SnO2GN composite carrier supported PtMo alloy catalyst as well as preparation method and application thereof

By using the PtMo alloy catalyst supported by the SnO2GN composite support in a direct ethanol fuel cell, the problem of poisoning of Pt-based catalysts in the ethanol electrooxidation reaction is solved, the efficiency and stability of the catalyst are improved, and more efficient ethanol electrooxidation is achieved.

CN119008989AActive Publication Date: 2024-11-22BEIJING INSTITUTE OF PETROCHEMICAL TECHNOLOGY
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411127310.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-22
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

Pt-based catalysts are susceptible to toxicity by intermediate products such as CO during ethanol electrooxidation reaction, resulting in a degradation of catalytic performance and affecting the efficiency and stability of direct ethanol fuel cells.

Method used

The SnO2GN composite support was used to support the PtMo alloy catalyst, and the SnO2GN composite support was prepared by the sol-gel method, and the PtMo alloy was supported on it by microwave reduction method to form a PtMo/SnO2GN catalyst, which optimized the structure and performance of the catalyst.

Benefits of technology

It improves the anti-toxicity and cycle stability of the catalyst, enhances the efficiency of the electrooxidation reaction of ethanol, generates more CO2 instead of intermediate products, and improves the utilization efficiency and stability of the catalyst.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119008989A_ABST
    Figure CN119008989A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of electrochemical catalysis, in particular to a SnO2GN composite carrier supported PtMo alloy catalyst as well as a preparation method and application thereof. According to the specific technical scheme, according to the preparation method of the SnO2GN composite carrier supported PtMo alloy catalyst, the SnO2GN composite carrier jointly composed of SnO2 and graphene serves as a catalyst carrier, PtMo alloy serves as an active component, the PtMo alloy is supported on the SnO2GN composite carrier, and the PtMo / SnO2GN catalyst is obtained. According to the invention, the problems of low ethanol electrooxidation catalytic efficiency and easy attenuation in the reaction process of a Pt-based catalyst in practical application are solved; the prepared catalyst has more active sites in the ethanol electrooxidation process, so that the ethanol electrooxidation catalytic effect is enhanced, the poisoning resistance of the catalyst is remarkably improved, the influence of poisoning intermediates in the reaction process is reduced, the service life of the catalyst is prolonged, and the cycle stability of the catalyst is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of electrochemical catalysis, and in particular to a SnO 2 GN composite carrier supported PtMo alloy catalyst and its preparation method and application. Background Art

[0002] Direct ethanol fuel cell (DEFC) is a clean energy device that uses ethanol as fuel and converts chemical energy into electrical energy through electrochemical reactions. Due to the advantages of ethanol such as high energy density, wide sources, easy storage and transportation, and safe use, DEFC has great potential in replacing traditional fossil fuels and reducing greenhouse gas emissions. However, the commercial application of DEFC still faces many challenges, especially in terms of the efficiency and stability of ethanol electrooxidation catalysts. The ideal ethanol electrooxidation catalyst should not only be able to efficiently and completely oxidize ethanol to produce CO 2 It must also be resistant to poisoning to cope with the poisoning effects of intermediates (such as CO) generated during the reaction. The accumulation of these intermediates will significantly reduce the activity of the catalyst, thereby affecting the overall performance of the battery.

[0003] At present, Pt-based catalysts are widely used in the research of ethanol electro-oxidation catalysts, but single Pt catalysts are easily poisoned by intermediate products such as CO during long-term use, resulting in a rapid decline in catalytic performance. Therefore, research and development of catalysts with high efficiency, stability and strong anti-poisoning ability is the key to improving DEFC performance. In order to obtain highly efficient and stable ethanol electro-oxidation catalysts, researchers have developed composite catalysts, which are formed by introducing a second metal or metal oxide as a co-catalyst of Pt to improve the anti-poisoning ability and cycle stability of ethanol electro-oxidation catalysts. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides a SnO 2 The GN composite carrier-supported PtMo alloy catalyst and its preparation method and application solve the problems faced by Pt-based catalysts in practical applications, namely, low catalytic efficiency of ethanol electro-oxidation and easy attenuation during the reaction process.

[0005] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0006] The invention discloses a SnO 2 Preparation method of PtMo alloy catalyst supported by GN composite carrier, using SnO 2 SnO and graphene 2 The GN composite carrier is the catalyst carrier, and the PtMo alloy is used as the active component. 2GN composite support, PtMo / SnO 2 GN Catalyst.

