Ga-doped LLZO oxide solid electrolyte, preparation method and lithium ion battery
By introducing Ga-doped LLZO oxide solid electrolyte into lithium-ion batteries, the problems of high surface roughness of electrolytes and growth of lithium dendrites in lithium batteries are solved, and higher ionic conductivity and battery life are achieved, which is suitable for industrial production. .
Patent Information
- Application Number
- CN202411125781.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
AI Technical Summary
The solid electrolyte surface interface of existing solid-state lithium-ion batteries is high in high roughness and many pores, making it difficult to achieve close contact with metal lithium. Li dendrites are prone to nucleation and growth at grain boundaries and pores, resulting in a short circuit in the battery and limiting lithium ions. Battery performance and lifespan.
By introducing Ga-doped LLZO oxide solid electrolyte, solid phase sintering method is used to regulate grain growth, reduce grain boundaries and pores, improve the density and ionic conductivity of the electrolyte, and micro-crystal particles with uniform glass phase structure are prepared. Enhance the migration ability of lithium ions.
It significantly improves the conductivity of lithium ions, extends the cycle life of lithium batteries, reduces the interface resistance, enhances the stability and electrochemical performance of lithium batteries, and is suitable for large-scale industrial production.
Smart Images

Figure CN119009080A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solid-state lithium-ion batteries, and in particular relates to a Ga-doped LLZO oxide solid electrolyte, a preparation method and a lithium-ion battery. Background Art
[0002] Due to the high demand for lithium batteries due to the development of science and technology, such as smaller size and longer life, these factors have undoubtedly become factors hindering the development of liquid lithium-ion batteries. Solid-state lithium-ion batteries (LIBs) can meet the needs due to their high energy density, flexible design, light weight and long life, and are widely used in electronic devices. However, due to the influence of the preparation process, the surface interface roughness of the solid electrolyte is relatively high and there are many pores, making it difficult to achieve close contact with metallic lithium. In addition, lithium dendrites are more likely to nucleate and grow at defects such as grain boundaries and pores, which can easily cause the battery to short-circuit. Therefore, it is necessary to regulate the growth of grains, inhibit the generation of microstructural defects, and design and develop high-density and high-ionic conductivity solid electrolytes to break the bottleneck of lithium-ion battery development and fundamentally solve the problems existing in the current lithium-ion battery industry.
[0003] Qin Shiying et al. (Qin S, Zhu X, Jiang Y, et al. Growth of self-textured Ga3 + -substituted Li7La3Zr2O 12 ceramics by solid state reaction and their significant enhancement in ionic conductivity[J].AppliedPhysics Letters,2018,112(11):113901.) LiOH·H2O, La2O3, Ga2O3, ZrO2 and a small amount of Al2O3 were mixed with isopropanol and mechanically ground for 12 h to obtain a mixed slurry. After the mixed slurry was dried in air, it was calcined at 1000°C in a muffle furnace for 12 h. Thereafter, the reaction product was ball-milled again and cold-pressed into pellets. The pellets were sintered at 1075°C for 12 h at a heating rate of 1°C / min, cooled to 500°C at a cooling rate of 1°C / min, and then naturally cooled to room temperature in the furnace. However, there were a large number of pores in the cross section of the ceramic, which greatly limited the migration barrier of lithium ions.
