Aluminum alloy-based heat exchanger obtained by brazing

By using the core layer, cover layer and interlayer of 6xxx series aluminum alloy with high solid-phase line temperature, combined with brazing temperature control and tempering steps, the mechanical strength, corrosion resistance and ability of aluminum alloys in the prior art are solved after brazing in the prior art. The problem of difficult brazing properties is difficult to balance, and aluminum alloy strips or plates with high yield strength and good corrosion resistance are achieved.

CN119013140AInactive Publication Date: 2024-11-22CONSTELLIUM NEUF BRISACH SAS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202380033852.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-19
Filing Date
2023-04-18
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

It is difficult to achieve a balance between good mechanical strength, corrosion resistance and brazability after brazing of existing aluminum alloys. Especially when the solid phase line temperature of the core layer is high, it is difficult to melt the brazing layer at the same time without melting the core. layer problem.

Method used

Using a core layer made of 6xxx series aluminum alloy, combining high solid-phase line temperature and appropriate cover and interlayer, the temperature control and cooling rate optimization during the brazing process is increased to increase the post-brazing tempering step to improve mechanical strength , while maintaining corrosion resistance and brazability.

Benefits of technology

The yield strength of the industrial strip or sheet after brazing is achieved to reach 130MPa or above, meeting the high mechanical performance requirements of battery coolers for electric vehicles, while maintaining good corrosion resistance and brazability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013140A_ABST
    Figure CN119013140A_ABST
Patent Text Reader

Abstract

The invention relates to a strip or sheet intended for manufacturing a brazed heat exchanger, comprising a core layer 18, optionally a cover layer 16, 17 on one or both sides of the core layer 18, and optionally an interlayer on one or both sides of the core layer 18, said interlayer being interposed between the core layer 18 and the cover layer 16, 17, said core layer 18 being made of an aluminum alloy of the 6xxx series, the 6xxx series aluminum alloy has the following composition: Si: 0.45 to 0.75 wt%; 0.18 to 0.40 wt% of Fe; cu: 0.40 wt% or less; mn: 0.30 wt% or less; mg: 0.25 to 0.56 wt%; ti: lt; 0.050% by weight; optionally V: 0.05 to 0.16 wt%; inevitable impurities: 1t of each; 0.05 wt% and the total lt; 0.15% by weight; and the balance of aluminum.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to thin strips or plates (thickness typically 0.1 to 2.5 mm) made of an aluminum-magnesium-silicon core alloy (6xxx series according to the nomenclature of the Aluminum Association), possibly coated on one or both surfaces with a covering alloy, most often an aluminum-silicon brazing alloy (4xxx series according to the nomenclature of the Aluminum Association) or a sacrificial aluminum alloy, aluminum-manganese or aluminum-zinc (1xxx, 3xxx or 7xxx series according to the nomenclature of the Aluminum Association), and / or coated with an interlayer alloy, which is aluminum or an aluminum-manganese alloy (1xxx or 3xxx series according to the nomenclature of the Aluminum Association), between the core layer and the possible brazing alloy. In particular, these strips or plates are intended for use in the manufacture of components such as plates for heat exchangers assembled by brazing, in particular coolers for batteries of motor vehicles, such as electric vehicles. For example, the brazing technology of aluminum alloys is described in the article "Le brasage fort de l'aluminium et sesalliages" by JC Cucza, A. Uhry and JC Guussain (published in Soudage et Techniques Connexes, November-December 1991, pages 18-29). In particular, the strip or sheet according to the present invention can be used for brazing aluminum alloys using Brazing techniques with non-corrosive fluxes of the CAB (“controlled atmosphere brazing”) or type. Background Art

[0002] With the development of electric vehicles, the battery cooler market is expanding rapidly. The current goal of this component is to control the operating temperature of the battery typically between 20 and 100° C., preferably between 30 and 80° C. This component may be of large size (1 to 2 meters).

[0003] Figure 1An example of an existing design of an electric vehicle battery cooler is shown. It consists of two parts with a core layer 15 made of a 3xxx series alloy: a flat plate component 11 and a stamped component 12, which are assembled to establish a channel 13. In this specification, the term "flat plate component" refers to a component that is not stamped before assembly. On the other hand, the term "stamped component" refers to a component that is stamped before assembly so as to establish a channel after assembly with a flat plate component. In operation, the channel is used for the circulation of coolant in an electric vehicle battery cooler. In addition to the core layer 15 made of a 3xxx series alloy, a sacrificial layer 16 made of, for example, a 7xxx series or 1xxx series alloy may be added to ensure corrosion resistance SWAAT on the outer surface of each of the two components 11 and 12. The stamped component 12 also includes a brazing layer 17 made of a 4xxx series alloy, which is located on the other side of the core layer 15 made of a 3xxx series alloy relative to the sacrificial layer 16 to ensure that the two components 11 and 12 are brazed together. The battery 14 is in contact with the flat plate component 11, but not with the stamped component 12.

[0004] Specifically, the properties required of aluminum alloy strips or plates for manufacturing brazed exchangers include: sufficient formability so that the plate can be easily formed before brazing; good brazing; high mechanical strength after brazing so that the smallest possible thickness can be used and the partial strength of the overall structure of the battery box can be ensured; good fatigue stress resistance during operation; good corrosion resistance after brazing. Of course, it is important that the selected alloy is easy to cast and roll, and the manufacturing cost of the strip or plate is compatible with the requirements of the vehicle industry.

[0005] In order to facilitate the reduction of the thickness of heat exchanger plates (e.g. coolers for electric vehicle batteries, which may also be used as structural components), it is of particular interest to improve the mechanical properties of the material after brazing, in particular the yield strength (Rp) of the tensile strength curve obtained according to standard ISO 6892-1. 0.2 ) (“Yield Strength” or “YS” in English) without reducing corrosion resistance or brazeability.

