Positive electrode active material for lithium secondary battery, method for preparing same, and lithium secondary battery comprising same
Lithium is solved by using the superlithiated layered oxide of the chemical formula rLi2MnO3·(1-r)LiaNixCoyMnzM11-(x+y+z)O2 in a lithium secondary battery and forming an amorphous glass oxide coating on its surface Voltage attenuation and life problems in secondary batteries improve the magnification characteristics and life.
Patent Information
- Application Number
- CN202411097707.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2020-06-26
- Filing Date
- 2020-10-19
- Publication Date
- 2024-11-22
AI Technical Summary
The overlithiated layered oxides in existing lithium secondary batteries have voltage attenuation problems during their lifetime, and their rate and high-temperature life characteristics are poor, so it is necessary to improve lithium ion conductivity and suppress Mn of manganese-rich positive electrode active substances. Dissolve to extend life.
The superlithiated layered oxide of the chemical formula rLi2MnO3·(1-r)LiaNixCoyMnzM11-(x+y+z)O2 is used, and an amorphous glass oxide coating is formed on its surface to adjust the size of primary particles and dopants. The content is to improve the mobility and structural stability of lithium ions and inhibit the lattice changes of spinel-shaped to the lithosaic phase.
By reducing resistance and suppressing Mn dissolution, the rate characteristics and life of the lithium secondary battery are improved, the overpotential during charging and discharging are reduced, and the service life of the battery is extended.
Smart Images

Figure CN119008890A_ABST
Abstract
Description
[0001] This application is a divisional application of the invention patent application with the application number 202080073047.4. The filing date of the original application is October 19, 2020, and the invention title is "Positive Electrode Active Material for Lithium Secondary Battery, Method for Preparing the Same, and Lithium Secondary Battery Comprising the Same". Technical Field
[0002] The present invention relates to a positive electrode active material including an overlithiated layered oxide (OLO), and more particularly, to a positive electrode active material for a lithium secondary battery having an amorphous glass oxide coating formed on its surface, a method for preparing the same, and a lithium secondary battery including the same. Background Art
[0003] With the development of portable mobile electronic devices such as smart phones, MP3 players, and tablet personal computers (PCs), the demand for secondary batteries capable of storing electric energy has increased explosively. In particular, with the emergence of electric vehicles, medium and large-scale energy storage systems, and portable devices requiring high energy density, the demand for lithium secondary batteries is increasing day by day.
[0004] A recently spotlighted positive electrode active material is lithium nickel manganese cobalt oxide Li(Ni x Co y Mn z )O2 (in this case, x, y, and z are respectively the atomic fractions of the oxide constituent elements, 0 < x ≤ 1, 0 < y ≤ 1, 0 < z ≤ 1, and 0 < x + y + z ≤ 1). Compared with the positive electrode active material LiCoO2 that has been actively studied heretofore, this positive electrode active material has the advantages of high output capacity because it is used at a high voltage and low cost because the Co content is relatively low. However, it has the disadvantages of poor rate capability and poor life characteristics at high temperatures.
[0005] Therefore, research is being conducted on applying an overlithiated layered oxide that exhibits a higher reversible capacity than existing Li(Ni x Co y Mn z )O2 to lithium secondary batteries.
[0006] However, the phenomenon of voltage decay that occurs during the life cycle of such an overlithiated layered oxide has become a problem, which is caused by the phase transition from a spinel-like structure to a cubic structure due to the movement of transition metals during the life cycle. In order to be used for the commercialization of lithium secondary batteries, this voltage decay phenomenon of the overlithiated layered oxide must be solved.
[0007] Moreover, a solution capable of improving the electrochemical characteristics of the over-lithiated layered oxide is required. Summary of the Invention
[0008] Technical Problem
[0009] An object of the present invention is to improve the lithium-ion conductivity of a positive electrode active material containing an over-lithiated layered oxide, reduce the overpotential generated during charge and discharge by reducing the resistance, and improve the rate performance.
[0010] Moreover, an object of the present invention is to suppress the Mn dissolution of a Mn-rich positive electrode active material and suppress the lattice change from the spinel phase to the rock-salt phase starting from the surface phase during cycling to suppress voltage decay and improve the lifespan.
[0011] Technical Solution
[0012] The positive electrode active material according to an embodiment of the present invention includes an over-lithiated layered oxide represented by the following Chemical Formula 1.