[0007] Preferably, the PtMo / SnO 2 The total mass fraction of the PtMo alloy in the GN catalyst is 3-10%, the atomic ratio of Pt to Mo in the PtMo alloy is 1:1-1:5, and the SnO 2 The mass loading ratio is 5 to 20%.

[0008] Preferably, the SnO 2 The preparation process of the GN composite carrier is as follows: using ammonia water as a precipitant, a soluble tin source and graphene as raw materials to prepare the composite carrier by a sol-gel method; the concentration of the ammonia water is 0.4-0.6 mol / L, the concentration of the tin source is 0.1 mol / L; the tin source is tin tetrachloride, and the graphene is precipitated by nitric acid or sulfuric acid vapor and H 2 O 2 Graphene after oxidation treatment.

[0009] Preferably, the oxidation treatment process of the graphene is: heating concentrated nitric acid or concentrated sulfuric acid to generate acid vapor, continuously heating the graphene in the concentrated acid vapor environment for acid treatment, and after stopping the treatment, continuing to maintain the temperature of the graphene to dry the graphene treated with acid vapor, washing it until the pH value of the filtrate is 7; then transferring it to H 2 O 2 The solution is heated and ultrasonicated for 1 to 3 hours, then washed with deionized water, dried in a vacuum drying oven for 8 to 12 hours, and ground for 10 to 20 minutes to obtain oxidized graphene.

[0010] Preferably, the concentrated nitric acid or concentrated sulfuric acid and the graphene are heated separately, the heating temperature of the concentrated nitric acid or concentrated sulfuric acid is 130-150°C, the graphene is continuously heated at a temperature of 110-130°C in a concentrated acid vapor environment, and the heating time is 7-9h. After the concentrated acid heating is stopped, the temperature of the graphene is continued to be maintained to dry the graphene treated with acid vapor, and the temperature is maintained at 110-130°C for 24h.

[0011] Preferably, the H 2 O 2 The concentration of the solution is 3-30%, the heat treatment temperature is 60° C., and the time is 10 minutes; after the heat treatment, the substrate is washed with deionized water for at least 3 times.

[0012] Preferably, the PtMo alloy is supported on SnO 2 The process on the GN composite carrier is: ethylene glycol is used as a reducing agent, and a soluble platinum source and a molybdenum source are used as raw materials to prepare the GN composite carrier by a microwave reduction method; the platinum source is chloroplatinic acid, and the molybdenum source is ammonium molybdate.

[0013] Preferably, 0.1-0.2 mol / L chloroplatinic acid ethylene glycol solution and 0.1-0.2 mol / L ammonium molybdate ethylene glycol solution are mixed and stirred for 30 min, and then SnO is added. 2 GN composite carrier, ultrasonically and stirred for 30 minutes each to form a uniform solution, and added 3-5wt.% NaOH / EG to adjust the pH value to 9-10 to obtain a precursor solution; the precursor solution was heated to 160-180°C in a microwave reactor at a power of 450-550W and maintained for 90 seconds; after standing and cooling, a 3-5wt.% dilute nitric acid aqueous solution was used to adjust the pH value to 5-7, and stirred for 30 minutes; washed until the filtrate was neutral, vacuum dried, and treated with plasma in an Ar environment for 5-15 minutes to obtain PtMo / SnO 2 GN Catalyst.

[0014] Accordingly, a nO 2 GN composite carrier supports PtMo alloy catalyst, the PtMo / SnO 2 The total mass fraction of the PtMo alloy in the GN catalyst is 3-10%, the atomic ratio of Pt to Mo in the PtMo alloy is 1:1-1:5, and the SnO 2 The mass loading ratio is 5 to 20%.

[0015] Accordingly, a SnO 2 Application of GN composite carrier-supported PtMo alloy catalyst in catalyzing ethanol electrooxidation reaction in direct ethanol fuel cells.

[0016] The present invention has the following beneficial effects:

[0017] 1. In the process of GN (graphene) oxidation treatment, the present invention first uses concentrated nitric acid or sulfuric acid for high-temperature oxidation, and then uses hydrogen peroxide to treat it, which can not only achieve the purpose of oxidizing and removing carbon debris in GN and on the surface of GN, but also introduce -NO, -NO 2 and -OH groups, and the subsequent formation of SnO 2 Precursor colloid coordination is beneficial to SnO 2 Uniform distribution on the GN surface.

