Positive electrode material as well as preparation method and application thereof
By forming a lithium oxide layer on the surface of the lithium-rich manganese-based layered oxide and using residual lithium to form a cladding layer, the problems of low initial Coulomb efficiency and slow kinetics of the material are solved, the process is simplified, energy consumption is reduced, and the The capacity and conductivity of lithium-ion batteries enhance the stability and safety of the material.
Patent Information
- Application Number
- CN202411091567.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-22
AI Technical Summary
Lithium-rich manganese-based layered oxides have low initial Coulomb efficiency, slow kinetics, poor rate performance in lithium-ion batteries, and residual lithium on the surface of the material can easily react with air, resulting in battery safety risks. The existing technology is complex and has high energy consumption.
By forming a lithium oxide layer on the surface of the lithium-rich manganese-based matrix material, forming a cladding layer with residual lithium, controlling the addition amount of lithium source compounds and precursors, performing primary and secondary calcination to form lithium nickel manganese oxide or lithium cobalt The oxide layer enhances the capacity and conductivity of the material.
The preparation process is simplified, energy consumption is reduced, the first capacity and conductivity of the material are improved, the interface stability and mechanical strength of the material are enhanced, and the safety hazards of battery inflation are avoided.
Smart Images

Figure BDA0004986726740000081 
Figure BDA0004986726740000091 
Figure BDA0004986726740000092
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a positive electrode material and a preparation method and application thereof. Background Art
[0002] Lithium-rich layered oxides (LLOs), also known as Li 1+x M 1-x O 2 or xLi 2 MnO 3 -(1-x)LiMO 2 (0<x<1, M=Ni,Co,Mn), due to its high specific capacity (280~310mAh·g -1 )、High working potential (~3.7V(vs.Li + / Li 0 )) and high energy density (~900Wh·kg -1 ) and other advantages, and is considered to be one of the most promising positive electrode materials for lithium-ion batteries. However, due to the fact that metal cations and oxygen anions participate in charge compensation during the charge and discharge process of lithium-rich manganese-based layered oxides, they have low initial coulombic efficiency, slow kinetics, poor rate performance, voltage decay during electrochemical cycles, and continuous structural changes during the cycle. These technical problems restrict the development and commercialization of lithium-rich materials. In addition, lithium-rich manganese-based materials are alkaline as a whole, and the free lithium and residual lithium oxides on the surface are easily reacted with moisture and CO in the air. 2 The reaction will generate lithium carbonate and lithium hydroxide, which will further increase the pH value of the material, and will also affect the preparation of battery slurry in the future. After the battery is made, it may also cause safety hazards such as flatulence. In addition, the residual lithium Li on the surface of the material 2 O will also participate in the reaction during the charging and discharging process, affecting the capacity of the material.
[0003] In response to the above problems, currently, technical means such as washing and coating materials are commonly used methods to modify battery positive electrode materials. Chinese invention patent CN111793824 B generates a surface coating layer of lithium bis(oxalatoborate) LiBOB in situ under low temperature conditions, which can realize the surface BOB salt coating of high-nickel positive electrode materials while reducing the residual lithium on the surface of the material, but the capacity is poor. Customized equipment tablet presses are required during the preparation process, which makes mass production difficult and difficult to meet market demand. Chinese invention patent CN111653761B chooses to use an aqueous solution containing additives as a washing detergent. The additives can inhibit the release of structural lithium from the material during the washing process, protect the material structure, and improve the washing process. However, during the washing process, the material must undergo a series of process flows such as screening, washing, filtration, and drying to obtain a one-time process product. It still needs to be coated and sintered to obtain the finished material. The process is relatively complicated and the cost is high.
[0004] In order to solve the technical problems of low initial Coulombic efficiency, slow kinetics, and poor rate performance of lithium-rich materials, and to prevent safety hazards such as homogenization problems and battery bloating caused by excessive residual alkali in the materials, the existing technology mainly uses water washing and coating to reduce residual lithium and improve the initial Coulombic efficiency. However, compared with high-temperature solid-phase sintering, reducing residual lithium in materials by water washing has a complicated process flow and high energy loss. Traditional coating methods will reduce the initial capacity of the material.
[0005] Therefore, providing a positive electrode material with a simple preparation method, low energy consumption, and high initial capacity becomes a problem to be solved. Summary of the invention
[0006] In view of this, the technical problem to be solved by the present invention is to provide a positive electrode material and a preparation method and application thereof. The preparation method of the positive electrode material provided by the present invention is simple, has low energy consumption, and has a higher initial capacity.