[0013] Chemical Formula 1: rLi2MnO3·(1-r)Li a Ni x Co y Mn z M1 1-(x+y+z) O2
[0014] In Chemical Formula 1 above, 0 < r ≤ 0.6, 0 < a ≤ 1, 0 ≤ x ≤ 1, 0 ≤ y < 1, 0 ≤ z < 1, 0 < x + y + z ≤ 1, and M1 is one or more selected from Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Mg, Gd, Sm, Ca, Ce, Fe, Al, Ta, Mo, Sc, V, Zn, Cu, In, S, B, Ge, Si, and Bi.
[0015] The over-lithiated layered oxide may be a solid solution phase in which monoclinic-structured Li2MnO3 and rhombohedral-structured LiMO2 are mixed, and M may be one or more selected from Ni, Co, Mn, and M1.
[0016] Moreover, the over-lithiated layered oxide may have a plateau caused by Li2MnO3 in the 4.4V region of the initial charge-discharge curve. In the over-lithiated layered oxide of the embodiment of the present invention, during the initial charging process, the Li2MnO3 phase is electrochemically inactive relative to lithium up to the 4.4V region, and in the region above 4.4V, lithium may separate from the Li2MnO3 phase and oxygen may evolve.
[0017] In the overlithiated layered oxide represented by the above Chemical Formula 1, a ratio of moles of lithium to total moles of metal Ni, Co or Mn contained (Li / Ni+Co+Mn) may be 1.1 to 1.6, 1.2 to 1.6, 1.3 to 1.6 or 1.4 to 1.5.
[0018] In the chemical formula 1, the value of x may be greater than 0 and less than or equal to 0.5, greater than 0 and less than or equal to 0.4, greater than 0 and less than or equal to 0.3, greater than 0 and less than or equal to 0.2, or greater than 0 and less than or equal to 0.1.
[0019] In the chemical formula 1, the value of y may be greater than 0 and less than or equal to 0.5, greater than 0 and less than or equal to 0.4, greater than 0 and less than or equal to 0.3, greater than 0 and less than or equal to 0.2, or 0.1 to 0.2.
[0020] In the above chemical formula 1, M1 is one or more substances selected from Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Mg, Gd, Sm, Ca, Ce, Fe, Al, Ta, Mo, Sc, V, Zn, Nb, Cu, In, S, B, Ge, Si and Bi, and as an example, it can be a dopant that can be included in the above-mentioned over-lithiated layered oxide. More preferably, it can be one or more selected from Ba, Sr, B, P, Y, Zr, Nb, Mo, Ta and W that can be adjusted to grow the size of the primary particles to a more suitable range, and most preferably, it can be one or more selected from Nb and Ta.
[0021] And, the ratio of the mole number of Mn to the total mole number of Ni (Mn / Ni) may be 1 to 4.5, 1 to 4, 2 to 4.5, 2 to 4, 3 to 4.5, or 3 to 4.
[0022] The oxide of the present invention has a layered structure, which may be a layered structure in which lithium atomic layers and metal atomic layers of Ni, Co, Mn or M1 are alternately stacked via oxygen atomic layers.
[0023] The plane of the layer forming the layered structure of the above positive electrode active material may have a crystal orientation in a direction perpendicular to the C axis. In this case, the mobility of lithium ions contained in the above positive electrode active material is improved, the structural stability of the above positive electrode active material is increased, and the initial capacity characteristics, power output characteristics, resistance characteristics, and long-term life characteristics can be improved when applied to a battery.
[0024] The positive electrode active material of the present invention is an oxide rich in lithium and manganese, and an amorphous glass oxide coating is formed on the surface to inhibit Mn dissolution and inhibit the lattice change from the spinel phase to the rock salt phase starting from the surface phase during cycling to inhibit voltage decay and improve the life.
[0025] Moreover, in the present invention, an amorphous glass oxide coating is coated on the surface of the over-lithiated layered oxide particles, so the problem of non-uniformity that occurs in the case of coating in a crystalline state can be solved, and the movement of lithium ions can be further improved.
[0026] Moreover, in the present invention, an amorphous glass oxide coating is coated on the surface of the over-lithiated layered oxide particles, so the overpotential that occurs during charge and discharge in the over-lithiated layered oxide can be reduced, and the rate performance can be improved.
[0027] The above amorphous glass oxide coating may contain one or more elements selected from Si, B, P, and Ge.
[0028] Moreover, the above amorphous glass oxide coating may contain a substance represented by the following Chemical Formula 2.