[0004] Dawei Wang et al. (Wang D, Zhong G, Pang WK, et al. Toward Understanding the Lithium Transport Mechanismin Garnet-type Solid Electrolytes: Li + Ion Exchanges and Their Mobility at Octahedral / Tetrahedral Sites[J].Chemistry of Materials,2015,27(19):6650–6659.) The raw materials LiOH·H2O, La2O3, ZrO2 and WO3 were mixed and ground in a planetary grinder using isopropanol as a grinding agent. The precursor was crushed for 12 hours, dried at 120°C, and then calcined at 800°C for 12 hours. After secondary crushing and drying, it was uniaxially cold pressed into pellets at 2MPa. Finally, the W-containing pellets were sintered in an Al2O3 crucible at 1150°C, 1175°C and 1200°C for 12 hours. However, the grain size was about 3-10μm and the grain boundary component was high, resulting in poor air stability and electrochemical performance of the electrolyte. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a Ga-doped LLZO oxide solid electrolyte, a preparation method and a lithium-ion battery, by introducing the doping element Ga through a simple solid-phase sintering method, which has a kinetic acceleration effect on the migration of lithium ions, can improve the electrochemical properties of the solid electrolyte, and expand the field application of lithium batteries.
[0006] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0007] A Ga-doped LLZO oxide solid electrolyte, the chemical formula of which is Li 7- 3x Ga x La3Zr2O 12 , where 0.2≤x≤0.35.
[0008] The oxide solid electrolyte is micron crystal particles with a uniform glass phase structure, a particle size of 5-500 μm, and a cubic garnet structure.
[0009] A method for preparing the Ga-doped LLZO oxide solid electrolyte as described above comprises the following steps:
[0010] Step 1: Press Li 7-3x Ga x La3Zr2O12 Chemical formula Weigh raw material powders LiOH·H2O, La2O3, Ga2O3 and ZrO2 respectively to obtain a mixed raw material;
[0011] Step 2: adding an organic wet grinding solvent to the mixed raw material in step 1, ball milling, and drying in sequence to obtain a dry mixed raw material;
[0012] Step 3: pre-calcining the mixed raw material dried in step 2, so that the Ga-doped LLZO is transformed from a tetragonal phase to a cubic phase; then performing secondary ball milling and drying to obtain a pre-calcined powder;
[0013] Step 4: isostatically pressing the pre-sintered powder in step 3 to obtain a dense green blank;
[0014] Step 5: Sinter the dense green blank in step 4 to obtain a Ga-doped LLZO oxide solid electrolyte.
[0015] The ball milling speed in step 2 and step 3 is 280-320 rpm / min, and the time is 17-19 h; the drying temperature in step 2 and step 3 is 65-80° C., and the time is 4-5 h.
[0016] The organic wet grinding solvent is isopropanol, tert-butanol or n-butanol.
[0017] In the step 3, the mixed raw material dried in the step 2 is heated to 850-950° C. at 2-3° C. / min and pre-calcined for 5-7 hours.
[0018] The pressure of the medium static pressure in step 4 is 29-32 MPa, and the holding time is 10-12 minutes.
[0019] In the step 5, the dense green blank in the step 4 is sintered at 1120-1170° C. for 5-7 hours.
[0020] The present invention also provides a lithium-ion battery, comprising the Ga-doped LLZO oxide solid electrolyte or the Ga-doped LLZO oxide solid electrolyte prepared by the above method.
[0021] Compared with the prior art, the present invention has the following beneficial effects:
[0022] 1. The present invention prepares Li doped with different Ga contents by solid phase sintering method 7-3x Ga x La3Zr2O 12 The solid electrolyte has fewer pores and grain boundaries, generates a uniform glass phase structure, improves the flatness of the interface, has a higher relative density, and improves the ionic conductivity of the solid electrolyte.
[0023] 2. The present invention can effectively reduce the content of the passivation layer (Li2CO3, LiOH) at the grain boundary by doping different contents of Ga into the LLZO oxide solid electrolyte, thereby enhancing the ability of lithium ions to cross the grain boundary; and the elimination of pores and grain boundaries can significantly improve the ability of the electrolyte to inhibit the growth of lithium dendrites. The Ga-doped LLZO oxide solid electrolyte prepared by the present invention has a small surface roughness, high flatness, uniform potential distribution, sufficient electrochemical reaction at the interface, reduced interface resistance, improved the ability to inhibit the growth of lithium dendrites, and thus improved the conductivity of lithium ions.