[0018] 2. The present invention is SnO 2 The GN composite carrier is synthesized by loading the gel precipitate onto the oxidized graphene through the sol-gel method and then subjected to rotary evaporation and vacuum calcination to obtain SnO 2 The composite carrier SnO is evenly distributed on GN. 2GN exhibits good hydrophilicity and excellent electrical conductivity, providing a good dispersion platform for PtMo alloy nanoparticles to be loaded on the carrier. 2 The distribution on GN is very uniform, so the utilization efficiency of the catalyst is higher and the current density obtained by ethanol oxidation is larger.

[0019] 3. PtMo / SnO provided by the present invention 2 The GN composite catalyst uses transition metal Mo as a promoter of Pt. Mo in the alloy can change the electronic structure of Pt and reduce the adsorption energy of intermediate products such as CO. 2 The oxygen vacancies generated by the precursor during vacuum calcination can adsorb oxygen-containing species, which can increase the oxidation rate of intermediates such as CO. Mo is also beneficial to the breakage of CC bonds during ethanol oxidation. Therefore, PtMo alloy can effectively promote the complete oxidation of ethanol and generate more CO. 2 , rather than intermediates, improving the catalytic efficiency and catalytic stability. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 is Pt in Example 1 1 Mo 3 / SnO 2 XRD patterns of GN and Pt / GN catalysts;

[0021] Figure 2 The SnO in Example 1 has an atomic ratio of 1:3 for PtMo. 2 Transmission electron microscopy image of PtMo alloy catalyst supported on GN composite carrier;

[0022] Figure 3 SnO with different PtMo atomic ratios in Example 1 2 Comparison of the chronoamperometric stability of PtMo alloy catalysts supported on GN composite carriers. DETAILED DESCRIPTION

[0023] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art.

[0025] 1. SnO disclosed in the present invention 2The PtMo alloy catalyst supported by the GN composite carrier is based on SnO 2 SnO and graphene 2 The GN composite carrier is a catalyst carrier, and the PtMo alloy is used as an active component. Mo is used as a promoter of Pt to form an alloy with Pt. The PtMo alloy is supported on the composite carrier SnO 2 On GN, PtMo / SnO 2 GN catalyst. Wherein, the PtMo / SnO 2 The total mass fraction of the PtMo alloy in the GN catalyst is 3-10%, the atomic ratio of Pt to Mo in the PtMo alloy is 1:1-1:5, and the SnO 2 The mass loading ratio is 5 to 20%.

[0026] Wherein, the SnO 2 The GN composite carrier is prepared by using ammonia water as a precipitant, a soluble tin source and graphene as raw materials, adopting a sol-gel method and calcining in a vacuum tube furnace. The tin source is tin tetrachloride, and the graphene is oxidized graphene.

[0027] The PtMo alloy is supported on SnO 2 The GN composite carrier is reduced by microwave using ethylene glycol as a reducing agent and soluble platinum source and molybdenum source as raw materials. The platinum source is chloroplatinic acid and the molybdenum source is ammonium molybdate.

[0028] 2.SnO 2 The specific preparation steps of the GN composite carrier-supported PtMo alloy catalyst are as follows:

[0029] S1. Oxidation treatment of graphene: Concentrated nitric acid or concentrated sulfuric acid is heated to generate acid vapor, and graphene is continuously heated in a concentrated acid vapor environment for acid treatment. After the treatment is stopped, the temperature of the graphene is continued to dry the graphene treated with acid vapor, and then the graphene is washed with deionized water until the pH value of the filtrate is 7, and then transferred to H 2 O 2 The solution is heated, ultrasonicated for 1 to 3 hours, and then washed with deionized water, dried in a vacuum drying oven for 8 to 12 hours, and ground for 10 to 20 minutes to obtain oxidized graphene;

[0030] The concentrated nitric acid or concentrated sulfuric acid and graphene are heated separately. The heating temperature of the concentrated nitric acid or concentrated sulfuric acid is 130-150°C. The graphene is continuously heated at 110-130°C in the concentrated acid vapor environment for 7-9 hours. After the concentrated acid heating is stopped, the temperature of the graphene is continued to be maintained to dry the graphene treated with acid vapor. The temperature is maintained at 110-130°C for 24 hours. 2 O 2Heat treatment in solution, H 2 O 2 The concentration is 3-30%, the heat treatment temperature is 60°C, and the time is 10 minutes. After the heat treatment, wash with deionized water for at least 3 times.