[0007] The present invention provides a positive electrode material, comprising a lithium-rich manganese-based matrix material and a lithium oxide layer coated on the surface of the lithium-rich manganese-based matrix material, wherein the lithium oxide layer is selected from a lithium nickel manganese oxide layer, a lithium nickel cobalt manganese oxide layer or a lithium cobalt oxide layer;
[0008] The general formula of the lithium nickel manganese oxide layer and the lithium nickel cobalt manganese oxide layer is Li x Ni a Co b Mn c O 2 , where 0.4≤x≤1.33, 0≤a≤0.8, 0≤b≤0.2, 0≤c≤1.2, x+a+b+c=2;
[0009] The lithium cobalt oxide layer has the general formula Li x Co2-x O 2 , where 0.4≤x≤1.
[0010] Preferably, the lithium-rich manganese-based matrix material has the general formula Li 1+x Ni a Co b Mn c M d O 2 , wherein 0≤x≤0.33, 0≤a≤0.8, 0≤b≤0.2, 0≤c≤0.6, 0≤d≤0.1, x+a+b+c+d=1, and M is selected from one or more of Al, Mg, Ti, Zr, Y, Zn, Nb, Mo, W, B, Ca, Si and La series elements.
[0011] Preferably, the average particle size of the lithium-rich manganese-based matrix material is 2 μm to 14 μm.
[0012] Preferably, the mass of the lithium oxide layer accounts for 1% to 7% of the mass of the lithium-rich manganese-based matrix material.
[0013] The present invention also provides a method for preparing the above-mentioned positive electrode material, comprising the following steps:
[0014] A) calcining a mixture containing a Li source compound, a precursor and an M source compound to obtain a lithium-rich manganese-based matrix material, wherein the precursor is selected from a nickel-cobalt-manganese precursor or a nickel-manganese precursor;
[0015] B) testing and calculating the residual lithium content on the surface of the lithium-rich manganese-based matrix material;
[0016] C) mixing the raw material for preparing the lithium oxide layer with the lithium-rich manganese-based matrix material, and then calcining the mixture twice to obtain a lithium-rich manganese-based positive electrode material;
[0017] The raw materials for preparing the lithium oxide layer include a Li source compound and a precursor, wherein the precursor is selected from at least one of a Co source compound, a nickel-manganese compound or a nickel-cobalt-manganese compound;
[0018] The amount of the lithium source compound added is controlled by the residual lithium content.
[0019] Preferably, in step A), the Li source compound includes at least one of lithium carbonate, lithium hydroxide monohydrate, lithium fluoride, lithium acetate, lithium oxalate, and lithium nitrate;
[0020] The nickel-cobalt-manganese precursor includes at least one of nickel-cobalt-manganese hydroxide and nickel-cobalt-manganese carbonate;
[0021] The nickel manganese precursor includes at least one of nickel manganese hydroxide and nickel manganese carbonate;
[0022] The M source compound is selected from oxides containing M elements;
[0023] The total molar amount of the metal element in the precursor and the M element in the M source compound is called the total metal molar amount. The ratio of lithium in the Li source compound to the total metal molar amount is 1.2 to 2.0, preferably 1.3 to 1.9.
[0024] Preferably, in step A), the primary calcination is carried out at a temperature of 750 to 1050° C. and for a time of 6 to 40 hours.
[0025] Preferably, in step C), the Li source compound is selected from at least one of lithium carbonate, lithium hydroxide monohydrate, lithium fluoride, lithium acetate, lithium oxalate, and lithium nitrate;
[0026] The Co source compound is selected from Co oxide, Co hydroxide, and Co carbonate, and the particle size D50 of the Co source compound is in the range of 0.5 to 2 μm;
[0027] The nickel-manganese compound is selected from one or more of nickel-manganese hydroxides and nickel-manganese carbonates;
[0028] The nickel-cobalt-manganese compound is selected from one or more of nickel-cobalt-manganese hydroxides and nickel-cobalt-manganese carbonates; the particle size D50 of the nickel-manganese compound and the nickel-cobalt-manganese compound is in the range of 0.5 to 2 μm;
[0029] The ratio of the total molar amount of lithium in the Li source compound and residual lithium on the surface of the lithium-rich manganese-based matrix material to the total molar amount of cobalt, nickel and manganese in the Co source compound and / or nickel manganese compound and / or nickel cobalt manganese compound is 0.1-2.0, preferably 0.8-1.8.
[0030] Preferably, the secondary sintering temperature is 350-950° C. and the time is 3-15 hours.
[0031] The present invention also provides a lithium ion battery comprising the above-mentioned positive electrode material.