[0024] 3. The present invention can effectively control the grain size by doping different contents of Ga into the LLZO oxide solid electrolyte.
[0025] 4. Compared with the prior art, the present invention adopts a lower pre-firing temperature (850-950°C) and a higher sintering temperature (1120-1170°C), and can realize the transformation from tetragonal phase to cubic phase within the pre-firing temperature range (the cubic phase has a higher ionic conductivity). Within the sintering temperature range, Ga2O3 will react with Li2O to generate a binary system of LiGaO2-Li5GaO4, and the eutectic temperature point is 950-975°C. Above 1100°C, the binary system can be fully liquefied, and the Ga content in the range of 0.2-0.35 can make the liquid phase fully fill the grain boundaries and pores, making it easier for ions to move and grow along the interface during sintering, which can effectively promote grain growth.
[0026] In summary, compared with the LLZO oxide solid electrolyte in the prior art, the Ga-doped LLZO oxide solid electrolyte prepared by the present invention has the characteristics of small surface roughness, good density, small interface resistance and low activation energy, improves the ability to inhibit the growth of lithium dendrites, thereby improving the conductivity of lithium ions, and extending the cycle life of lithium batteries. The preparation method is simple and suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 1 is the XRD diagram of the LLZO oxide solid electrolyte at different Ga doping contents of the present invention (x=0 to x=0.35 are Comparative Example 1, Example 1, Example 2, Example 3, and Example 4, respectively).
[0028] Figure 2 : is the SEM image of LLZO oxide solid electrolyte with different Ga doping contents of the present invention, wherein: Figure 2 a- Figure 2 e is the surface morphology image, Figure 2 g- Figure 2 k is a cross-sectional morphology diagram (from left to right are Comparative Example 1, Example 1, Example 2, Example 3, Example 4).
[0029] Figure 3 It is the XPS spectrum of comparative example 1 and embodiment 2, wherein, Figure 3 a is the XPS spectra of Li 1s of Comparative Example 1 and Example 2, Figure 3 b is the XPS spectrum of O1s of Comparative Example 1 and Example 2.
[0030] Figure 4 : is the AFM image of the LLZO oxide solid electrolyte with different Ga doping contents of the present invention, wherein: Figure 4 a is the surface morphology of comparative example 1, Figure 4 b is the surface morphology of Example 2, Figure 4 c is the potential distribution diagram of comparative example 1, Figure 4 d is the potential distribution diagram of Example 2.
[0031] Figure 5 : is the temperature-dependent impedance diagram of the LLZO oxide solid electrolyte at different Ga doping contents of the present invention, wherein: Figure 5 a is comparative example 1, Figure 5 b is Example 2.
[0032] Figure 6 for Figure 5 The trend of conductivity with temperature.
[0033] Figure 7 It is a density bar graph of the LLZO oxide solid electrolyte at different Ga doping contents of the present invention.
[0034] Figure 8 The electrochemical impedance spectra of the LLZO oxide solid electrolyte prepared in Comparative Example 1 and Example 2 are shown in FIG. Figure 8 a is Example 2, Figure 8 b is comparative example 1.
[0035] Fig. 9 Critical current density diagram of LLZO oxide solid electrolyte prepared in Comparative Example 1 and Example 2, wherein: Fig. 9 a is comparative example 1, Fig. 9 b is Example 2.
[0036] Fig.10 This is a test chart of the long-cycle stability of lithium batteries using the Ga-doped LLZO oxide solid electrolyte prepared in Example 2. DETAILED DESCRIPTION
[0037] The present invention is further described in detail below in conjunction with the accompanying drawings and embodiments, but the protection scope of the present invention is not limited to these embodiments.
[0038] A Ga-doped LLZO oxide solid electrolyte, the chemical formula of which is Li7-3x Ga x La3Zr2O 12 , wherein 0.2≤x≤0.35, the oxide solid electrolyte is a micron crystal particle with a uniform glass phase structure, the particle size of which is 5-500 μm and has a cubic garnet structure.