[0031] S2.SnO 2 Preparation of GN composite carrier: 0.4-0.6 mol / L NH 4 OH solution was added dropwise to 0.1 mol / L SnCl 4 The aqueous solution was stirred continuously until no sol was produced, aged for 3 to 5 hours, centrifuged, and washed with water three times, and then the produced gel-like substance was added to the graphene suspension aqueous solution after oxidation treatment in S1 and stirred for 5 to 7 hours, and then allowed to stand for 24 hours, and the mixed solution was subjected to rotary evaporation at 80°C for 1 to 3 hours, and the sample after rotary evaporation was placed in a vacuum tube furnace at 550°C for 2 to 3 hours to obtain SnO 2 GN composite carrier;

[0032] S3. Preparation of precursor solution: Mix 0.1-0.2 mol / L chloroplatinic acid ethylene glycol solution and 0.1-0.2 mol / L ammonium molybdate ethylene glycol solution and stir for 30 min, then add SnO 2 The GN composite carrier was ultrasonicated and stirred for 30 min each to form a uniform solution, and 3-5 wt.% NaOH / EG was added to adjust the pH value to 9-10;

[0033] Wherein, chloroplatinic acid ethylene glycol solution and ammonium molybdate ethylene glycol solution of equal concentration are mixed and stirred, wherein the atomic ratio of Pt to Mo is 1:1 to 1:5.

[0034] S4. Microwave reduction: The precursor solution adjusted in pH value in S3 was transferred to a three-necked flask, and heated to 160-180°C at a power of 450-550W in a microwave reactor for 90s; after standing and cooling, the pH value was adjusted to 5-7 with a 3-5wt.% dilute nitric acid aqueous solution, and stirred for 30min;

[0035] S5. Drying-plasma treatment: Filter and wash the solution stirred in S4 with deionized water until the filtrate is neutral. Dry the collected powder in a vacuum oven at 80°C for 8-12 hours and then treat it with plasma in an Ar environment for 5-15 minutes at a discharge power of 200W to obtain PtMo / SnO 2 GN catalyst, namely SnO 2 GN composite carrier supported PtMo alloy catalyst.

[0036] 3. The SnO prepared by the present invention 2Application of PtMo alloy catalyst supported on GN composite carrier for electrocatalytic oxidation of ethanol in direct ethanol fuel cells.

[0037] Example 1

[0038] This embodiment provides five SnO with different PtMo ratios (Pt and Mo atomic ratios are 1:1, 1:2, 1:3, 1:4, and 1:5, respectively). 2 SnO with a content of 20% 2 The preparation method of the GN composite carrier-supported PtMo alloy catalyst comprises the following steps:

[0039] (1) Oxidation treatment of graphene: 200 mL of concentrated nitric acid was placed in a three-necked flask, 2 g of graphene was placed in a quartz tube with a sand core wrapped in an electric heating jacket, and the quartz tube was inserted into the right neck of the three-necked flask. The three-necked flask was heated to 140°C in an oil bath to generate acid vapor from the concentrated nitric acid. The electric heating jacket was maintained at 120°C to maintain the temperature of the graphene in the concentrated nitric acid vapor environment for 8 hours. After stopping the concentrated nitric acid heating, the temperature of the electric heating jacket was continued to be maintained to dry the graphene treated with acid vapor. The temperature was maintained at 120°C for 24 hours.

[0040] The graphene was then washed with deionized water until the pH value of the filtrate was 7, and the washed graphene was transferred to a 30% H 2 O 2 The solution was heat treated at 60° C. for 10 min, ultrasonicated for 2 h, washed with deionized water three times, dried in a vacuum drying oven for 12 h, and ground for 20 min to obtain oxidized graphene.

[0041] (2) SnO 2 Preparation of GN composite carrier: 0.5 mol / L NH 4 OH solution was added dropwise to 0.1 mol / L SnCl 4 The aqueous solution was stirred continuously until no precipitation was generated, aged for 4 hours, centrifuged, and washed with water three times; the resulting gel-like substance was then added to the graphene (100 mg) suspension aqueous solution after acid treatment (step (1)) and stirred for 6 hours, then allowed to stand for 24 hours, the mixed solution was subjected to rotary evaporation at 80°C for 1 hour, and the sample after rotary evaporation was placed in a vacuum tube furnace and calcined at 550°C for 2 hours to obtain SnO 2 GN composite carrier.