[0032] Compared with the prior art, the present invention provides a positive electrode material, comprising a lithium-rich manganese-based matrix material and a lithium oxide layer coated on the surface of the lithium-rich manganese-based matrix material, wherein the lithium oxide layer is selected from a lithium nickel manganese oxide layer, a lithium nickel cobalt manganese oxide layer or a lithium cobalt oxide layer, and the general formula of the lithium nickel manganese oxide layer and the lithium nickel cobalt manganese oxide layer is Li x Ni a Co b Mn c O 2 , wherein 0.4≤x≤1.33, 0≤a≤0.8, 0≤b≤0.2, 0≤c≤1.2, x+a+b+c=2, and the lithium cobalt oxide layer has the general formula Lix Co 2-x O 2 , wherein 0.4≤x≤1. The lithium oxide layer in the positive electrode material provided by the present invention can utilize the residual lithium on the surface of the lithium-rich manganese-based matrix material, consume the residual lithium and form a coating layer that can provide capacity, thereby improving the capacity of the material; at the same time, the coating layer can modify the surface of the lithium-rich manganese-based matrix material particles, improve the material interface stability, and improve the mechanical strength of the particles. The coating layer can also improve the problem of poor electronic conductivity of the traditional inert coating layer, thereby improving the Li + Transmission efficiency, thereby increasing capacity.
[0033] The present invention also provides a method for preparing a positive electrode material, comprising the following steps: A) calcining a mixture containing a Li source compound, a precursor and an M source compound once to obtain a lithium-rich manganese-based matrix material, wherein the precursor is selected from a nickel-cobalt-manganese precursor or a nickel-manganese precursor; B) testing and calculating the residual lithium content on the surface of the lithium-rich manganese-based matrix material; C) mixing the raw material for preparing a lithium oxide layer with the lithium-rich manganese-based matrix material, and calcining for a second time to obtain a lithium-rich manganese-based positive electrode material; the raw material for preparing the lithium oxide layer includes a Li source compound and a precursor, and the raw material for preparing the precursor is selected from at least one of a Co source compound, a nickel-manganese compound or a nickel-cobalt-manganese compound; and controlling the amount of the lithium source compound added by the residual lithium content. The present invention tests the content of residual alkali on the surface of the particles, wherein the residual alkali mainly exists in the form of lithium hydroxide and lithium carbonate, and calculates the free Li on the surface of the lithium-rich manganese-based matrix material through the test results. + Content, that is, the total amount of residual lithium on the surface of the primary particles. According to the calculation results, a lithium source and one or more of a small-particle Co source compound, a nickel-manganese compound or a nickel-cobalt-manganese compound are added again to make the Li / Me value at a certain value or within a certain range. While in-situ coating, the residual lithium on the surface is utilized to generate an in-situ Co-rich or Mn-rich coating layer to provide capacity for the material and improve the initial coulombic efficiency and conductivity of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 This is a SEM image of the positive electrode material prepared in Example 8;
[0035] Figure 2 This is an enlarged SEM image of the surface of the positive electrode material prepared in Example 8. DETAILED DESCRIPTION
[0036] The present invention provides a positive electrode material, comprising a lithium-rich manganese-based matrix material and a lithium oxide layer coated on the surface of the lithium-rich manganese-based matrix material, wherein the lithium oxide layer is selected from a lithium nickel manganese oxide layer, a lithium nickel cobalt manganese oxide layer or a lithium cobalt oxide layer;
[0037] The general formula of the lithium nickel manganese oxide layer and the lithium nickel cobalt manganese oxide layer is Li x Ni a Co b Mn c O 2 , where 0.4≤x≤1.33, 0≤a≤0.8, 0≤b≤0.2, 0≤c≤1.2, x+a+b+c=2;
[0038] When the lithium oxide layer is a lithium nickel manganese oxide layer, b=0 in the general formula, which is Li x Ni a Mn c O 2 , where 0.4≤x≤1.33, 0≤a≤0.8, 0≤c≤1.2, x+a+c=2;
[0039] When the lithium oxide layer is a lithium nickel cobalt manganese oxide layer, b≠0 in the general formula, Li x Ni a Co b Mn c O 2 , where 0.4≤x≤1.33, 0≤a≤0.8, 0<b≤0.2, 0≤c≤1.2, x+a+b+c=2.
[0040] The lithium cobalt oxide layer has a general formula of Li x Co 2-x O 2 , where 0.4≤x≤1.
[0041] The positive electrode material provided by the present invention comprises a lithium-rich manganese-based matrix material, wherein the lithium-rich manganese-based matrix material has a general formula of Li 1+x Ni a Co b Mn c M d O 2 , wherein 0≤x≤0.33, 0≤a≤0.8, 0≤b≤0.2, 0≤c≤0.6, 0≤d≤0.1, x+a+b+c+d=1, and M is selected from one or more of Al, Mg, Ti, Zr, Y, Zn, Nb, Mo, W, B, Ca, Si and La series elements.
[0042] The average particle size of the lithium-rich manganese-based matrix material is 2 μm to 14 μm, and can be 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or any value between 2 μm and 14 μm.
[0043] The mass of the lithium oxide layer accounts for 1% to 7% of the mass of the lithium-rich manganese-based matrix material, and can be 1%, 2%, 3%, 4%, 5%, 6%, 7%, or any value between 1% and 7%.