[0039] A method for preparing a Ga-doped LLZO oxide solid electrolyte comprises the following steps:
[0040] Step 1: Press Li 7-3x Ga x La3Zr2O 12 Chemical formula Weigh raw material powders LiOH·H2O, La2O3, Ga2O3 and ZrO2 respectively to obtain a mixed raw material;
[0041] Step 2: adding an organic wet grinding solvent to the mixed raw material of step 1, ball milling at a speed of 280-320rpm / min for 17-19h, and then drying at 65-80℃ for 4-5h to obtain a dry mixed raw material; the organic wet grinding solvent is isopropanol, tert-butyl alcohol or n-butyl alcohol, which is not easy to produce Li2CO3 impurities by side reaction during the preparation process; the mass ratio of the mixed raw material to the ZrO2 ball is (5-10):1, and two ZrO2 grinding balls with different diameters are used, and the mass ratio is 1:1, and the diameters of the two ZrO2 grinding balls are 5μm and 3μm respectively;
[0042] Step 3: The mixed raw material dried in step 2 is heated to 850-950°C at 2-3°C / min and pre-calcined for 5-7h, so that the Ga-doped LLZO is transformed from a tetragonal phase to a cubic phase; then ball milled at a speed of 280-320rpm / min for 17-19h, and then dried at 65-80°C for 4-5h to obtain a pre-calcined powder;
[0043] Step 4: isostatically pressing the pre-sintered powder in step 3 to obtain a dense green blank; the isostatic pressing pressure is 29-32 MPa, and the holding time is 10-12 min;
[0044] Step 5: Place the dense green body obtained in step 4 in a muffle furnace and sinter at 1120-1170° C. for 5-7 hours to obtain a Ga-doped LLZO oxide solid electrolyte.
[0045] The present invention also provides a lithium-ion battery, comprising the Ga-doped LLZO oxide solid electrolyte or the Ga-doped LLZO oxide solid electrolyte prepared by the above method.
[0046] Example 1
[0047] A kind of Li 6.4 Ga0.20 La3Zr2O 12 A method for preparing an oxide solid electrolyte comprises the following steps:
[0048] Step 1: Press Li 6.4 Ga 0.20 La3Zr2O 12 Chemical formula Weigh raw material powders LiOH·H2O, La2O3, Ga2O3 and ZrO2 respectively to obtain a mixed raw material;
[0049] Step 2: adding isopropanol to the mixed raw material, ball milling at a speed of 280 rpm / min for 17 hours, and then drying at 65° C. for 4 hours to obtain a dry mixed raw material; the mass ratio of the mixed raw material to the ZrO2 ball is 5:1; the mass ratio of the two ZrO2 grinding balls with different diameters is 1:1, and the diameters of the two ZrO2 grinding balls are 5 μm and 3 μm respectively;
[0050] Step 3: pre-calcining the dried mixed raw material at 850°C for 5 hours at a heating rate of 2°C / min; then ball milling at a speed of 280 rpm / min for 17 hours, and then drying at 65°C for 4 hours to obtain a pre-calcined powder;
[0051] Step 4: isostatically pressing the pre-sintered powder to obtain a green body; the isostatic pressing pressure is 29 MPa, and the holding time is 10 min;
[0052] Step 5: Place the green blank in a muffle furnace and sinter at 1120°C for 5 hours to obtain Li 6.4 Ga 0.20 La3Zr2O 12 Solid electrolyte.