[0029] Chemical Formula 2: xLi2O*(1-x)M2 a O b
[0030] Regarding the x value of the above Chemical Formula 2, it can be 0 < x ≤ 8, more preferably, it can be 0.13 ≤ x ≤ 8. Moreover, regarding the a value of the above Chemical Formula 2, it can be 0 < a ≤ 2, more preferably, it can be 1 ≤ a ≤ 2. Moreover, regarding the b value of the above Chemical Formula 2, it can be 0 < b ≤ 5, more preferably, it can be 2 ≤ b ≤ 5. And M2 can be one or more selected from Si, B, P, and Ge.
[0031] Compared with the above over-lithiated layered oxide, the content of the above amorphous glass oxide coating can be 0.05 mol% to 5 mol%, or 0.1 mol% to 3 mol%, or 0.1 mol% to 2 mol%.
[0032] The above amorphous glass oxide coating may be uniformly or non-uniformly contained on the surface of the over-lithiated layered oxide represented by the above Chemical Formula 1.
[0033] As a more preferred embodiment, the present invention coats the surface of the over-lithiated layered oxide with amorphous glass oxide, which has better diffusivity than coating with other oxides and can be evenly coated on the surface.
[0034] Furthermore, as an example, the amorphous glass oxide coating layer may be formed on the surface of the secondary particles or the primary particles.
[0035] Furthermore, as an example, in the amorphous glass oxide coating layer, an element included in the amorphous glass oxide coating layer may form a concentration gradient portion on the surface of the secondary particle or the primary particle.
[0036] In the positive electrode active material of the embodiment of the present invention, the thickness of the amorphous glass oxide coating can be 1nm to 100nm, more preferably, 10nm to 100nm. If it is thinner than the above coating, the improvement effect is minimal, and if it is thicker than the above coating, the resistance to lithium ions will increase. When the amorphous glass oxide coating meets the above range, the Mn dissolution of the manganese-rich positive electrode active material of the present invention can be suppressed, and the lattice change from the spinel type to the rock salt phase starting from the surface phase during the cycle can be suppressed to suppress voltage decay and increase life.
[0037] In the above-mentioned positive electrode active material of the embodiment of the present invention, secondary particles can be formed by aggregation of primary particles. Among the primary particles constituting the above-mentioned secondary particles, the primary particles with a size of 300nm to 10μm can be adjusted to 50 volume percent to 100 volume percent, 70 volume percent to 100 volume percent or 100 volume percent.
[0038] Furthermore, as an example, among the primary particles constituting the secondary particles, the primary particles in the positive electrode active material having a size greater than 500 nm and less than or equal to 10 μm can be adjusted to 50 volume percent to 100 volume percent, 70 volume percent to 100 volume percent or 100 volume percent.
[0039] Furthermore, as an example, in the above-mentioned positive electrode active material, the primary particles with a size of 1 μm to 10 μm can be adjusted to 50 volume percent to 100 volume percent, 70 volume percent to 100 volume percent or 100 volume percent relative to the total volume of the above-mentioned overlithiated layered oxide.
[0040] Furthermore, as an example, in the above-mentioned positive electrode active material, the primary particles having a size greater than 1 μm can be adjusted to 50 volume percent to 100 volume percent, 70 volume percent to 100 volume percent or 100 volume percent relative to the total volume of the above-mentioned overlithiated layered oxide.
[0041] Furthermore, as an example, in the above-mentioned positive electrode active material, the primary particles with a size of 2 μm or more can be adjusted to 50 volume percent to 100 volume percent, 70 volume percent to 100 volume percent or 100 volume percent relative to the total volume of the above-mentioned overlithiated layered oxide.
[0042] Furthermore, as an example, since the size of the primary particles in the positive electrode active material is adjusted, the number of primary particles in the secondary particles may be 1 to 1000, 1 to 100, 1 to 10, or 1 to 10, or may be formed by one primary particle.
[0043] The above-mentioned size of the primary particle refers to the longest length of the particle.
[0044] Furthermore, as an example, the average particle size of the primary particles of the positive electrode active material may be adjusted to be greater than 500 nm and less than or equal to 10 nm, or to be 1 μm to 10 nm.
[0045] The voltage decay phenomenon of the over-lithiated layered oxide of the present invention during the life cycle becomes a problem, which is caused by the phase transition from a spinel-like structure to a cubic structure due to the migration of transition metals during the life cycle. The present invention can improve the density of the positive electrode active material by adjusting the size of the primary particles to solve the above problem.
[0046] However, since the primary particles become larger, the diffusion distance of lithium ions increases, so the concentration polarization of lithium ions causes overpotential during charge and discharge. Ultimately, the capacity of the positive electrode active material is reduced due to reduced kinetics. However, since the ion conductivity is increased by forming an amorphous glass oxide coating, the kinetics of lithium ions are increased, so the capacity is increased and the overpotential is reduced.