[0044] The present invention also provides a method for preparing the above-mentioned positive electrode material, comprising the following steps:
[0045] A) calcining a mixture containing a Li source compound, a precursor and an M source compound to obtain a lithium-rich manganese-based matrix material, wherein the precursor is selected from a lithium nickel manganese oxide layer, a lithium nickel cobalt manganese oxide layer or a nickel manganese precursor;
[0046] B) testing and calculating the residual lithium content on the surface of the lithium-rich manganese-based matrix material;
[0047] C) mixing the raw material for preparing the lithium oxide layer with the lithium-rich manganese-based matrix material, and then calcining the mixture twice to obtain a lithium-rich manganese-based positive electrode material;
[0048] The raw materials for preparing the lithium oxide layer include a Li source compound and a precursor, and the raw materials for preparing the precursor are selected from at least one of a Co source compound, a nickel-manganese compound or a nickel-cobalt-manganese compound;
[0049] The amount of the lithium source compound added is controlled by the residual lithium content.
[0050] The present invention first prepares a lithium-rich manganese-based matrix material. Specifically, a mixture containing a Li source compound, a precursor and an M source compound is calcined once to obtain the lithium-rich manganese-based matrix material.
[0051] Wherein, the Li source compound includes at least one of lithium carbonate, lithium hydroxide monohydrate, lithium fluoride, lithium acetate, lithium oxalate, and lithium nitrate, preferably lithium carbonate;
[0052] The precursor is selected from a nickel-cobalt-manganese precursor or a nickel-manganese precursor, wherein the nickel-cobalt-manganese precursor includes at least one of nickel-cobalt-manganese hydroxide and nickel-cobalt-manganese carbonate; the nickel-manganese precursor includes at least one of nickel-manganese hydroxide and nickel-manganese carbonate;
[0053] The total molar amount of the metal element in the precursor and the M element in the M source compound is called the total metal molar amount. The ratio of the lithium in the Li source compound to the total metal molar amount is 1.2 to 2.0, preferably 1.3 to 1.9, and can be 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, or any value between 1.3 and 1.9.
[0054] The primary calcination temperature is 750-1050°C, which can be 750, 800, 850, 900, 950, 1000, 1050, or any value between 750 and 1050°C, and the time is 6-40h, which can be 6, 10, 15, 20, 25, 30, 35, 40, or any value between 6 and 40h.
[0055] The average particle size of the obtained lithium-rich manganese-based matrix material is 2 μm to 14 μm, and can be 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, or any value between 2 μm and 14 μm.
[0056] Then, the residual lithium content on the surface of the lithium-rich manganese-based matrix material is tested and calculated. In the present invention, the method provided in "GB / T41704-2022 Lithium-ion Battery Positive Electrode Material Detection Method Determination of Magnetic Foreign Matter Content and Residual Alkali Content" is used to test and calculate the residual lithium content on the surface of the lithium-rich manganese-based matrix material.
[0057] Then, after obtaining the residual lithium content on the surface of the lithium-rich manganese-based matrix material, the addition amount of the raw material lithium source compound in the lithium oxide layer can be controlled.
[0058] The raw material for preparing the lithium oxide layer is mixed with the lithium-rich manganese-based matrix material, and then calcined twice to obtain a lithium-rich manganese-based positive electrode material;
[0059] The raw materials for preparing the lithium oxide layer include a Li source compound and a precursor, and the raw materials for preparing the precursor are selected from at least one of a Co source compound, a nickel-manganese compound or a nickel-cobalt-manganese compound;
[0060] The amount of the lithium source compound added is controlled by the residual lithium content.
[0061] The Li source compound is selected from at least one of lithium carbonate, lithium hydroxide monohydrate, lithium fluoride, lithium acetate, lithium oxalate, and lithium nitrate;
[0062] The Co source compound is selected from Co oxides, Co hydroxides, and Co carbonates, preferably Co(OH) 2 The particle size D50 of the Co source compound is in the range of 0.5 to 2 μm, and can be 0.5, 1, 1.5, 2, or any value between 0.5 and 2 μm;
[0063] The nickel-manganese compound is selected from one or more of nickel-manganese hydroxides and nickel-manganese carbonates;
[0064] The nickel-cobalt-manganese compound is selected from one or more of nickel-cobalt-manganese hydroxides and nickel-cobalt-manganese carbonates;
[0065] The particle size D50 of the nickel-manganese compound and the nickel-cobalt-manganese compound is in the range of 0.5 to 2 μm, and can be 0.5, 1, 1.5, 2, or any value between 0.5 and 2 μm;
[0066] The present invention can achieve good coating of the lithium oxide layer by controlling the particle size of the precursor raw material used in the secondary coating.