[0053] Example 2
[0054] A kind of Li 6.25 Ga 0.25 La3Zr2O 12 A method for preparing an oxide solid electrolyte comprises the following steps:
[0055] Step 1: Press Li 6.25 Ga 0.25 La3Zr2O 12 Chemical formula Weigh raw material powders LiOH·H2O, La2O3, Ga2O3 and ZrO2 respectively to obtain a mixed raw material;
[0056] Step 2: adding isopropanol to the mixed raw material of step 1, ball milling at a speed of 300 rpm / min for 18 hours, and then drying at 70°C for 4.5 hours to obtain a dry mixed raw material; the mass ratio of the mixed raw material to the ZrO2 ball is 5:1; the mass ratio of the two ZrO2 grinding balls with different diameters is 1:1, and the diameters of the two ZrO2 grinding balls are 5 μm and 3 μm respectively;
[0057] Step 3: pre-calcining the dried mixed raw material at 900°C for 6 hours at a heating rate of 2.5°C / min; then ball milling at a speed of 300 rpm / min for 18 hours, and then drying at 70°C for 4.5 hours to obtain a pre-calcined powder;
[0058] Step 4: isostatically pressing the pre-sintered powder to obtain a green body; the isostatic pressing pressure is 30 MPa, and the holding time is 11 minutes;
[0059] Step 5: Place the green blank in a muffle furnace and sinter at 1150°C for 6 hours to obtain Li 6.25 Ga 0.25 La3Zr2O 12 Solid electrolyte.
[0060] Example 3
[0061] A kind of Li 6.1 Ga 0.30 La3Zr2O 12 A method for preparing an oxide solid electrolyte comprises the following steps:
[0062] Step 1: Press Li 6.1 Ga 0.30 La3Zr2O 12 Chemical formula Weigh raw material powders LiOH·H2O, La2O3, Ga2O3 and ZrO2 respectively to obtain a mixed raw material;
[0063] Step 2: adding tert-butyl alcohol to the mixed raw material, ball milling at a speed of 320 rpm / min for 19 hours, and then drying at 75° C. for 5 hours to obtain a dry mixed raw material; the mass ratio of the mixed raw material to the ZrO2 ball is 7:1; the mass ratio of the two ZrO2 grinding balls with different diameters is 1:1, and the diameters of the two ZrO2 grinding balls are 5 μm and 3 μm respectively;
[0064] Step 3: pre-calcining the dried mixed raw material at 900°C for 6 hours at a heating rate of 3°C / min, then ball milling at a speed of 320 rpm / min for 19 hours, and then drying at 75°C for 5 hours to obtain a pre-calcined powder;
[0065] Step 4: isostatically pressing the pre-sintered powder to obtain a green body; the isostatic pressing pressure is 31 MPa, and the holding time is 11 minutes;
[0066] Step 5: Place the green blank in a muffle furnace and sinter at 1150°C for 6 hours to obtain Li 6.1 Ga 0.30 La3Zr2O 12 Solid electrolyte.
[0067] Example 4
[0068] A kind of Li 5.95 Ga 0.35 La3Zr2O 12 A method for preparing an oxide solid electrolyte comprises the following steps:
[0069] Step 1: Press Li 5.95 Ga 0.35 La3Zr2O 12 Chemical molecular formula: Raw material powders LiOH·H2O, La2O3, Ga2O3 and ZrO2 are weighed respectively to obtain a mixed raw material; the mass ratio of two ZrO2 grinding balls with different diameters is 1:1, and the diameters of the two ZrO2 grinding balls are 5μm and 3μm respectively;
[0070] Step 2: adding n-butanol to the mixed raw material, ball milling at a speed of 320 rpm / min for 19 hours, and then drying at 80° C. for 5 hours to obtain a dry mixed raw material; the mass ratio of the mixed raw material to the ZrO2 ball is 10:1;
[0071] Step 3: pre-calcining the dried mixed raw material at 950°C for 7 hours at a heating rate of 3°C / min, then ball milling at a speed of 320 rpm / min for 19 hours, and then drying at 80°C for 5 hours to obtain a pre-calcined powder;
[0072] Step 4: isostatically pressing the pre-sintered powder to obtain a green body; the isostatic pressing pressure is 32 MPa, and the holding time is 12 min;
[0073] Step 5: Place the green blank in a muffle furnace and sinter at 1170°C for 7 hours to obtain Li 5.95 Ga 0.35 La3Zr2O 12 Solid electrolyte.