[0047] The average particle size of the secondary particles of the positive electrode active material of the embodiment of the present invention may be 2 μm to 20 μm, more preferably, 10 μm to 20 μm, and more preferably, 14 μm to 16 μm. The average particle size may be defined as the particle size at which the volume accumulation is equivalent to 50% in the particle size distribution curve of the particles. The average particle size may be measured, for example, by a laser diffraction method.
[0048] The above-mentioned positive electrode active material of the embodiment of the present invention has a primary particle size in the positive electrode active material stage that is larger than the primary particle size in the precursor stage under the preparation process conditions of the following embodiments. In addition, under the preparation conditions of the following embodiments, the ratio of (the primary particle size of the positive electrode active material with the addition of a dopant that acts as a flux) / (the primary particle size of the positive electrode active material without the addition of a dopant that acts as a flux) is greater than 1, more preferably, greater than 30, and most preferably, greater than 50.
[0049] The M1 in the chemical formula 1 is a dopant that acts as a flux for the growth of the primary particles, and can be doped in the lattice structure. As an embodiment, the flux dopant can be added and mixed with the lithium compound in the sintering step and heat-treated together to increase the size of the primary particles. The role of the flux may refer to the role of a dopant that increases the size of the primary particles through the growth between the primary particles.
[0050] In the positive electrode active material of the present invention, the more the portion corresponding to the single crystal structure is, that is, the smaller the number of primary particles is, the more the voltage decay problem exhibited by the polycrystalline structure can be improved.
[0051] In the X-ray diffraction (XRD) analysis of the positive active material of the embodiment of the present invention, although the full width at half maximum (FWHM (deg.)) in I (104) can be 0.1 to 0.25 (deg.), the above value can be changed according to the manganese content. Therefore, the reduction rate of the full width at half maximum can be adjusted by the additive and adjustment content of the dopant M1, thereby solving the problems of life and voltage decay.
[0052] The present invention increases the size of primary particles in the over-lithiated layered oxide by adjusting the size, and can reduce the full width at half maximum (FWHM (deg.)) in I(104) in X-ray diffraction analysis of the case containing M1 by 5% to 50% or 5% to 40%, or 5% to 30%, 5% to 20%, 10% to 25% or 10% to 20% when sintered under the same conditions compared with the comparative example not containing M1.
[0053] The positive active material of the embodiment of the present invention may include a substance represented by the following chemical formula 3. The substance represented by the following chemical formula 3 may be a substance generated by a reaction between a dopant that functions as a flux for inducing growth between primary particles and lithium.
[0054] Chemical formula 3: Li a M3O b
[0055] In the above chemical formula 3, 0 < a ≤ 8, 0 < b ≤ 15, and M3 is one or more selected from Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Mg, Gd, Sm, Ca, Ce, Fe, Al, Ta, Mo, Sc, V, Zn, Cu, In, S, B, Ge, Si, and Bi.
[0056] Relative to the total molar amount of the metals constituting the above positive electrode active material, the content of M1 in the above chemical formula 1 can be 0.001 mol% to 10 mol%, 0.01 mol% to 5 mol%, 0.01 mol% to 3 mol%, 0.1 mol% to 2 mol%, or 0.1 mol% to 1 mol%. If the dopant M1, which is a flux for inducing the growth of primary particles, contained is greater than the above range, it will cause an excessive amount of lithium composite oxide and become a cause of decreased capacity and efficiency. If it is less than the above range, the effect of primary particle growth will be negligible.
[0057] Moreover, the volume energy density (Wh / L) of the above positive electrode active material in the embodiments of the present invention can be 2.7 Wh / L to 4.0 Wh / L.
[0058] Moreover, the volume energy density (Wh / L) of the above positive electrode active material in the embodiments of the present invention can be increased by 5% to 30% compared to the material not containing M1. The positive electrode active material of the present invention can increase the size of primary particles by adjustment in the over-lithiated layered oxide, and thus the volume energy density (Wh / L) in the case of containing M1 can be increased by 5% to 25%, 5% to 20%, 10% to 25%, or 10% to 20% compared to the comparative example not containing M1 by adjustment.
[0059] Moreover, the tap density (g / cc) of the above positive electrode active material adjusted by the addition and content adjustment of the dopant M1 can be 2.0 g / cc to 4.0 g / cc.
[0060] Moreover, the specific surface area (BET, m 2 / g) of the above positive electrode active material adjusted by the addition and content adjustment of the dopant M1 can be 0.1 m 2 / g to 1.5 m 2 / g.
