Composite diaphragm, preparation method thereof and battery containing composite diaphragm

By using composite separators on lithium-ion battery separators, including hydrophilic polymer hydrogels and ceramic coatings, the problem of insufficient heat resistance and safety of lithium-ion battery separators is solved, achieving high safety and low cost Battery manufacturing avoids the risk of battery short circuit and explosion.

CN119009372AInactive Publication Date: 2024-11-22JIANGSU TIANHE ENERGY STORAGE CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411105321.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing lithium-ion batteries and sodium-ion batteries have insufficient heat resistance and safety, which leads to battery safety problems, limits manufacturing levels, and has a wide range of production processes, increasing the use of manpower and equipment.

Method used

Using composite separators, including separator substrate layer and hydrogel coating, the hydrogel coating consists of hydrophilic polymers and binders, and a ceramic coating is provided on the surface of the separator substrate to enhance the battery through these hierarchies. The safety and heat resistance of the slabs are reduced, and the contact with the positive and negative electrodes is avoided, and short circuits and explosions are avoided.

Benefits of technology

It realizes high safety of lithium-ion batteries, reduces the risk of battery short circuit and fire explosion, reduces production costs and process complexity, can replace the traditional Mylar film, and improves the overall safety performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119009372A_ABST
    Figure CN119009372A_ABST
Patent Text Reader

Abstract

The invention provides a composite diaphragm, a preparation method thereof and a battery containing the composite diaphragm. The composite diaphragm comprises a diaphragm base material layer and a hydrogel coating, the hydrogel coating is located on at least one surface of the diaphragm base material layer, and the hydrogel coating comprises hydrophilic polymer hydrogel and a binder; the hydrophilic polymer hydrogel comprises a natural hydrophilic polymer and / or a synthetic hydrophilic polymer. The composite diaphragm provided by the invention can slow down contact with positive and negative pole pieces while maintaining excellent battery capacity effect, avoids battery short circuit and fire explosion, can replace the effect of a Mylar membrane, and further can reduce the processing cost and the production cost of a battery cell.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of batteries and relates to a composite diaphragm, a preparation method thereof and a battery containing the composite diaphragm. Background Art

[0002] Existing lithium-ion batteries and sodium-ion batteries are mainly composed of positive electrode materials, negative electrode materials, diaphragms, electrolytes, Mylar films, etc. The diaphragm is one of the core key materials of lithium-ion batteries and sodium-ion batteries. In lithium-ion batteries and sodium-ion batteries, the diaphragm mainly prevents the positive and negative electrodes from contacting and allows ion conduction. Commercial lithium-ion batteries mainly use PP or PE diaphragm materials with microporous structures, and then add inorganic and organic coatings on their surfaces.

[0003] However, since the heat resistance and safety of the diaphragm cannot meet the existing usage requirements, the battery safety problem caused by the performance of the lithium-ion battery diaphragm and the sodium-ion battery diaphragm itself has not been solved. This is a technical bottleneck restricting the manufacturing level of lithium-ion batteries and sodium-ion batteries. The square aluminum shell has many processes, and reducing the process will greatly reduce the use of manpower / cost / equipment.

[0004] Therefore, there is an urgent need for a diaphragm that can achieve high safety of lithium-ion batteries and sodium-ion batteries, while reducing the "Mylar wrapping" process of the square aluminum shell, thereby reducing the production process of the square aluminum shell and reducing the investment in manpower / cost / equipment. Summary of the invention

[0005] In order to overcome the above problems, the present invention provides a composite diaphragm, a preparation method thereof and a lithium ion battery containing the same. The composite diaphragm of the present invention achieves high safety of the battery, can reduce contact with the positive and negative electrodes, avoid battery short circuit and fire and explosion, can replace the role of Mylar film, and reduce safety costs.

[0006] Specifically, the first aspect of the present invention provides a composite diaphragm, which includes a diaphragm substrate layer and a hydrogel coating, wherein the hydrogel coating is located on at least one surface of the diaphragm substrate layer, and the hydrogel coating contains a hydrophilic polymer hydrogel and a binder; the hydrophilic polymer hydrogel contains natural hydrophilic polymers and / or synthetic hydrophilic polymers.