[0067] The present invention controls the lithium metal molar ratio during secondary coating of the mixture, adds a Li source compound and a small-particle Co source compound, a nickel-manganese compound or a nickel-cobalt-manganese compound and performs secondary sintering, thereby utilizing the residual lithium on the surface of the primary process product and generating a Co-rich or Mn-rich coating layer in situ, providing capacity for the material and improving the initial coulombic efficiency and conductivity of the material.
[0068] The ratio of the total molar amount of lithium in the Li source compound and the residual lithium on the surface of the lithium-rich manganese-based matrix material to the total molar amount of cobalt, nickel and manganese in the Co source compound and / or the nickel-manganese compound and / or the nickel-cobalt-manganese compound is 0.1 to 2.0, and can be 0.1, 0.3, 0.5, 0.8, 1.0, 1.2, 1.4, 1.5, 1.6, 1.8, 2.0, or any value between 0.1 and 2.0, preferably any value between 0.8 and 1.8.
[0069] The secondary sintering temperature is 350-950°C, which can be 350, 400, 450, 500, 550, 600, 650, 700, 750, 800, 850, 900, 950, or any value between 350 and 950°C, and the time is 3-15h, which can be 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, or any value between 3 and 15h.
[0070] In the present invention, part of the lithium in the lithium oxide layer comes from the residual lithium on the surface of the lithium-rich manganese-based matrix material, and the other part comes from the lithium source compound in the raw material for preparing the lithium-rich oxide layer.
[0071] The present invention tests and calculates the residual lithium content on the surface of the material after the primary sintering, controls the primary residual lithium amount during the secondary coating mixture, and the lithium metal molar ratio of the Li source compound to the Co-rich and / or Mn-rich precursor as a whole. This not only utilizes the surface residual lithium of the primary process product to make it contribute capacity to the material, but also can in-situ generate a Co-rich and / or Mn-rich coating layer during the secondary coating to provide capacity for the material, thereby improving the initial coulombic efficiency and conductivity of the material.
[0072] The present invention also provides a positive electrode plate, comprising the above-mentioned positive electrode material, wherein the positive electrode material is a lithium-rich manganese-based positive electrode material.
[0073] The present invention also provides a lithium-ion battery, comprising the above-mentioned positive electrode plate.
[0074] The lithium-rich oxide layer in the positive electrode material provided by the present invention can utilize the residual lithium on the surface of the lithium-rich manganese-based matrix material, consume the residual lithium and form a coating layer that can provide capacity, thereby improving the capacity of the material; at the same time, the coating layer can modify the surface of the particles, improve the material interface stability, and improve the mechanical strength of the particles. The coating layer can also improve the problem of poor electronic conductivity of the traditional inert coating layer, thereby improving the Li + Transmission efficiency, thereby increasing capacity.
[0075] The preparation method of the positive electrode material provided by the present invention tests and calculates the residual lithium content on the surface of the lithium-rich manganese-based matrix material, and according to the calculation result, adds a lithium source and one or more of a small-particle Co source compound, a nickel-manganese compound or a nickel-cobalt-manganese compound again to make Li / Me within a certain value or a certain range, and utilizes the residual lithium on the surface during in-situ coating to generate a Co-rich or Mn-rich coating layer in-situ, thereby providing capacity for the material and improving the initial coulombic efficiency and conductivity of the material.
[0076] In order to further understand the present invention, a positive electrode material provided by the present invention and its preparation method and application are described below in conjunction with embodiments. The protection scope of the present invention is not limited by the following embodiments.
[0077] Example 1 and Examples 2 to 9 and Comparative Examples
[0078] 1. Preparation of positive electrode materials
[0079] 100 g of a hydroxide precursor containing Ni, Co, and Mn [Ni 0.25 Mn 0.66 Co 0.09 ](OH) 2 、53.15gLi 2 CO 3 , 0.21g Mg-containing oxide MgO was mixed and milled for the first sintering at a temperature of 830°C for 20h. After natural cooling, the mixture was crushed and sieved to obtain a lithium-rich manganese-based matrix material Li 1.128 Ni 0.217 Mn 0.573 Co 0.078 Mg 0.004 O 2 ;
[0080] 50g of lithium-rich manganese-based matrix material Li 1.128 Ni 0.217 Mn 0.573 Co 0.078 Mg 0.004 O 2 , 0.03g Li 2 CO 3and 1.0gD50 of 0.6um Co(OH) 2 After the mixed ball milling, the second sintering was carried out at a sintering temperature of 880 ° C for 8 hours. After natural cooling, the material was crushed and sieved to obtain the coated lithium-rich manganese-based material Li 1.128 Ni 0.217 Mn 0.573 Co 0.078 Mg 0.004 O 2 O 2 @Li 0.95 Co 1.05 O 2 .