[0061] The positive electrode active material of the present invention can adjust the size of primary particles in the above over-lithiated layered oxide, and thus the specific surface area (BET, m 2 / g) in the case of containing M1 can be reduced by 20% to 80% compared to the comparative example not containing M1 by adjustment.
[0062] The present invention adjusts the portion of the single crystal structure equivalent to the positive electrode active material by inducing the growth of the primary particles, and reduces the surface portion of the positive electrode active material by increasing the volume energy density and reducing the specific surface area, thereby solving the problems of life and voltage decay. In the present invention, the content of inducing the growth of the primary particles includes all the concepts of nucleation, Ostwald ripening, and particle aggregation.
[0063] The method for preparing a positive electrode active material according to an embodiment of the present invention includes a first step of preparing a positive electrode active material precursor.
[0064] The precursor may be prepared by co-precipitation, spray-drying, solid state method, wet pulverization, fluidized bed drying method, or vibration drying method, but the present invention is not limited thereto.
[0065] Next, the method includes a second step of mixing a lithium compound with the positive electrode active material precursor and firing the mixture to form a lithium composite oxide.
[0066] The second step may also be performed by mixing a compound including M1 of the chemical formula 1 and firing.
[0067] The temperature of the sintering step may be 750°C to 950°C, 800°C to 950°C, or 850°C to 950°C.
[0068] Next, a third step is included of mixing the substance formed in the second step with a coating precursor to form an amorphous glass oxide coating.
[0069] The present invention can uniformly coat the amorphous glass oxide coating on the surface of the over-lithiated layered oxide through the following steps.
[0070] In the third step, the coating precursor may be prepared by a dry mixing process.
[0071] Furthermore, in the third step, the coating precursor may be prepared by a wet mixing process. For example, the coating precursor may be dispersed or dissolved in water, alcohol or a dispersion solution and mixed with the substance formed in the second step.
[0072] The third step may include: after mixing the substance formed in the second step with the coating precursor, maintaining the mixture at a temperature of 250°C to 700°C for 7 to 12 hours and then performing furnace cooling. The temperature may vary depending on the type of coating precursor. For example, when forming a coating containing B, the temperature may be 250°C to 500°C or 250°C to 400°C, and when forming a coating containing P, the temperature may be 500°C to 700°C or 550°C to 650°C.
[0073] In the method for preparing the positive electrode active material of the embodiment of the present invention, when the coating precursor contains B or P, it can be one or more selected from B2O3, P2O5, H3BO3, NH4HPO4, NH4H2PO4, (NH4)2HPO4 or H3PO4. And, more preferably, it can be H3BO3 or NH4HPO4, but it is not particularly limited as long as it is a material that can form an amorphous glass oxide coating.
[0074] In the method for preparing the positive electrode active material of the embodiment of the present invention, after the first step and before the second step, a step of calcining the prepared precursor at a temperature of 300° C. to 600° C. may be further included.
[0075] In the method for preparing the positive electrode active material of the embodiment of the present invention, after the first step and before the second step, the steps of washing and drying the sintered material may be further included.
[0076] In the method for preparing the positive electrode active material of the embodiment of the present invention, after the second step and before the third step, the steps of washing and drying the sintered material may be further included.
[0077] The secondary battery according to the embodiment of the present invention includes the above-mentioned positive electrode active material.
[0078] The positive electrode active material is as described above, and the binder, the conductive material, and the solvent are not particularly limited as long as they can be used on the positive electrode collector of the secondary battery.
[0079] Specifically, the lithium secondary battery may include a positive electrode, a negative electrode disposed opposite to the positive electrode, and an electrolyte between the positive electrode and the negative electrode, but is not particularly limited as long as it can be used in a secondary battery.
[0080] Effects of the Invention
[0081] The present invention improves lithium ion conductivity in a super-lithiated layered oxide, reduces overpotential during charge and discharge by reducing resistance, and improves rate characteristics.
[0082] In addition, the Mn dissolution of the manganese-rich positive electrode active material is suppressed, and the lattice change from the spinel type to the rock salt phase starting from the surface phase during cycling is suppressed to suppress voltage decay and improve life. BRIEF DESCRIPTION OF THE DRAWINGS
[0083] Figure 1 The results of scanning electron microscopy (SEM) examination of the positive electrode active materials of the examples of the present invention and the comparative examples are shown.
[0084] Figure 2 The EDS test results of the positive electrode active material of the embodiment of the present invention are shown.
[0085] Figure 3 The following are the results of X-ray diffraction (XRD) analysis of the positive electrode active materials of Examples and Comparative Examples of the present invention.