[0007] In one or more embodiments, the separator substrate layer is a PP film, a PE film, a composite film of PP and PE, or an aramid separator.

[0008] In one or more embodiments, the separator substrate layer has a thickness of 3-20 μm.

[0009] In one or more embodiments, the natural hydrophilic polymer is selected from one or more of polysaccharide hydrophilic polymers and polypeptide hydrophilic polymers; the polysaccharide hydrophilic polymer is selected from one or more of starch, cellulose, alginate, hyaluronic acid and chitosan; the polypeptide hydrophilic polymer is selected from one or more of collagen, poly-L-lysine and poly-L-glutamic acid.

[0010] In one or more embodiments, the synthetic hydrophilic polymer is selected from polyacrylic acid and its derivatives.

[0011] In one or more embodiments, the single-side thickness of the hydrogel coating is 1-200 μm.

[0012] In one or more embodiments, the ratio of the length of the hydrogel coating layer to the length of the membrane substrate layer is 0.1% to 100%, such as 0.5% to 5%.

[0013] In one or more embodiments, the length of the hydrogel coating is 0.01-0.5 m.

[0014] In one or more embodiments, the hydrogel coating extends along the length direction of the diaphragm substrate layer, and the width of the hydrogel coating is consistent with the width of the diaphragm substrate.

[0015] In one or more embodiments, the hydrogel coating is located at an end of the separator substrate layer.

[0016] In one or more embodiments, the binder is selected from one or more of polyvinylidene fluoride, carboxymethyl cellulose and styrene-butadiene rubber.

[0017] In one or more embodiments, in the hydrogel coating, the mass ratio of the binder to the hydrophilic polymer hydrogel is 1:(10-20).

[0018] In one or more embodiments, the composite separator further includes a ceramic coating layer, the ceramic coating layer is located on at least one surface of the separator substrate layer, and the material of the ceramic coating layer includes a ceramic material and a binder.

[0019] In one or more embodiments, the ceramic material is Al2O3 and / or TiO2.

[0020] In one or more embodiments, the binder is selected from one or more of polyvinylidene fluoride, carboxymethyl cellulose and styrene-butadiene rubber.

[0021] In one or more embodiments, in the ceramic coating, the mass ratio of the binder to the ceramic material is 1:(10-20).

[0022] In one or more embodiments, the ceramic coating extends along the length direction of the diaphragm substrate layer, and the width of the ceramic coating is consistent with the width of the diaphragm substrate layer. In one or more embodiments, the ceramic coating and the hydrogel coating are adjacently arranged along the length direction of the diaphragm substrate layer, and the hydrogel coating is located at a position on the diaphragm substrate where the ceramic coating is not arranged.

[0023] In one or more embodiments, the ceramic coating has a single-side thickness of 0-5 μm.

[0024] In one or more embodiments, the ceramic coating has a length of 0.01-10 m.

[0025] The second aspect of the present invention provides a method for preparing a composite diaphragm as described in any embodiment of the present invention, the method comprising the following steps: uniformly mixing the hydrophilic polymer hydrogel, the binder and water to obtain a hydrogel coating slurry;

[0026] The hydrogel coating slurry is coated on at least one surface of the membrane substrate and dried to obtain the composite membrane.

[0027] A third aspect of the present invention provides a lithium ion battery, wherein the lithium ion battery comprises the composite separator as described in any embodiment of the present invention.

[0028] In one or more embodiments, the lithium-ion battery includes a battery cell formed by winding the composite separator with a positive electrode sheet and a negative electrode sheet, the hydrogel coating exists in the outermost circle of the battery cell, and the difference between the outer circumference of the battery cell and the length of the hydrogel coating is ≤10 mm. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The schematic diagram of the diaphragm structure prepared in Example 1. 1 is the diaphragm substrate, 2 is the ceramic coating, and 3 is the hydrogel coating.

