixed solution is 10% to 20%.

5. The method for preparing sodium iron sulfate as a positive electrode material for sodium ion batteries according to claim 4, It is characterized in that In step 1, the mass ratio of the antioxidant to the ferrous sulfate in the iron source is 1:3-12.

6. The method for preparing sodium iron sulfate as a positive electrode material for sodium ion batteries according to claim 5, It is characterized in that In step 2, the thickener is one or more of methyl cellulose, ethyl cellulose, carboxymethyl cellulose, sodium carboxymethyl cellulose, hydroxypropyl methyl cellulose, acrylic copolymer, polyurethane thickener, polyethylene glycol, polyvinyl alcohol, and starch; The amount of thickener added is that the carbon content provided by the thickener accounts for 3-18% of the total mass of the sodium source, the iron source and the additives, and the mass of the thickener corresponding to the carbon content is the amount of thickener added.

7. The method for preparing sodium iron sulfate as a positive electrode material for sodium ion batteries according to claim 6, It is characterized in that In step 2, the viscosity of the gel is 1000 mPa·s to 10000 mPa·s.

8. The method for preparing sodium iron sulfate as a positive electrode material for sodium ion batteries according to claim 7, It is characterized in that In step 3, the dehydration and drying is one of spray drying, low-temperature drying in a nitrogen atmosphere, vacuum drying or freeze drying.

9. The method for preparing sodium iron sulfate as a positive electrode material for sodium ion batteries according to claim 8, It is characterized in that In step 4, the sintering temperature is 300° C. to 400° C., the holding time is 20 h to 48 h, and the atmosphere is nitrogen or argon.

10. Use of the sodium iron sulfate powder obtained by the preparation method according to any one of claims 2 to 9 as a positive electrode material for sodium ion batteries.

Citation Information

Cited By

  • Co-doped sodium ferrous sulfate positive electrode material as well as preparation method and application thereof

    CN120854551A

  • Sodium ferric sulfate composite positive electrode material for quasi-solid sodium ion battery and preparation method of sodium ferric sulfate composite positive electrode material

    CN122393255A