[0086] Figure 4 The dispersion spectrum detection results of the positive electrode active material of the embodiment of the present invention are shown.
[0087] Figure 5 The dispersion spectrum detection results of the positive electrode active material of the embodiment of the present invention are shown.
[0088] Figure 6 The following are charge and discharge curves of Examples of the present invention and Comparative Examples.
[0089] Figure 7 Overpotential curves of Examples of the present invention and Comparative Examples are shown.
[0090] Figure 8 The rate characteristic curves of the examples of the present invention and the comparative examples are shown.
[0091] Fig. 9 The life characteristics of the examples of the present invention and comparative examples are shown.
[0092] Fig.10 The voltage holding ratios of the examples of the present invention and the comparative examples are shown. DETAILED DESCRIPTION
[0093] Hereinafter, the present invention will be described in more detail by way of examples, but the present invention is not limited to the following examples.
[0094] Expressions such as “including” and the like used in this specification should be interpreted as open-ended terms containing the possibility of including other embodiments.
[0095] The terms “preferred” and “preferably” used in this specification refer to embodiments of the present invention that can provide specified advantages under specified circumstances, rather than excluding other embodiments from the scope of the present invention.
[0096] Example 1. Preparation of positive electrode active material
[0097] synthesis
[0098] Spherical Ni was synthesized by co-precipitation method. 0.2 Co 0.1 Mn 0.7 CO3 precursor. In a 90L reactor, 25 weight percent NaCO3 and 28 weight percent NH4OH were added to a 2.5M aqueous solution of composite transition metal sulfuric acid in which NiSO4·6H2O, CoSO4·7H2O and MnSO4·H2O were mixed at a mole ratio of 20:10:70. In this case, the pH in the reactor was maintained at 8.0 to 11.0 and the temperature was maintained at 45°C to 50°C. In addition, inert gas N2 was added to the reactor to prevent the prepared precursor from being oxidized.
[0099] After the synthesis stirring was completed, the mixture was washed and dehydrated using a filter press (F / P) device. Finally, the dehydrated product was dried at 120°C for 2 days and passed through a 75μm (200 mesh) sieve to obtain Ni particles with a particle size of 4 to 20μm. 0.17 Co 0.106 Mn 0.719 CO3 precursor.
[0100] Roasting
[0101] The precursor prepared as above is kept in an O2 or air (Air) (50L / min) atmosphere in a box-type calcining furnace, the temperature is increased at a rate of 2°C per minute and maintained at 550°C for 1 to 6 hours, and then the furnace is cooled.
[0102] Firing
[0103] LiOH or Li2CO3 was weighed so that the Li / (Ni+Co+Mn) ratio of the calcined precursor was 1.45, and 0.6 mol% of Nb2O5 was weighed as a flux dopant, and mixed using a manual mixer (MM).
[0104] The mixture is kept in an atmosphere of O2 or air (50L / min) in a box-type calcining furnace, the temperature is increased at a rate of 2°C per minute, and after being kept at a sintering temperature of 900°C for 7 to 12 hours, the furnace is cooled to prepare the positive electrode active material.
[0105] The composition of the positive electrode active material prepared in Example 1 is Li:Ni:Co:Mn:Nb=15.3:15.1:9.3:59.8:0.4 (weight percentage).
[0106] Coating
[0107] 1.5 mol% of H3BO3 was weighed as a surface treatment dopant and mixed using a hand mixer.
[0108] The mixture is kept in an atmosphere of O2 or air (50 L / min) in a box-type calcining furnace, the temperature is increased at a rate of 4.4°C per minute, and after being kept at a sintering temperature of 300°C for 7 to 12 hours, the furnace is cooled to prepare the positive electrode active material.
[0109] Example 2. Preparation of positive electrode active material
[0110] In the coating step of the above-mentioned Example 1, 0.5 mol % of NH4HPO4 was weighed as a surface treatment dopant, and the positive electrode active material was prepared in the same manner as in the above-mentioned Example 1 except that the sintering temperature in the coating step was 600°C.
[0111] The composition of the positive electrode active material prepared in Example 2 is Li:Ni:Co:Mn:Nb=15.0:14.8:9.3:60.0:0.8 (weight percentage).
[0112] Comparative Example 1. Preparation of positive electrode active material
[0113] A positive electrode active material was prepared in the same manner as in Example 1, except that the flux dopant was not mixed and the coating step was not performed.
[0114] Comparative Example 2. Preparation of positive electrode active material
[0115] A positive electrode active material was prepared in the same manner as in Example 1, except that the coating step was not performed.