[0030] Figure 2 Schematic diagram of the structure of a lithium-ion battery made using the diaphragm of Example 1. DETAILED DESCRIPTION

[0031] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in this article. Unless otherwise specified, all technical and scientific terms used in this article are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definitions in this article shall prevail.

[0032] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.

[0033] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.

[0034] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values ​​within the range (including integers and fractions).

[0035] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.

[0036] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.

[0037] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.

[0038] The present invention provides a hydrogel coating on at least one surface of the diaphragm substrate, thereby greatly improving the safety of the battery while maintaining excellent battery capacity. It can reduce contact with positive and negative electrodes to avoid battery short circuit and fire and explosion, and can replace the role of Mylar film, thereby reducing the processing cost and BOM (bill of materials) cost of the battery cell.

[0039] In the present invention, the hydrogel coating comprises a hydrophilic polymer hydrogel and a binder, and the hydrophilic polymer hydrogel comprises a natural hydrophilic polymer and / or a synthetic hydrophilic polymer.

[0040] The natural hydrophilic polymer can be selected from one or more of polysaccharide hydrophilic polymers and / or polypeptide hydrophilic polymers. The polysaccharide hydrophilic polymer can be selected from one or more of starch, cellulose, alginic acid, hyaluronic acid and chitosan. The polypeptide hydrophilic polymer can be selected from one or more of collagen, poly-L-lysine and poly-L-glutamic acid.

[0041] The synthetic hydrophilic polymer can be selected from polyacrylic acid and its derivatives, wherein the derivatives can be one or more of polyacrylic acid, polymethacrylic acid, polyacrylamide and poly-N-polyacrylamide.

[0042] In the hydrogel coating, the mass ratio of the binder to the hydrophilic polymer hydrogel is 1:(10-20), for example, 1:12, 1:15, 1:18.

[0043] The hydrogel coating of the present invention may further include functional additives. The functional additives help increase the plastic strength of the hydrogel. The functional additives may be selected from inorganic and / or organic additives, such as Al2O3, TiO2, etc.

[0044] In some specific embodiments, the hydrogel coating of the present invention comprises cellulose hydrogel, styrene-butadiene rubber (SBR), carboxymethyl cellulose (CMC).

[0045] In some specific embodiments, the hydrogel coating of the present invention comprises polyacrylic acid hydrogel, styrene-butadiene rubber (SBR), and carboxymethyl cellulose (CMC).

[0046] The hydrophilic polymer hydrogel of the present invention has the effect of covering the external needle puncture tip, thereby reducing the contact with the positive and negative electrode sheets to cause a short circuit effect.

[0047] The hydrogel coating may be disposed on one surface or two surfaces of the membrane substrate disposed oppositely. The thickness of the hydrogel coating on a single surface may be 1-200 μm or 40-100 μm, for example 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 80 μm, 100 μm, 120 μm, 150 μm, 180 μm.

[0048] The hydrogel coating may cover all or part of the length of the diaphragm substrate layer. When the hydrogel coating does not cover the entire length of the diaphragm layer, the hydrogel coating is preferably disposed near the end point of the diaphragm, and the length of the hydrogel coating is preferably sufficient to cover the outermost winding core of the core package. In some embodiments, the ratio of the length of the hydrogel coating to the length of the diaphragm substrate layer is 0.1%-100%, such as 0.5%-5%, such as 1.2%, 2%, 3%, 4%. In some embodiments, the length of the hydrogel coating is 0.01-0.5m, such as 0.05m, 0.1m, 0.2m, 0.3m, 0.4m.

[0049] In the present invention, the separator substrate layer may be a PP film, a PE film, an aramid separator, or a composite film of PP and PE.

[0050] The thickness of the separator substrate layer may be 3-20 μm, for example, 8 μm, 10 μm, 13 μm, 15 μm, or 18 μm.