[0042] (3) Preparation of precursor solution: 0.1 mol / L chloroplatinic acid ethylene glycol solution and 0.1 mol / L ammonium molybdate ethylene glycol solution were mixed and stirred in five beakers at PtMo atomic ratios of 1:1, 1:2, 1:3, 1:4, and 1:5 for 30 min, and then SnO 2The GN composite carrier was ultrasonicated and stirred for 30 min each to form a uniform solution, and 5 wt.% NaOH / EG was added to adjust the pH value to 10, thereby obtaining five precursor solutions.

[0043] (4) Microwave reduction: The five precursor solutions with adjusted pH values ​​were transferred to five three-necked flasks respectively, and heated to 170°C for 90 seconds at a power of 450 W in a microwave reactor. After cooling, the pH value was adjusted to 5 with a 5 wt.% dilute nitric acid aqueous solution and stirred for 30 minutes.

[0044] (5) Drying-plasma treatment: The five solutions stirred in step (4) were filtered and washed with deionized water until the filtrate was neutral. The collected wet samples were dried in a vacuum oven at 80 °C for 12 h and then treated with plasma (200 W) in an Ar environment for 10 min to obtain five PtMo / SnO with different PtMo ratios. 2 GN catalyst, namely SnO 2 GN composite carrier supported PtMo alloy catalyst, denoted as Pt 1 Mo 1 / SnO 2 GN, Pt 1 Mo 2 / SnO 2 GN, Pt 1 Mo 3 / SnO 2 GN, Pt 1 Mo 4 / SnO 2 GN, Pt 1 Mo 1 / SnO 2 G.N.

[0045] X-ray powder diffractometer was used to characterize the PtMo / SnO 2 GN and Pt / GN are used for detection. The diffraction peaks at different positions and the shift of the diffraction peaks can be used to determine the SnO 2 Whether GN composite support and PtMo alloy are formed.

[0046] In Example 1, the atomic ratio of PtMo is 1:3, which is PtMo / SnO 2 The X-ray diffraction spectra of GN and Pt / GN are shown in Figure 1 As shown. Figure 1 It can be seen that both catalysts show characteristic diffraction peaks of the face-centered structure of Pt, and significant diffraction peaks appear at positions of about 33.8° and 51.7°, which are attributed to SnO 2 The diffraction peak at 26° can be attributed to the diffraction peak of graphite carbon, confirming that SnO2 The GN composite support was successfully formed; when the Mo element was introduced, the characteristic diffraction peak of Pt shifted negatively, indicating that a PtMo alloy was generated.

[0047] In Example 1, the atomic ratio of PtMo is 1:3 SnO 2 Transmission electron microscopy image of PtMo alloy catalyst supported on GN composite carrier Figure 2 As shown. Figure 2 It can be seen that the SnO 2 In the PtMo alloy catalyst supported on the GN composite carrier, graphene is a thin layer structure, and is stacked on each other to form a wrinkled appearance, without obvious agglomerates, and many fine nanoparticles are evenly distributed, indicating that the PtMo alloy is uniformly reduced and loaded on the SnO 2 The GN composite carrier has good dispersibility and provides more active sites.

[0048] Example 2

[0049] The five SnO 2 The electrochemical performance of the PtMo alloy catalyst supported on the GN composite carrier as an anode ethanol electro-oxidation catalyst for direct ethanol fuel cells was evaluated and tested, including:

[0050] Five types of SnO 2 The performance evaluation of the PtMo alloy catalyst loaded on the GN composite carrier was carried out by preparing it into an electrode and forming a three-electrode test system for quantitative analysis on an electrochemical workstation (CHI660E, Shanghai Chenhua Instrument Co., Ltd.).

[0051] 1. Preparation of working electrode

[0052] Take 1 mg of the prepared SnO 2 The GN composite carrier loaded with PtMo alloy catalyst was mixed with 51 μL nafion solution (nafion:EG=2:8) and 102 μL deionized water to prepare electrode slurry, which was ultrasonically oscillated for 30 min. Then, 15 μL of the ultrasonically treated slurry was measured and evenly applied on the working electrode. The working electrode was then placed in an oven for drying and used as the working electrode after drying.

[0053] 2. Cyclic voltammetry test

[0054] The dried working electrode, reference electrode and counter electrode were used to form a three-electrode test system. Nitrogen was introduced for 20 minutes before the test to achieve saturation. 2 SO 4 Cyclic voltammetry was performed in an electrolyte solution of 0.5 mol / L H2 SO 4 +0.5mol / LC 2 H 5 Cyclic voltammetry was performed in an electrolyte solution containing OH, using the peak current density (I f ) and the peak current density of the negative scan (I b ) was used to evaluate the ethanol electrooxidation activity of the catalyst, and its ratio (I f / I b ) was used to evaluate the accumulation of residual intermediates during the oxidation process.