[0116] Comparative Example 3. Preparation of positive electrode active material
[0117] A positive electrode active material was prepared in the same manner as in Example 1 except that the flux dopant was not mixed.
[0118] Preparation Example. Preparation of lithium secondary battery
[0119] 90 weight percent of the positive electrode active material of the above-mentioned embodiment and comparative example, 5.5 weight percent of carbon black, and 4.5 weight percent of polyvinylidene fluoride (PVDF) binder were dispersed in 30g of N-methyl-2-pyrrolidone (NMP) to prepare positive electrode slurry. The above positive electrode slurry was applied to a 15μm thick aluminum (Al) film as a positive electrode collector and dried, and then roll pressed to prepare a positive electrode. The filling amount of the positive electrode was 5.5mg / cm 2, the electrode density is 2.3g / cm 3 .
[0120] With respect to the above-mentioned positive electrode, metallic lithium was used as a counter electrode, 1M LiPF6 was used as an electrolyte, and ethylene carbonate / dimethyl carbonate (EC / DMC)=1 / 1 (v / v).
[0121] A separator formed of a porous polyethylene (PE) film was interposed between the positive electrode and the negative electrode to form a battery assembly, and the electrolyte was injected to prepare a lithium secondary battery (button battery).
[0122] Experimental example
[0123] Reference Figure 1 When comparing Comparative Example 2 with Examples 1 and 2, it can be confirmed that the size and shape of the primary particles coated with B and P do not change. When comparing Comparative Example 1 with Comparative Example 3, it can be confirmed that there is no particle growth through the amorphous glass oxide coating.
[0124] Reference Figure 2 It can be confirmed that not only the Ni, Co, and Mn elements, but also the flux dopant Nb that induces particle growth is uniformly distributed within the particles.
[0125] Figure 3 The X-ray diffraction analysis was wavelength. Figure 3 , when Nb is added as a flux dopant, the (003) peak shifts, which can be confirmed as evidence that Nb as a flux dopant is doped into the over-lithiated layered oxide lattice.
[0126] Reference Figure 4 It can be confirmed that the coating layer containing B is evenly distributed on the surface of the positive electrode active material of Example 1.
[0127] Reference Figure 5 It can be confirmed that the coating layer containing P is evenly distributed on the surface of the positive electrode active material of Example 2.
[0128] Reference Figure 6 , compared to Comparative Example 1, in the case of Comparative Example 2, the capacity decreases slightly as the primary particles become larger. This is due to the increase in the diffusion distance of lithium ions, resulting in a decrease in kinetics. However, in the case of the embodiment in which the amorphous glass oxide coating is formed, it can be confirmed that the capacity is increased by increasing the kinetics of lithium ions by increasing the ion conductivity.
[0129] Reference Figure 7Since the primary particle size increases the diffusion distance of lithium ions, there is a problem of overpotential caused by concentration polarization of lithium ions. However, in the case of the embodiment in which the amorphous glass oxide coating is formed, it can be confirmed that the overpotential is reduced by increasing the kinetics of lithium ions.
[0130] Reference Figure 8 It can be confirmed that the rate characteristics of the embodiment are improved by about 10% or more compared to the comparative example. This is because the resistance is reduced by the amorphous glass oxide coating.
[0131] Reference Fig. 9 Compared with Comparative Example 1, it can be confirmed that the life characteristics of Comparative Example 3 in which an amorphous glass oxide coating is formed are improved by about 10% or more. Moreover, in the case of Examples 1 and 2 in which particles are grown and an amorphous glass oxide coating is formed, the capacity retention rate based on the cycle is more than 80%. This is because the amorphous glass oxide coating reduces the resistance, inhibits the dissolution of Mn, and inhibits the phase transition from the spinel type to the rock salt phase starting from the surface phase during the cycle to improve the life.
[0132] Reference Fig.10 In the case of the example, a voltage retention ratio of 97% was shown. This is because the phase transition of the over-lithiated layered oxide that occurs during cycling due to the amorphous glass oxide coating is suppressed.
[0133] The above experimental results are shown in Table 1 below.