[0051] In the present invention, at least one surface of the diaphragm substrate layer may also be coated with a ceramic coating. The material of the ceramic coating may include one or more of a self-adhesive and a ceramic. The binder may be selected from one or more of polyvinylidene fluoride (PVDF), carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR); the ceramic may be selected from Al2O3 and / or TiO2. The ceramic coating may be disposed on one surface of the diaphragm substrate or on two surfaces disposed oppositely. The single-sided thickness of the ceramic coating may be 0-5 μm.

[0052] In the ceramic coating, the mass ratio of the binder to the ceramic material is 1:(10-20), for example, 1:12, 1:15, 1:18.

[0053] When the surface of the diaphragm substrate layer is coated with a ceramic coating, the ceramic coating and the hydrogel coating may be disposed adjacently or non-adjacently on one surface or both surfaces of the diaphragm substrate. The length of the ceramic coating and the hydrogel coating may be flexibly adjusted depending on the winding length and may vary depending on the number of pole pieces and the size of the winding needle. The length of the ceramic coating may be 0.01-10 m. The length of the hydrogel coating may be 0.01-0.5 m. The total length of the hydrogel coating may be the total length of the diaphragm substrate minus the total length of the ceramic coating.

[0054] In some embodiments, the membrane structure of the present invention is as follows Figure 1 As shown, it includes a hydrogel coating and a ceramic coating, the ceramic coating and the hydrogel coating are adjacently arranged on at least one surface of the diaphragm substrate, and the coating position of the hydrogel coating is from the starting point after the ceramic coating to the end point of the diaphragm.

[0055] The present invention provides a method for preparing the above-mentioned diaphragm, which comprises the following steps: coating a hydrogel coating on at least one surface of a diaphragm substrate.

[0056] There is no particular limitation on the coating method, and conventional coating methods in the art may be used.

[0057] In some specific embodiments, a ceramic coating is coated on at least one surface of the membrane substrate, and then a hydrogel coating is coated adjacent to the ceramic coating, and this is a cycle, so that the ceramic coating and the hydrogel coating are alternately arranged on at least one surface of the membrane substrate.

[0058] After coating, the separator may be dried. After drying, the thickness of the ceramic coating on a single surface may be 0-3 μm. The thickness of the hydrogel coating on a single surface may be 5-200 μm.

[0059] Lithium-ion battery

[0060] The lithium ion battery comprises a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The lithium ion battery of the present invention is characterized in that it comprises the composite separator of the present invention. The composite separator of the present invention is applicable to various types of lithium ion batteries.

[0061] The positive electrode sheet includes a positive electrode current collector and a positive electrode material layer formed on the surface of the positive electrode current collector. The positive electrode material layer includes a positive electrode active material, a conductive agent and a binder. The positive electrode material layer is obtained by coating a positive electrode slurry containing a positive electrode active material, a conductive agent, a binder and a solvent onto the positive electrode current collector, and then rolling and baking. The positive electrode current collector can be copper foil, aluminum foil, titanium foil, nickel foil, iron foil, zinc foil, etc. The solvent of the positive electrode slurry can be N-methylpyrrolidone (NMP).

[0062] The positive electrode active material may be selected from lithium iron phosphate, lithium iron manganese phosphate, lithium cobaltate, lithium manganate, binary positive electrode material, ternary positive electrode material, quaternary positive electrode material, etc. The conductive agent of the positive electrode may be one or more selected from conductive carbon black (SP), carbon fiber (CF), acetylene black, conductive graphite, graphene, carbon nanotubes and carbon microspheres. The binder of the positive electrode may be one or more selected from polyvinylidene fluoride (PVDF), polytetrafluoroethylene, polyvinyl alcohol, polyolefin, styrene butadiene rubber, fluorinated rubber, polyurethane and sodium alginate. In some embodiments, the conductive agent in the positive electrode material layer is SP and the binder is PVDF. The content ratio of each component in the positive electrode material layer may be conventional. For example, the mass fraction of the positive electrode active material may be 90% to 98%, such as 92%, 94%, 96%, 96.7%, 97.5%. The mass fraction of the conductive agent may be 1% to 5%, such as 1.2%, 1.3%, 1.5%, 2%, 3%, 3.5%, 4%. The mass fraction of the binder can be 1% to 5%, for example, 1.2%, 1.5%, 1.8%, 2%, 2.5%, 3%, 4%. The compaction density of the positive electrode material layer can be 3.4 to 3.7 g / cm 3 , for example 3.45g / cm 3 、3.5g / cm 3 、3.55g / cm 3 、3.6g / cm 3 、3.65g / cm 3 .