[0074] Comparative Example 1
[0075] A Li7La3Zr2O 12 A method for preparing an oxide solid electrolyte comprises the following steps:
[0076] Step 1: Press Li7La3Zr2O12 Chemical formula: Weigh raw material powders LiOH·H2O, La2O3 and ZrO2 respectively to obtain a mixed raw material;
[0077] Step 2: adding isopropanol to the mixed raw material, ball milling at a speed of 300 rpm / min for 18 hours, and then drying at 70° C. for 4.5 hours to obtain a dry mixed raw material; the mass ratio of the mixed raw material to the ZrO2 ball is 5:1; the mass ratio of the two ZrO2 grinding balls with different diameters is 1:1, and the diameters of the two ZrO2 grinding balls are 5 μm and 3 μm respectively;
[0078] Step 3: pre-calcining the dried mixed raw material at 900°C for 6 hours at a heating rate of 2.5°C / min, then ball milling at a speed of 300 rpm / min for 18 hours, and then drying at 70°C for 4.5 hours to obtain a pre-calcined powder;
[0079] Step 4: molding the pre-sintered powder under isostatic pressing to obtain a green body; the isostatic pressing pressure is 30 MPa, and the holding time is 11 minutes;
[0080] Step 5: Place the green blank in a muffle furnace and sinter at 1150°C for 6 hours to obtain Li7La3Zr2O 12 Solid electrolyte.
[0081] Figure 1 : XRD diagram of LLZO oxide solid electrolyte at different Ga doping contents, (x=0 to x=0.35 are Comparative Example 1, Example 1, Example 2, Example 3, and Example 4, respectively); Figure 1 It can be seen that the Ga-doped LLZO oxide solid electrolytes prepared in the present invention all synthesized a cubic garnet structure.
[0082] Figure 2 : is the SEM image of LLZO oxide solid electrolyte with different Ga doping contents of the present invention, wherein: Figure 2 a- Figure 2 e is the surface morphology image, Figure 2 g- Figure 2 k is a cross-sectional morphology diagram (from left to right are Comparative Example 1, Example 1, Example 2, Example 3, Example 4).
[0083] Depend on Figure 2 a- Figure 2It can be seen that the relative density of Comparative Example 1 is 84.5%, and the relative densities of Examples 1 to 4 are 90.9%, 95.1%, 90.2% and 89.5%, respectively; compared with Comparative Example 1, the present invention doped different amounts of Ga in the LLZO oxide solid electrolyte, and it is obvious that the pores on the surface of the Ga-doped LLZO oxide solid electrolyte in Examples 1-4 are greatly reduced, the grain boundaries are reduced, and a uniform glass phase is generated, especially when x=0.25, the relative density is the highest, and the pores on the surface almost disappear, indicating that the Ga-doped LLZO oxide solid electrolyte prepared by the present invention has a higher relative density and improves the ionic conductivity of the solid electrolyte.
[0084] Depend on Figure 2 g- Figure 2 k It can be seen that compared with Comparative Example 1, by doping with different contents of Ga, the pores between the grains of the LLZO oxide solid electrolyte are eliminated, and the grains grow significantly, from 5μm to 500μm, indicating that the Ga element can regulate the grain growth of the LLZO oxide solid electrolyte, and the greater the doping content, the larger the grain size.
[0085] Figure 3 It is the XPS spectrum of comparative example 1 and embodiment 2, wherein, Figure 3 a is the XPS spectra of Li 1s of Comparative Example 1 and Example 2, Figure 3 b is the XPS spectrum of O1s of Comparative Example 1 and Example 2. Figure 3 It can be seen that the Li2CO3 content and LiOH content of Example 2 are both less than those of Comparative Example 1, indicating that the content of the passivation layer (Li2CO3, LiOH) at the grain boundary of the Ga-doped LLZO oxide solid electrolyte is reduced, which effectively inhibits the reaction of the impurity phase at its interface and enhances the ability of lithium ions to cross the grain boundaries.