[0134] Table 1
[0135]
Claims
1. A positive electrode active material for a secondary battery, characterized in that: Comprising: Over-lithiated layered oxide, represented by Chemical Formula 1 below; and An amorphous glass oxide coating located on the surface of the over-lithiated layered oxide represented by the above Chemical Formula 1, Chemical formula 1: rLi2MnO3·(1-r)Li a Ni x Co y Mn z M1 1-(x+y+z) O2 In the above Chemical Formula 1, 0 < r ≤ 0.6, 0 < a ≤ 1, 0 ≤ x ≤ 1, 0 ≤ y < 1, 0 ≤ z < 1, 0 < x + y + z ≤ 1, the above M1 is one or more selected from Na, K, Mg, Al, Fe, Cr, Y, Sn, Ti, B, P, Zr, Ru, Nb, W, Ba, Sr, La, Ga, Gd, Sm, Ca, Ce, Ta, Mo, Sc, V, Zn, Cu, In, S, Ge, Si, and Bi, Wherein, secondary particles are formed by aggregation of primary particles, and among the primary particles constituting the above secondary particles, the primary particles with a size greater than 500 nm to not greater than 10 μm are adjusted to 50 volume percentages to 100 volume percentages.
2. The positive electrode active material for secondary battery according to claim 1, characterized in that The above amorphous glass oxide coating contains one or more selected from Si, B, P, and Ge.
3. The positive electrode active material for a secondary battery according to claim 1, characterized in that The above amorphous glass oxide coating contains a substance represented by Chemical Formula 2 below: Chemical formula 2: xLi2O*(1-x)M2 a O b In the above Chemical Formula 2, 0 < x ≤ 0.8, 0 < a ≤ 2, 0 < b ≤ 5, M2 is one or more selected from Si, B, P, and Ge.
4. The positive electrode active material for a secondary battery according to claim 1, characterized in that Relative to the above over-lithiated layered oxide, it contains 0.05 mole percentage to 5 mole percentage of the above amorphous glass oxide coating.
5. The positive electrode active material for secondary battery according to claim 1, characterized in that The thickness of the above amorphous glass oxide coating is 1 nm to 100 nm.
6. The positive electrode active material for secondary battery according to claim 1, characterized in that The above M1 in Chemical Formula 1 is a dopant that acts as a flux for the growth of the above primary particles.
7. The positive electrode active material for a secondary battery according to claim 1, characterized in that: The above M1 in Chemical Formula 1 is one or more selected from Ba, Sr, B, P, Y, Zr, Nb, Mo, Ta, and W.
8. The positive electrode active material for secondary battery according to claim 1, characterized in that Relative to the total molar number of metals in the above over-lithiated layered oxide, it contains 0.001 mole percentage to 10 mole percentage of the above M1 in Chemical Formula 1.
9. The positive electrode active material for a secondary battery according to claim 1, characterized in that In the over-lithiated layered oxide represented by the above Chemical Formula 1, the ratio of the molar number of lithium to the total molar number of the contained metals Ni, Co, or Mn, i.e., Li / Ni + Co + Mn, is 1.1 to 1.
6.
10. The positive electrode active material for a secondary battery according to claim 1, characterized in that In the over-lithiated layered oxide represented by the above Chemical Formula 1, the ratio of the molar number of Mn to the total molar number of Ni, i.e., Mn / Ni, is 1 to 4.
5.
11. A method for preparing a positive electrode active material for a secondary battery according to claim 1, characterized in that: Including: The first step of preparing a precursor of the positive electrode active material; The second step of mixing a lithium compound with the above precursor of the positive electrode active material and firing to form a lithium composite oxide; And The third step of mixing the substance formed in the second step with a coating precursor to form an amorphous glass oxide coating.
12. The method for preparing a positive electrode active material for a secondary battery according to claim 11, characterized in that: In the above second step, a compound containing M1 of the above Chemical Formula 1 is also mixed and fired.
13. The method for preparing a positive electrode active material for a secondary battery according to claim 11, characterized in that: The above third step includes: after mixing the substance formed in the second step with the coating precursor, holding at a temperature of 250 °C to 700 °C for 7 hours to 12 hours and then performing furnace cooling.
14. The method for preparing a positive electrode active material for a secondary battery according to claim 13, characterized in that: The above coating precursor contains one or more selected from B2O3, P2O5, H3BO3, NH4HPO4, NH4H2PO4, (NH4)2HPO4, or H3PO4.
15. The method for preparing a positive electrode active material for a secondary battery according to claim 11, characterized in that: After the first step and before the second step, the method further includes calcining the prepared precursor at a temperature of 300° C. to 600° C.
16. The method for preparing a positive electrode active material for a secondary battery according to claim 11, characterized in that: After the first step and before the second step, the method further includes washing the calcined material with water.
17. The method for preparing a positive electrode active material for a secondary battery according to claim 11, characterized in that: After the second step and before the third step, the method further includes washing the calcined material with water.
18. A secondary battery, characterized in that: Contains the positive electrode active material according to claim 1.