[0063] The negative electrode sheet includes a negative electrode current collector and a negative electrode material layer formed on the surface of the negative electrode current collector. The negative electrode current collector may be a copper foil. The negative electrode material layer includes a negative electrode active material, a conductive agent and a binder. The negative electrode material layer is obtained by coating a negative electrode slurry containing a negative electrode active material, a conductive agent, a binder and a solvent onto a positive electrode current collector, and then rolling and baking. The solvent of the negative electrode slurry may be water. The negative electrode active material may be one or more selected from carbon materials (such as graphite), silicon, silicon compounds, lithium titanate, tin and tin compounds. The negative electrode conductive agent may be one or more selected from conductive carbon black (SP), acetylene black, carbon nanotubes, carbon nanowires, carbon microspheres, carbon fibers and graphene. The negative electrode binder may be one or more selected from polyvinylidene fluoride, polytetrafluoroethylene, acrylonitrile multipolymer, polybutyl acrylate, polyacrylonitrile and styrene-butadiene rubber (SBR). The negative electrode material layer and the negative electrode slurry may also include a thickener, such as sodium carboxymethyl cellulose (CMC-Na). In some embodiments, the negative electrode active material in the negative electrode material layer is graphite, the conductive agent is conductive carbon black, the binder is styrene-butadiene rubber, and the thickener is sodium carboxymethyl cellulose. The mass ratio of each component in the negative electrode material layer can be conventional. For example, the mass fraction of the negative electrode active material can be 90% to 98%, such as 93%, 95%, 95.7%, 96%, 97%. The mass fraction of the conductive agent can be 0.5% to 5%, such as 1%, 1.5%, 2%. The mass fraction of the binder can be 0.5% to 5%, such as 1%, 1.5%, 2%, 3%. The mass fraction of the thickener can be 0 to 5%, such as 1%, 1.5%, 1.8%, 2%, 3%. The compaction density of the negative electrode material layer can be 1.4 to 1.7 g / cm 3 , for example 1.45g / cm 3 , 1.5g / cm 3 , 1.55g / cm 3 , 1.6g / cm 3 , 1.65g / cm 3 .

[0064] The electrolyte of a lithium-ion battery contains an organic solvent and a lithium salt. The organic solvent commonly used in the electrolyte is a carbonate solvent. Suitable carbonate solvents include, but are not limited to, one or more selected from ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate, dimethyl carbonate (DMC), diethyl carbonate (DEC), and ethyl methyl carbonate (EMC), preferably two or more. Preferably, the carbonate solvent contains at least one cyclic carbonate and at least one chain carbonate. Examples of cyclic carbonates include EC, PC, and butylene carbonate. Examples of chain carbonates include DMC, DEC, and EMC. The mass ratio of cyclic carbonates to chain carbonates can be 1:4 to 1:1. For example, 1:3, 3:7, 1:2. The lithium salt in the electrolyte of the present invention can be a lithium salt commonly used in the art, including but not limited to lithium hexafluorophosphate (LiPF6), lithium bistrifluoromethanesulfonyl imide (LiTFSI), lithium bis(fluorosulfonyl) imide (LiFSI), lithium bisoxalate borate (LiBOB), lithium difluorooxalate borate (LiODFB), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium perchlorate (LiClO4), lithium fluoride (LiF), lithium trifluoromethanesulfonate (LiCF3SO3), etc. In some embodiments, the lithium salt is LiPF6. The concentration of the lithium salt in the electrolyte can be 0.5 to 2 mol / L, for example 0.8 mol / L, 1 mol / L, 1.2 mol / L.

[0065] Part or all of the separators in the lithium ion battery of the present invention are the composite separators of the present invention.