[0055] In this embodiment, the test was performed using a CHI660E electrochemical workstation produced by Shanghai Chenhua. The reference electrode was a saturated calomel electrode, the counter electrode was a platinum electrode, the potential range was -0.2 to 1 V, and the test temperature was 25°C.

[0056] 3. Chrono current test

[0057] Chronoamperometry is a potential-controlled analytical method that measures the current that changes with time at a certain potential. After the cyclic voltammetry test, the catalyst is continued to be heated at 0.5 mol / L H 2 SO 4 +0.5mol / LC 2 H 5 In the electrolyte solution of OH, a certain voltage was applied and a chronoamperometric test was carried out for 3600s to evaluate the stability of the catalyst for the electro-oxidation reaction of ethanol. The test voltage was 0.5V.

[0058] 4. CO dissolution test

[0059] CO is considered to be the main poison in the ethanol oxidation process. In order to evaluate the catalyst's ability to resist CO poisoning, a CO dissolution test is performed. This test completes the complete oxidation of CO on the catalyst through two consecutive cyclic voltammetric scans.

[0060] The specific implementation steps are: nitrogen gas with a concentration of 0.5 mol / LH 2 SO 4 The electrode was placed in an electrolyte solution for 20 minutes to remove dissolved oxygen; CO gas was then introduced into the solution for 15 minutes to saturate the solution with CO; nitrogen was finally introduced into the solution for 20 minutes to remove the remaining CO gas in the solution, thereby forming a monolayer of CO on the electrode surface. After the ventilation was completed, a CO dissolution test was performed with a potential range of -0.2 to 1 V and a test temperature of 25°C.

[0061] The five SnO 2The electrochemical performance data of the PtMo alloy catalyst supported on the GN composite carrier (Pt:Mo atomic ratios are 1:1, 1:2, 1:3, 1:4, and 1:5, respectively) in the ethanol electrooxidation reaction are shown in Table 1. The 0.5 V chronoamperometric stability data are shown in Table 1. Figure 3 shown.

[0062] Table 1 SnO 2 Electrochemical Performance of PtMo Alloy Catalyst Supported on GN Composite Support

[0063] catalyst <![CDATA[ECSA(m 2 ·g -1 Pt )]]> <![CDATA[I f (mA·mg -1 Pt )]]> <![CDATA[I b (mA·mg -1 Pt )]]> <![CDATA[I f / I b ]]> CO oxidation peak potential (V) <![CDATA[Pt 1 Mo 1 / SnO 2 GN]]> 54.7 1388.9 1147.9 1.21 0.70 <![CDATA[Pt 1 Mo 2 / SnO 2 GN]]> 80.2 1643.6 1192.1 1.38 0.66 <![CDATA[Pt 1 Mo 3 / SnO 2 GN]]> 129.3 1898.7 1293.8 1.47 0.62 <![CDATA[Pt 1 Mo 4 / SnO 2 GN]]> 105.8 1593.2 1271.2 1.25 0.69 <![CDATA[Pt 1 Mo 5 / SnO 2 GN]]> 94.4 1439.4 1189.5 1.21 0.71

[0064] As shown in Table 1, with the increase of Mo atomic weight, SnO 2 The electrochemically active surface area and positive scan peak current density of the PtMo alloy catalyst supported on the GN composite carrier first increased and then decreased. When the PtMo atomic ratio was 1:3, the electrochemically active surface area and positive scan peak current density of the catalyst reached the maximum, and the maximum active surface area was 129.3 m 2 ·g -1 Pt The highest positive scan peak current density reached 1898.7 mA mg -1 Pt At this time, the ratio of the peak current density of the positive scan to the negative scan during the electro-oxidation of ethanol reaches (I f / I b ) is the largest, indicating that this catalyst has the least residual intermediates during the ethanol electro-oxidation process; when the PtMo atomic ratio is 1:3, its CO electro-oxidation peak potential is the lowest among the five catalysts, at 0.62 V, indicating that this catalyst has the best tolerance to CO and CO-like species during the ethanol electro-oxidation process.

[0065] like Figure 3 It can be seen that the current density of PtMo catalysts with all atomic ratios decayed rapidly before 600s of the chronoamperometric test. This is because Pt was poisoned by intermediates such as CO. After 1200s, the current density gradually changed slowly and tended to be stable when the PtMo atomic ratio of SnO was 1:3. 2 The PtMo alloy catalyst supported on the GN composite carrier has the highest current density, indicating that the catalytic stability is best when the PtMo atomic ratio is 1:3.