[0081] The preparation methods of the positive electrode materials in Examples 2-9 are basically similar to the preparation method of the positive electrode materials in Example 1, and the main differences are: the chemical formula of the hydroxide precursor containing Ni, Co, and Mn, the type and / or amount of the soluble lithium salt added during the first mixing and ball milling, the type and / or amount of the doping element and the compound containing the doping element during the first mixing and ball milling, the first sintering temperature, the first sintering insulation time, the chemical formula of the matrix added during the second mixing and ball milling, the type and / or amount of the soluble lithium salt added during the second mixing and ball milling, the type and / or amount of the coating precursor during the second mixing and ball milling, the particle size of the coating precursor during the second mixing and ball milling, the molar ratio of lithium to the total metal elements during the second mixing and ball milling, the second sintering temperature, and the second sintering insulation time are different. For details, see Tables 1 to 6.
[0082] In particular, the residual lithium test results of the primary matrix in Examples 1-9 are detailed in Table 7, and the lithium content in the "molar ratio of lithium to total metal elements" during the secondary mixing and ball milling includes the residual lithium content in the primary matrix.
[0083] See also Figure 1 and Figure 2 , Figure 1 This is the SEM image of the positive electrode material prepared in Example 8. Figure 2 This is an enlarged SEM image of the surface of the positive electrode material prepared in Example 8.
[0084] The preparation parameters and structural parameters of the positive electrode materials in the above-mentioned embodiments and comparative examples are shown in Tables 1 to 7, respectively.
[0085] Table 1 Chemical formula of lithium-rich manganese-based matrix materials
[0086]
[0087]
[0088] Table 2 Chemical formula and dosage of precursors for preparing lithium-rich manganese-based matrix materials
[0089] Example Precursor chemical formula Precursor mass / g Example 1 < 2 ]]> 100 Example 2 < 2 ]]> 100 Example 3 < 2 ]]> 100 Example 4 < 2 ]]> 100 Example 5 < 2 ]]> 100 Example 6 < 2 ]]> 100 Example 7 < 2 ]]> 100 Example 8 < 2 ]]> 100 Example 9 < 2 ]]> 100 Comparative Example 1 < 2 ]]> 100 Comparative Example 2 < 2 ]]> 100 Comparative Example 3 < 2 ]]> 100
[0090] Table 3 Primary lithium salts for preparing lithium-rich manganese-based matrix materials
[0091] Example Primary lithium salt Primary lithium salt mass / g One-time Li / Me Example 1 <![CDATA[Li 2 CO 3 ]]> 53.15 1.3 Example 2 <![CDATA[Li 2 CO 3 ]]> 65.40 1.6 Example 3 <![CDATA[Li 2 CO 3 ]]> 69.91 1.7 Example 4 <![CDATA[LiOH·H 2 The]]> 83.06 1.8 Example 5 <![CDATA[Li 2 CO 3 ]]> 77.15 1.9 Example 6 <![CDATA[Li 2 CO 3 ]]> 47.47 1.2 Example 7 <![CDATA[Li 2 CO 3 ]]> 65.49 1.6 Example 8 <![CDATA[Li 2 CO 3 ]]> 69.58 1.7 Example 9 <![CDATA[Li 2 CO 3 ]]> 73.67 1.8 Comparative Example 1 <![CDATA[Li 2 CO 3 ]]> 65.49 1.6 Comparative Example 2 <![CDATA[Li 2 CO 3 ]]> 65.49 1.6 Comparative Example 3 <![CDATA[Li 2 CO 3 ]]> 65.49 1.6
[0092] Table 4 Additive types and sintering conditions for preparing lithium-rich manganese-based matrix materials
[0093]
[0094]
[0095] Table 5 Parameters for preparing coating layer
[0096]
[0097] Table 6 Parameters for preparing coating layer
[0098] Example Secondary Li / Me Secondary lithium salt Secondary lithium salt mass / g Sintering temperature / ℃ Insulation time / h Example 1 0.8 <![CDATA[Li 2 CO 3 ]]> 0.03 880 8 Example 2 0.9 <![CDATA[Li 2 CO 3 ]]> 0.05 875 10 Example 3 1.1 <![CDATA[Li 2 CO 3 ]]> 0.57 680 12 Example 4 1.3 <![CDATA[LiOH·H 2 The]]> 0.09 350 15 Example 5 1.4 <![CDATA[Li 2 CO 3 ]]> 0.94 900 8 Example 6 1.6 <![CDATA[Li 2 CO 3 ]]> 0.39 875 3 Example 7 1 <![CDATA[Li 2 CO 3 ]]> 0.22 500 6 Example 8 1.2 LiF 0.18 650 6 Example 9 1.8 <![CDATA[Li 2 CO 3 ]]> 0.71 950 6 Comparative Example 1 / / / / / Comparative Example 2 / / / 880 6 Comparative Example 3 2 <![CDATA[Li 2 CO 3 ]]> 2.22 950 15
[0099] Table 7 Residual lithium content of primary matrix
[0100]
[0101]
[0102] 2. Preparation of batteries
[0103] (1) Preparation of a positive electrode for a lithium-ion half-cell: The positive electrode materials prepared in the above embodiments and comparative examples are uniformly mixed with a conductive agent, acetylene black (Super P), and polyvinylidene fluoride (PVDF) at a mass ratio of 90:5:5, and the mixture is adjusted into a slurry using N-methyl-pyrrolidone (NMP), and then evenly applied on an aluminum foil. After vacuum drying, the pressed sheet is taken out and cut into a positive electrode sheet of a desired size;
[0104] (2) Preparation of lithium-ion half-cell: The lithium-ion battery is assembled from the above-mentioned positive electrode sheet, lithium negative electrode sheet, separator between the positive and negative electrodes, and electrolyte. The assembled battery is used for capacity testing.