[0066] The positive electrode sheet, the negative electrode sheet and the separator are stacked or wound according to the design requirements, and then packaged in a shell, and then dried, injected (electrolyte is injected), packaged, left to stand, formed, and sorted to obtain a lithium ion battery. The form of the lithium ion battery of the present invention is not particularly limited, and can be a cylindrical lithium ion battery, a soft-pack lithium ion battery or an aluminum shell lithium ion battery.

[0067] In the present invention, when the positive electrode sheet, the negative electrode sheet and the separator are stacked or wound to prepare a core package, the clockwise distance between the starting point and the ending point of the hydrogel coating in a single core package preferably satisfies <10 mm.

[0068] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.

[0069] Example 1

[0070] (1) An organic microporous polyethylene (PE) film with a thickness H1 of 13 μm and a length of 5.2 m was used as the separator substrate.

[0071] (2) Al2O3 powder, binder (styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC)), and deionized water are fully mixed to form a slurry, wherein the mass ratio of Al2O3 powder, SBR, CMC, and deionized water is 95:3:2:900. The prepared slurry is evenly coated on both sides of the diaphragm substrate using an automatic coating apparatus, dried at room temperature, and then vacuum dried at 50°C for 10 hours to obtain a ceramic coating. Among them, the length L1 of the ceramic coating on one side after coating is 5.1m, the coating thickness H2 is 2μm, and the width of the ceramic coating is consistent with the width of the diaphragm substrate.

[0072] (3) Cellulose hydrogel (Shandong Qiyue, CNFs / PVA), binder (styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC)), and deionized water were fully mixed to form a slurry, wherein the mass ratio of cellulose hydrogel, SBR, CMC, and deionized water was 95:3:2:900. The prepared slurry was evenly coated on both sides of the diaphragm substrate using an automatic coating apparatus, and the coating position was from the starting point after the ceramic coating to the end point of the diaphragm. After drying at room temperature, it was vacuum dried at 50°C for 10 hours to obtain a hydrogel coating. Among them, the length L2 of the hydrogel coating was 0.1m, the thickness H3 of the hydrogel coating was 50μm, and the width of the hydrogel coating was consistent with the width of the diaphragm substrate.

[0073] Figure 1 The schematic diagram of the diaphragm structure prepared in Example 1. 1 is the diaphragm substrate, 2 is the ceramic coating, and 3 is the hydrogel coating.

[0074] Example 2

[0075] (1) An organic microporous polyethylene (PE) film with a thickness H1 of 13 μm and a length of 5.2 m was used as the separator substrate.

[0076] (2) Cellulose hydrogel (Shandong Qiyue, CNFs / PVA), binder (styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC)), and deionized water are fully mixed to form a slurry, wherein the mass ratio of cellulose hydrogel, SBR, CMC and deionized water is: 95:3:2:900. The prepared slurry is evenly coated on both sides of the diaphragm substrate using an automatic coating apparatus, and the coating position is the same as the position of the ceramic coating in Example 1 (the main difference from the diaphragm in Example 1 is that the diaphragm in Example 2 is not coated with a ceramic coating). After drying at room temperature, vacuum drying at 50°C for 10 hours to obtain a hydrogel coating. Among them, the length L2 of the hydrogel coating is 0.1m, the thickness H3 of the hydrogel coating is 50μm, and the width of the hydrogel coating is consistent with the width of the diaphragm substrate.

[0077] Example 3

[0078] The only difference between Example 3 and Example 2 is that the cellulose hydrogel is replaced by polyacrylic acid hydrogel (Xi'an Tianzheng Pharmaceutical Excipients, NP700).

[0079] Comparative Example 1

[0080] The diaphragm used in Comparative Example 1 is a diaphragm of conventional structure. The diaphragm substrate is a PE film, H1 is 9 μm, and the length is 5.2 m. The coating material is alumina and binder PVDF (mass ratio is 1:2), and the thickness is 1 μm.