[0066] Comparative Example 1

[0067] This comparative example provides the Pt prepared in Example 1. 1 Mo 3 / SnO 2Electrochemical performance of GN and Pt / GN as ethanol electrooxidation catalysts in direct ethanol fuel cells, wherein the test method and calculation standard in this comparative example are the same as those in Example 2, and will not be repeated here; Pt 1 Mo 3 / SnO 2 The electrochemical performance data of GN and Pt / GN in ethanol electrooxidation reaction are shown in Table 2.

[0068] Table 2Pt 1 Mo 3 / SnO 2 Electrochemical performance of GN and Pt / GN in ethanol electrooxidation

[0069]

[0070] It can be seen from Table 2 that, compared with the Pt / GN catalyst, the Pt 1 Mo 3 / SnO 2 The GN catalyst exhibited more excellent catalytic performance for ethanol electrooxidation. The electrochemical active specific surface area of ​​ethanol electrooxidation, the positive sweep current density, and the tolerance to ethanol oxidation intermediates were greatly improved.

[0071] Comparative Example 2

[0072] This comparative example provides the Pt prepared in Example 1. 1 Mo 3 / SnO 2 GN catalyst and Pt obtained by treating graphene with nitric acid vapor alone 1 Mo 3 / SnO 2 GN(N), SnO 2 The precursor was dried by forced air and calcined in air to obtain Pt 1 Mo 3 / SnO 2 GN(A) and Pt without plasma treatment 1 Mo 3 / SnO 2 Comparison of catalytic performance and CO poisoning resistance of GN(P) as ethanol electro-oxidation catalyst.

[0073] In addition, the test method and calculation standard in this comparative example are the same as those in Example 2, and will not be repeated here; Pt 1 Mo 3 / SnO 2 GN and Pt 1 Mo 3 / SnO 2GN(N),Pt 1 Mo 3 / SnO 2 GN(A) and Pt 1 Mo 3 / SnO 2 GN(P) These four Pt 1 Mo 3 The electrochemical performance and CO poisoning resistance of the alloy composite materials in catalytic ethanol electrooxidation applications are shown in Table 3.

[0074] Table 3 Pt prepared in Example 1 1 Mo 3 / SnO 2 Comparison of GN performance with related catalysts

[0075]

[0076] It can be seen from Table 3 that by comparing with Pt 1 Mo 3 / SnO 2 GN(N),Pt 1 Mo 3 / SnO 2 GN(A) and Pt 1 Mo 3 / SnO 2 GN(P) etc.SnO 2 Compared with the PtMo alloy supported by GN, the Pt prepared by the present invention 1 Mo 3 / SnO 2 The GN composite material exhibited more excellent ethanol electro-oxidation performance and CO poisoning resistance, and the ethanol oxidation onset potential, peak potential and CO poisoning resistance were greatly improved.

[0077] Through the above tests and comparative analysis, it can be seen that SnO 2 When the content is 20%, the molar ratio of Pt to Mo is 1:3, the content of PtMo alloy is 10%, and the calcination temperature is 550℃, the prepared PtMo / SnO 2 The GN composite material has higher catalytic activity, lower charge transfer resistance, and higher current density for ethanol oxidation. 1 Mo 3 / SnO 2 GN(N), SnO 2 The precursor was dried by forced air and calcined in air to obtain Pt 1 Mo 3 / SnO 2 GN(A) and Pt without plasma treatment 1Mo 3 / SnO 2 Compared with composite materials such as GN(P), the PtMo / SnO 2 GN has better catalytic effect, stronger ethanol electrochemical oxidation performance and CO poisoning resistance. The composite material of the present invention can be applied to direct ethanol fuel cells and used as a catalyst for ethanol electro-oxidation to improve the electro-oxidation efficiency of ethanol, so as to enable direct ethanol fuel cell technology to move further towards commercialization.

[0078] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A SnO 2 Preparation method of GN composite carrier-supported PtMo alloy catalyst, Features: SnO 2 SnO and graphene 2 The GN composite carrier is the catalyst carrier, and the PtMo alloy is used as the active component. 2 GN composite support, PtMo / SnO 2 GN Catalyst.

2. The preparation method according to claim 1, Features: The PtMo / SnO 2 The total mass fraction of the PtMo alloy in the GN catalyst is 3-10%, the atomic ratio of Pt to Mo in the PtMo alloy is 1:1-1:5, and the SnO 2 The mass loading ratio is 5 to 20%.