[0105] 3. Chemical performance test
[0106] The button cells prepared in the above embodiments and comparative examples were tested using a Blue Electric charge and discharge instrument. The charge and discharge capacity test format was as follows: at room temperature, the charge and discharge voltage range was 2.0 to 4.6V, the cells were charged to 4.6V at a constant current rate of 0.1C, charged to 50uA at a constant voltage, and then discharged to 2.0V at 0.1C, and the first charge and discharge specific capacity was tested. The test results are shown in Table 3.
[0107] Residual lithium test can test the residual lithium of the finished product after coating+ The test results are still shown in Table 8.
[0108] Table 8: Battery performance and residual lithium content of finished products after coating
[0109]
[0110] It can be seen from the results in Table 8 that, compared with the results of Comparative Examples 1 to 3, the specific charge and discharge capacity and the first coulombic efficiency of Examples 1 to 8 at 4.6V and 0.1C are significantly improved. The technicians analyzed that the reason may be that when synthesizing the lithium-rich material, the residual lithium content on the surface of the lithium-rich manganese-based matrix material is tested and calculated. According to the calculation results, one or more of the lithium source and the small-particle Co source compound, the nickel-manganese compound or the nickel-cobalt-manganese compound are added again to make Li / Me at a certain value or a certain range, thereby forming a secondary coating layer. On the one hand, the synthesis method can make the secondary added small-particle Co source compound, the nickel-manganese compound or the nickel-cobalt-manganese compound react with the residual lithium on the surface of the primary particles to consume the residual lithium on the surface, so as to avoid excessive residual lithium on the surface from reacting with H in the air. 2 O and CO 2 reaction, resulting in material failure; on the other hand, the residual lithium on the surface of the primary particles and the newly added lithium source and small-particle Co source compound, nickel-manganese compound or nickel-cobalt-manganese compound can form a lithium oxide coating layer in situ. This coating layer can exist as a similar lithium supplement during the charging process, provide active lithium ions, and contribute to the capacity. During the discharge process, the lithium oxide coating layer can provide more lithium ion reinsertion sites, and the in-situ synthesized coating layer adheres to the surface of the material, reducing the impedance of the active lithium ion reinsertion and improving the conductivity. Therefore, the lithium-rich material synthesized by this method simultaneously improves the charge and discharge capacity and the first coulombic efficiency of the material.
[0111] Comparing with Examples 1-5, the high primary Li / Me ratio and the high primary sintering temperature can lead to excessive primary residual lithium. If the secondary coating amount is large, the coating layer will be thicker, which will affect the Li + Transmission, increase impedance, and affect the performance of material capacity.
[0112] Compared with Examples 6-7, if the precursor particle size is too large during secondary coating, it is difficult to adhere to the particle surface, the coating effect is poor, and the material performance is affected.
[0113] Comparative Examples 7-9, the Li / Me ratio is low during the secondary coating, and it is difficult to form a lithium-rich phase. Therefore, the formed coating layer provides less active lithium, and the improvement effect is not obvious. The Li / Me ratio is high during the secondary coating, and excessive lithium will form an electrochemically inactive impurity phase with the precursor. It also leads to a high level of residual lithium on the surface of the material after coating, inhibiting the capacity of the material.
[0114] In summary, in the process of preparing the lithium-rich manganese-based positive electrode material, the present invention calculates the free Li on the surface of the lithium-rich manganese-based matrix material by testing the residual alkali content on the surface of the lithium-rich manganese-based matrix material. + According to the calculation results, one or more of a lithium source and a small-particle Co source compound, a nickel-manganese compound or a nickel-cobalt-manganese compound is added again to make the Li / Me ratio at a certain value or within a certain range to form a secondary coating layer, which can effectively improve the charge and discharge capacity, the first coulomb efficiency and the electrical conductivity of the material.