[0081] Test Example 1

[0082] The separators prepared in Examples 1-3 and Comparative Example 1 were used as separators for lithium-ion batteries to prepare lithium-ion batteries.

[0083] (1) Preparation of positive electrode sheet: The positive electrode active material lithium nickel cobalt manganese oxide LiNi with a mass ratio of 97.5:1.2:0.7:0.6 0.6 Co 0.2 Mn 0.2 O2, polyvinylidene fluoride, conductive carbon black and carbon nanotubes are uniformly mixed and dispersed in N-methylpyrrolidone to prepare a positive electrode slurry, which is coated on the surface of an aluminum foil current collector and dried to obtain a positive electrode sheet;

[0084] (2) Preparation of negative electrode sheet: Graphite, sodium carboxymethyl cellulose, styrene-butadiene rubber (SBR) and conductive carbon black, which are negative electrode active materials in a mass ratio of 96.1:1.2:1.7:1, are uniformly mixed and dispersed in water to prepare a negative electrode slurry. The negative electrode slurry is coated on the surface of a copper foil current collector and dried to obtain a negative electrode sheet.

[0085] (3) Preparation of electrolyte: Ethylene carbonate EC, ethyl methyl carbonate EMC, and diethyl carbonate DEC are mixed in a mass ratio of 1:1:1 to obtain a mixed solvent. After mixing evenly, 1 mol / L lithium hexafluorophosphate is added to dissolve completely, and stirred evenly to obtain an electrolyte;

[0086] (4) Preparation of lithium-ion batteries: The cells are stacked and wound into bare cells, and the electrolyte is injected into the cells, which are then sealed to form soft-pack lithium-ion batteries. Figure 2 Schematic diagram of the structure of a lithium-ion battery made using the separator of Example 1. The difference between the outer circumference of the lithium-ion battery cell and the length of the hydrogel coating is 1 mm.

[0087] The capacity of the lithium-ion battery corresponding to the separators of Examples 1-3 and Comparative Example 1 was tested. At 25°C, the lithium-ion battery was charged to 3.65V at a constant current of 1.0C, and then further charged to a current of 0.05C at a constant voltage of 3.65V, and then discharged to 2.5V at a constant current of 1.0C. The discharge capacity was the first discharge capacity of the lithium-ion battery. According to the above charge and discharge method, the charge and discharge were cycled for 3 times, and the minimum value was taken as the capacity of the battery cell.

[0088] Safety tests were performed on the lithium-ion batteries corresponding to the diaphragms of Examples 1-3 and Comparative Example 1. Safety tests were performed using a needle puncture test. The needle puncture test can well reflect the occurrence of battery short circuits. When the steel needle pierces, the steel needle provides a path for the short circuit inside the battery. The battery's electrical energy is converted into heat energy and stored inside the battery. The short circuit causes a concentrated burst and release of energy in a short period of time, which may cause smoke, leakage, or even fire and explosion. When the needle pierces the battery, a pair of short-circuit paths are formed inside the battery, which actually simulates both internal and external short circuit processes at the same time.

[0089] The method of the puncture test is: use a steel needle with a diameter of 3mm to puncture the battery by 8μm in the radial direction.

[0090] The capacity test and safety test results of the lithium ion batteries corresponding to the separators of Examples 1-3 and Comparative Example 1 are shown in Table 1.

[0091] Table 1. Capacity test and safety test results

[0092] Capacity(Ah) Acupuncture 3μm steel needle Acupuncture 8μm steel needle Example 1 10.2 No fire, no explosion No fire, no explosion Example 2 10.1 No fire, no explosion No fire, no explosion Example 3 10.2 No fire, no explosion No fire, no explosion Comparative Example 1 10.1 Fire, no explosion Fire, explosion

[0093] It can be seen from Table 1 that when Examples 1-3 use hydrophilic polymer hydrogel as the hydrogel coating, the battery does not catch fire or explode in the needle puncture test, and its capacity is comparable to that of the conventional separator of Comparative Example 1.