3. The preparation method according to claim 1, Features: The SnO 2 The preparation process of the GN composite carrier is as follows: using ammonia water as a precipitant, a soluble tin source and graphene as raw materials to prepare the composite carrier by a sol-gel method; the concentration of the ammonia water is 0.4-0.6 mol / L, the concentration of the tin source is 0.1 mol / L; the tin source is tin tetrachloride, and the graphene is precipitated by nitric acid or sulfuric acid vapor and H 2 O 2 Graphene after oxidation treatment.

4. The preparation method according to claim 3, Features: The oxidation treatment process of graphene is as follows: concentrated nitric acid or concentrated sulfuric acid is heated to generate acid vapor, and graphene is continuously heated in a concentrated acid vapor environment for acid treatment. After the treatment is stopped, the temperature of graphene is continued to dry the graphene treated with acid vapor, and the graphene is washed until the pH value of the filtrate is 7; and then transferred to H 2 O 2 The solution is heated and ultrasonicated for 1 to 3 hours, then washed with deionized water, dried in a vacuum drying oven for 8 to 12 hours, and ground for 10 to 20 minutes to obtain oxidized graphene.

5. The preparation method according to claim 4, Features: The concentrated nitric acid or concentrated sulfuric acid and the graphene are heated separately, the heating temperature of the concentrated nitric acid or concentrated sulfuric acid is 130-150° C., the graphene is continuously heated at a temperature of 110-130° C. in a concentrated acid vapor environment, and the heating time is 7-9 hours. After the concentrated acid heating is stopped, the temperature of the graphene is continued to be maintained to dry the graphene treated with acid vapor, and the temperature is maintained at 110-130° C. for 24 hours.

6. The preparation method according to claim 5, Features: The H 2 O 2 The concentration of the solution is 3-30%, the heat treatment temperature is 60° C., and the time is 10 minutes; after the heat treatment, the substrate is washed with deionized water for at least 3 times.

7. The preparation method according to any one of claims 1 to 6, Features: The PtMo alloy is supported on SnO 2 The process on the GN composite carrier is: ethylene glycol is used as a reducing agent, and a soluble platinum source and a molybdenum source are used as raw materials to prepare the GN composite carrier by a microwave reduction method; the platinum source is chloroplatinic acid, and the molybdenum source is ammonium molybdate.

8. The preparation method according to claim 7, Features: Mix 0.1-0.2 mol / L chloroplatinic acid ethylene glycol solution and 0.1-0.2 mol / L ammonium molybdate ethylene glycol solution and stir for 30 min, then add SnO 2 GN composite carrier, ultrasonically and stirred for 30 minutes each to form a uniform solution, and added 3-5wt.% NaOH / EG to adjust the pH value to 9-10 to obtain a precursor solution; the precursor solution was heated to 160-180°C in a microwave reactor at a power of 450-550W and maintained for 90 seconds; after standing and cooling, a 3-5wt.% dilute nitric acid aqueous solution was used to adjust the pH value to 5-7, and stirred for 30 minutes; washed until the filtrate was neutral, vacuum dried, and treated with plasma in an Ar environment for 5-15 minutes to obtain PtMo / SnO 2 GN Catalyst.

9. SnO prepared by the preparation method according to any one of claims 1 to 8 2 GN composite carrier supported PtMo alloy catalyst, Features: The PtMo / SnO 2 The total mass fraction of the PtMo alloy in the GN catalyst is 3-10%, the atomic ratio of Pt to Mo in the PtMo alloy is 1:1-1:5, and the SnO 2 The mass loading ratio is 5 to 20%.

10. SnO prepared by the preparation method according to any one of claims 1 to 8 2 GN composite carrier supported PtMo alloy catalyst or PtMo / SnO as claimed in claim 9 2 Application of GN catalyst in catalyzing ethanol electrooxidation reaction in direct ethanol fuel cells.

Citation Information

Patent Citations

  • Preparation method of platinum-nickel / nitrogen doped reduced graphene oxide

    CN111342060A

  • Oxygen vacancy type NiO loaded graphene electrocatalyst and preparation method thereof

    CN111883790A

  • Preparation and application of composite hollow graphene ball loaded platinum-nickel nanoparticles

    CN114695908A

  • Composite catalyst as well as preparation method and application thereof

    CN115966717A

  • Method for producing catalyst material

    JP2023114350A