[0115] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A positive electrode material, characterized in that: It comprises a lithium-rich manganese-based matrix material and a lithium oxide layer coated on the surface of the lithium-rich manganese-based matrix material, wherein the lithium oxide layer is selected from a lithium nickel manganese oxide layer, a lithium nickel cobalt manganese oxide layer or a lithium cobalt oxide layer; The general formula of the lithium nickel manganese oxide layer and the lithium nickel cobalt manganese oxide layer is Li x Ni a Co b Mn c O2, where 0.4≤x≤1.33, 0≤a≤0.8, 0≤b≤0.2, 0≤c≤1.2, x+a+b+c=2; The lithium cobalt oxide layer has the general formula Li x Co 2-x O2, where 0.4≤x≤1.
2. The positive electrode material according to claim 1, characterized in that The lithium-rich manganese-based matrix material has a general formula of Li 1+ x Ni a Co b Mn c M d O2, wherein 0≤x≤0.33, 0≤a≤0.8, 0≤b≤0.2, 0≤c≤0.6, 0≤d≤0.1, x+a+b+c+d=1, and M is selected from one or more of Al, Mg, Ti, Zr, Y, Zn, Nb, Mo, W, B, Ca, Si and La series elements.
3. The positive electrode material according to claim 1, characterized in that The average particle size of the lithium-rich manganese-based matrix material is 2 μm to 14 μm.
4. The positive electrode material according to claim 1, characterized in that The mass of the lithium oxide layer accounts for 1% to 7% of the mass of the lithium-rich manganese-based matrix material.
5. A method for preparing a positive electrode material according to any one of claims 1 to 4, characterized in that: The following steps are involved: A) calcining a mixture containing a Li source compound, a precursor and an M source compound to obtain a lithium-rich manganese-based matrix material, wherein the precursor is selected from a nickel-cobalt-manganese precursor or a nickel-manganese precursor; B) testing and calculating the residual lithium content on the surface of the lithium-rich manganese-based matrix material; C) mixing the raw material for preparing the lithium oxide layer with the lithium-rich manganese-based matrix material, and then calcining the mixture twice to obtain a lithium-rich manganese-based positive electrode material; The raw materials for preparing the lithium oxide layer include a Li source compound and a precursor, wherein the precursor is selected from at least one of a Co source compound, a nickel-manganese compound or a nickel-cobalt-manganese compound; The amount of the lithium source compound added is controlled by the residual lithium content.
6. The preparation method according to claim 5, characterized in that: In step A), the Li source compound includes at least one of lithium carbonate, lithium hydroxide monohydrate, lithium fluoride, lithium acetate, lithium oxalate, and lithium nitrate; The nickel-cobalt-manganese precursor includes at least one of nickel-cobalt-manganese hydroxide and nickel-cobalt-manganese carbonate; The nickel manganese precursor includes at least one of nickel manganese hydroxide and nickel manganese carbonate; The M source compound is selected from oxides containing M elements; The total molar amount of the metal element in the precursor and the M element in the M source compound is called the total metal molar amount. The ratio of lithium in the Li source compound to the total metal molar amount is 1.2 to 2.0, preferably 1.3 to 1.
9.
7. The preparation method according to claim 5, characterized in that: In step A), the primary calcination is carried out at a temperature of 750 to 1050° C. for a time of 6 to 40 hours.
8. The preparation method according to claim 5, characterized in that: In step C), the Li source compound is selected from at least one of lithium carbonate, lithium hydroxide monohydrate, lithium fluoride, lithium acetate, lithium oxalate, and lithium nitrate; The Co source compound is selected from Co oxide, Co hydroxide, and Co carbonate, and the particle size D50 of the Co source compound is in the range of 0.5 to 2 μm; The nickel-manganese compound is selected from one or more of nickel-manganese hydroxides and nickel-manganese carbonates; The nickel-cobalt-manganese compound is selected from one or more of nickel-cobalt-manganese hydroxides and nickel-cobalt-manganese carbonates; the particle size D50 of the nickel-manganese compound and the nickel-cobalt-manganese compound is in the range of 0.5 to 2 μm; The ratio of the total molar amount of lithium in the Li source compound and residual lithium on the surface of the lithium-rich manganese-based matrix material to the total molar amount of cobalt, nickel and manganese in the Co source compound and / or nickel manganese compound and / or nickel cobalt manganese compound is 0.1-2.0, preferably 0.8-1.
8.
9. The preparation method according to claim 5, characterized in that: The secondary sintering temperature is 350-950° C. and the time is 3-15 hours.
10. A lithium ion battery, characterized in that: The positive electrode material comprises the positive electrode material as claimed in any one of claims 1 to 4.
Citation Information
Cited By
Positive electrode material and preparation method thereof, secondary battery and electric device
CN119786570A
Composite lithium-rich manganese-based positive electrode material and preparation method and application thereof
CN120998963A
A composite lithium-rich manganese-based positive electrode material, a preparation method and application thereof
CN120998963B
Positive electrode material, preparation method thereof and lithium ion battery
CN121260749A