[0086] Figure 4 : is the AFM image of the LLZO oxide solid electrolyte with different Ga doping contents of the present invention, wherein: Figure 4 a is the surface morphology of comparative example 1, Figure 4 b is the surface morphology of Example 2, Figure 4 c is the potential distribution diagram of comparative example 1, Figure 4 d is the potential distribution diagram of Example 2; the flatness of the electrode interface and the uniformity of the potential distribution determine whether the electrochemical reaction at the interface is sufficient. The surface morphology and potential distribution of the sample were tested using an atomic force microscope, and the surface roughness was statistically shown in Table 1, which shows the average roughness Ra and mean square roughness Rq;
[0087] Table 1 shows the surface roughness and potential results of Comparative Example 1 and Example 2
[0088]
[0089] It can be seen from Table 1 that the average roughness Ra, mean square roughness Rq and corresponding potential of the Ga-doped LLZO oxide solid electrolyte prepared by Example 2 are all smaller than those of Comparative Example 1, indicating that the solid electrolyte prepared by the present invention has high flatness and uniform potential distribution, reduces the interfacial impedance of the solid electrolyte, and improves the conductivity of lithium ions.
[0090] Figure 5 : is the temperature-dependent impedance diagram of the LLZO oxide solid electrolyte at different Ga doping contents of the present invention, wherein: Figure 5 a is comparative example 1, Figure 5 b is Example 2. Figure 5 The figure is a trend diagram of the conductivity of the LLZO oxide solid electrolyte at different Ga doping contents according to the present invention as a function of temperature. Figure 5 The intercept of the horizontal axis is the internal resistance of the battery, and its reciprocal is the conductivity. The relationship between the conductivity and temperature is as follows: Figure 6 As shown, Figure 6 The slope in represents the activation energy of lithium ion migration, which is given by Figure 6 It can be seen that the activation energy of the Ga-doped LLZO oxide solid electrolyte prepared in Example 2 is 0.30 eV, and the activation energy of the LLZO oxide solid electrolyte prepared in Comparative Example 1 is 0.41 eV. The activation energy of the Ga-doped LLZO oxide solid electrolyte prepared in the present invention is low, and the migration ability of lithium ions is improved.
[0091] Figure 7 : is a density bar graph of LLZO oxide solid electrolyte with different Ga doping contents of the present invention. Figure 7 It can be seen that the relative density of the Ga-doped LLZO oxide solid electrolyte prepared by the present invention is higher than that of the undoped LLZO oxide solid electrolyte, and when x=0.25, the relative density reaches 95.1%, which improves the density of the solid electrolyte; at the same time, when x=0, the conductivity of Comparative Example 1 is only 0.07mS·cm -1 , while the conductivity range of Examples 1 to 4 is 0.38-0.99 mS·cm -1 , combined with Figure 2 It can be seen that with the introduction of Ga ions, the grains of LLZO oxide solid electrolyte grow, the pores and grain boundaries are reduced, and a denser Ga-doped LLZO oxide solid electrolyte can be obtained, thereby improving the conductivity of lithium ions.
[0092] Figure 8 The electrochemical impedance spectra of the LLZO oxide solid electrolyte prepared in Comparative Example 1 and Example 2 are shown in FIG. Figure 8 a is Example 2, Figure 8 b is comparative example 1; Figure 8 It can be seen that compared with Comparative Example 1 (6 KΩ), the interface resistance of the Ga-doped LLZO oxide solid electrolyte prepared by the present invention is 0.6 KΩ, and the preparation method of the present invention significantly reduces the interface resistance of the Ga-doped LLZO oxide solid electrolyte.