Claims

1. A composite diaphragm, It is characterized in that It comprises a membrane substrate layer and a hydrogel coating, wherein the hydrogel coating is located on at least one surface of the membrane substrate layer, and the hydrogel coating comprises a hydrophilic polymer hydrogel and a binder; the hydrophilic polymer hydrogel comprises a natural hydrophilic polymer and / or a synthetic hydrophilic polymer.

2. The composite diaphragm according to claim 1, It is characterized in that The composite membrane has one or more of the following features: The diaphragm substrate layer is a PP film, a PE film, a composite film of PP and PE, or an aramid diaphragm; The thickness of the separator substrate layer is 3-20 μm.

3. The composite diaphragm according to claim 1, It is characterized in that The natural hydrophilic polymer is selected from one or more of polysaccharide hydrophilic polymers and polypeptide hydrophilic polymers; the polysaccharide hydrophilic polymer is selected from one or more of starch, cellulose, alginic acid, hyaluronic acid and chitosan; the polypeptide hydrophilic polymer is selected from one or more of collagen, poly-L-lysine and poly-L-glutamic acid; and / or The synthetic hydrophilic polymer is selected from polyacrylic acid and its derivative hydrophilic polymers.

4. The composite diaphragm according to claim 1, It is characterized in that The hydrogel coating has one or more of the following characteristics: The single-side thickness of the hydrogel coating is 1-200 μm; The ratio of the length of the hydrogel coating to the length of the diaphragm substrate layer is 0.1%-100%, for example 0.5%-5%; The length of the hydrogel coating is 0.01-0.5 m; The hydrogel coating extends along the length direction of the diaphragm substrate layer, and the width of the hydrogel coating is consistent with the width of the diaphragm substrate; The hydrogel coating is located at an end of the separator substrate layer.

5. The composite diaphragm according to claim 1, It is characterized in that The binder is selected from one or more of polyvinylidene fluoride, carboxymethyl cellulose and styrene-butadiene rubber; and / or In the hydrogel coating, the mass ratio of the binder to the hydrophilic polymer hydrogel is 1:(10-20).

6. The composite diaphragm according to claim 1, It is characterized in that The composite diaphragm further includes a ceramic coating layer, which is located on at least one surface of the diaphragm substrate layer, and comprises a ceramic material and a binder.

7. The composite diaphragm according to claim 6, It is characterized in that in, The ceramic coating has one or more of the following characteristics: The ceramic material is Al 2 O 3 and / or TiO 2 ; The binder is selected from one or more of polyvinylidene fluoride, carboxymethyl cellulose and styrene-butadiene rubber; In the ceramic coating, the mass ratio of the binder to the ceramic material is 1:(10-20); The ceramic coating extends along the length direction of the diaphragm substrate layer, and the width of the ceramic coating is consistent with the width of the diaphragm substrate layer; The ceramic coating and the hydrogel coating are disposed adjacent to each other along the length direction of the diaphragm substrate layer, and the hydrogel coating is located at a position on the diaphragm substrate where the ceramic coating is not disposed; The single-side thickness of the ceramic coating is 0-5 μm; The length of the ceramic coating is 0.01-10m.

8. A method for preparing a composite diaphragm according to any one of claims 1 to 7, It is characterized in that The method comprises the following steps: Evenly mixing the hydrophilic polymer hydrogel, the binder and water to obtain a hydrogel coating slurry; The hydrogel coating slurry is coated on at least one surface of the membrane substrate and dried to obtain the composite membrane.

9. A lithium ion battery, It is characterized in that The lithium-ion battery comprises the composite separator according to any one of claims 1 to 7.

10. The lithium ion battery according to claim 9, It is characterized in that The lithium-ion battery comprises a battery core formed by winding the composite separator with a positive electrode sheet and a negative electrode sheet, the hydrogel coating exists in the outermost circle of the battery core, and the difference between the outer circumference of the battery core and the length of the hydrogel coating is ≤10 mm.

Citation Information

Patent Citations

  • Lithium ion battery composite isolating membrane

    CN109546063A

  • Diaphragm for water-based zinc ion battery and preparation method of diaphragm

    CN113839144A