[0093] Fig. 9 Critical current density diagram of LLZO oxide solid electrolyte prepared in Comparative Example 1 and Example 2, wherein: Fig. 9 a is comparative example 1, Fig. 9 b is embodiment 2; Fig. 9 The dashed line represents the current density, and the solid line represents the voltage. When working stably, the voltage should be linearly related to the current. However, when the current density of Comparative Example 1 is 0.03 mA cm -2 The short circuit obviously occurred under the condition of 0.8 mA cm -2 The short circuit occurred only after the short circuit occurred, and the time of the short circuit was prolonged, indicating that the ability of the Ga-doped LLZO oxide solid electrolyte prepared by the present invention to inhibit the growth of lithium dendrites has been greatly improved; the long cycle diagram of the battery prepared by the Ga-doped LLZO oxide solid electrolyte in Example 2 is as follows: Fig.10 As shown, at 0.05-0.2 mA cm -2 In the long cycle charge and discharge test carried out within the range, the cycle time reaches 500h. The Ga-doped LLZO oxide solid electrolyte prepared by the present invention has high operating stability in actual work.
Claims
1. A Ga-doped LLZO oxide solid electrolyte, Features: The general chemical formula of the solid electrolyte is Li 7- 3x Ga x La 3 Zr 2 O 12 , where 0.2≤x≤0.
35.
2. The Ga-doped LLZO oxide solid electrolyte according to claim 1, Features: The oxide solid electrolyte is micron crystal particles with a uniform glass phase structure, a particle size of 5-500 μm, and a cubic garnet structure.
3. A method for preparing the Ga-doped LLZO oxide solid electrolyte as claimed in claim 1 or 2, It is characterized in that The steps include: Step 1: Press Li 7-3x Ga x La 3 Zr 2 O 12 Chemical formula Weigh the raw material powder LiOH·H 2 O.La 2 O 3 , Ga 2 O 3 and ZrO 2 , obtaining a mixed raw material; Step 2: adding an organic wet grinding solvent to the mixed raw material in step 1, ball milling, and drying in sequence to obtain a dry mixed raw material; Step 3: pre-calcining the mixed raw materials dried in step 2 to transform the Ga-doped LLZO from a tetragonal phase to a cubic phase; then performing secondary ball milling and drying to obtain a pre-calcined powder; Step 4: isostatically pressing the pre-sintered powder in step 3 to obtain a dense green blank; Step 5: Sinter the dense green blank in step 4 to obtain a Ga-doped LLZO oxide solid electrolyte.
4. A method for preparing a Ga-doped LLZO oxide solid electrolyte according to claim 3, Features: The ball milling speed in step 2 and step 3 is 280-320 rpm / min, and the time is 17-19 h; the drying temperature in step 2 and step 3 is 65-80° C., and the time is 4-5 h.
5. The method for preparing a Ga-doped LLZO oxide solid electrolyte according to claim 3, Features: The organic wet grinding solvent is isopropanol, tert-butanol or n-butanol.
6. A method for preparing a Ga-doped LLZO oxide solid electrolyte according to claim 3, Features: In the step 3, the mixed raw material dried in the step 2 is heated to 850-950° C. at 2-3° C. / min and pre-calcined for 5-7 hours.
7. The method for preparing a Ga-doped LLZO oxide solid electrolyte according to claim 3, Features: The pressure of the medium static pressure in step 4 is 29-32 MPa, and the holding time is 10-12 minutes.
8. The method for preparing a Ga-doped LLZO oxide solid electrolyte according to claim 3, Features: In the step 5, the dense green blank in the step 4 is sintered at 1120-1170° C. for 5-7 hours.
9. A lithium ion battery, Features: A Ga-doped LLZO oxide solid electrolyte comprising the Ga-doped LLZO oxide solid electrolyte according to claim 1 or 2 or prepared by the method according to any one of claims 3 to 8.