[0006] In this regard, solutions have already been proposed. For example, the following patents and patent applications can be mentioned, which disclose the compositions and structures below:

[0007] - JP 2005 / 261026 discloses a core body, in particular for a tube, made of a 3xxx series alloy, said alloy comprising, in percentage by weight: >0.8% Mn; 0.3-0.6% Mg; <0.5% Si.

[0008] - EP1254965 discloses a structurally hardened aluminium alloy having the following composition (in wt%): 0.6-0.9% Si; 0.1-0.36% Mg; 0.4-0.7% Mn; 0.1-0.25% Ti; 0.25-0.35% Cu; <0.7% Fe; optionally 0.05-0.25% Zr.

[0009] - EP1687456 relates to the field of fluxless brazing and discloses a core comprising (in wt%): 0.3-1.0% Si; <1.0% Fe; 0.3-1.0% Cu; 0.3-2.0% Mn; 0.3-3.0% Mg; <6% Zn; <0.1% Ti; <0.3% Zr; <0.3% Cr; <2.0% Ni; <2.0% Co; <0.5% Bi; <0.5% Y; other elements <0.05% each and <0.15% in total, the remainder being aluminium, at least one surface of which is coated with a brazing aluminium alloy comprising (in wt%): 4-15% Si and 0.01-0.5% of at least one of the elements Ag, Be, Bi, Ce, La, Pb, Pd, Sb, Y or mixed rare earth metals.

[0010] -EP3423607 discloses a solution made from a 6xxx series alloy solution, which contains (in weight %): 0.2-1.3% Si; 0.40-1.3% Mg; ≤0.80% Cu; 0.05-1.0% Fe; 0.05-0.70% Mn; optionally one or two elements selected from 0.05-0.35% Zr and 0.04-0.35% Cr; ≤25% Zn; ≤0.25% Ti; the rest are unavoidable impurities and aluminum, or the Fe / Mn ratio is less than 1.90.

[0011] - WO2021204929 discloses a core made of an AA6xxx series alloy having the following composition (in weight percentage): 0.5-0.9% Si; ≤0.5% Fe; ≤0.5% Cu; ≤0.5% Mn; 0.4-0.8% Mg; ≤0.3% Cr; ≤0.3% Zn; ≤0.3% Ti; ≤0.1% Zr; the remainder being aluminum and unavoidable impurities, with a maximum of 0.05% each and a maximum of 0.15% in total.

[0012] However, the proposed solutions do not necessarily allow to solve the problem of good mechanical strength after brazing (especially Rp 0.2 The problem is to find a good balance between good corrosion resistance and good brazeability, especially when the solidus temperature of the core alloy is high enough to melt the brazing layer while avoiding melting the core layer.

[0013] In view of the growing market demand, there is still a need for a new core alloy having improved mechanical strength (especially in Rp 0.2 Such core alloys may allow meeting the ever-present need to reduce product thickness, as well as the need to develop solutions for battery coolers with high mechanical properties to improve their contribution to the overall strength of the structure protecting the battery (which includes the thermal cooler, integrated or not integrated into the body, and the components encapsulating the battery). Summary of the invention

[0014] Surprisingly, the Applicant has identified a composition range which allows to increase the mechanical strength without reducing the corrosion resistance or the brazeability. For example, the invention may aim at a yield strength Rp of an industrial strip or sheet after brazing of 0.2 Reaching higher than or equal to about 130 MPa, preferably 150 MPa, preferably 180 MPa, or higher than or equal to about 190 MPa, or higher than or equal to about 200 MPa.

[0015] In particular, the solution of the present invention is based on at least one of the following elements, which may be related to the alloy composition of the core layer, the construction of the flat part and the stamped part or the manufacturing method:

[0016] - using a core layer made of a 6xxx series alloy having the composition described in the present invention, preferably maintaining a solidus temperature of, for example, above 615° C., in particular in the case where the core is coated with a brazing layer comprising a 4xxx series aluminum alloy (e.g., AA4343 or AA4045 alloy), the solidus temperature of which is about 577° C. Typically, the solidus temperature of the core layer made of a 6xxx series alloy is preferably at least 20° C., preferably at least 30° C., preferably at least 40° C. relative to the solidus temperature of the brazing layer;

[0017] - For the plate part 11 of the heat exchanger, sacrificial layers are used on both surfaces of the core layer made of 6xxx series alloy to ensure good corrosion resistance on the outside of the heat exchanger (i.e. the side of the plate part 11 opposite to the side where the stamped part 12 is located).

[0018] - Assembling a flat plate component 11 and another component 12, wherein the flat plate component 11 has a core layer 18 made of a 6xxx series alloy, and a sacrificial layer 16 is plated on both surfaces of the core layer 18); the other component 12 has a core layer 18 made of a 6xxx series alloy, and a brazing layer 17 is plated on one surface of the core layer 18, and a sacrificial layer 16 is plated on the other surface, and the other component 12 is stamped to form a channel 13 between the flat plate component 11 and the stamped component 12, such as Figure 2 After assembly, according to Figure 2In a non-limiting configuration, the brazing layer 17 of the stamped component 12 is located between the core layer 18 of the 6xxx series alloy of the stamped component 12 and a sacrificial layer 16 of the flat component 11. It should be noted that the two core layers 18 or the two sacrificial layers 16 made of the 6xxx series alloy can have the same composition or different compositions. It should also be noted that according to a variation, there can be a sacrificial layer between the core layer 18 and the brazing layer 17 made of the 6xxx series alloy.

[0019] - Brazing, for example in a CAB furnace (brazing performed under a controlled atmosphere, for example controlling the amount of nitrogen or argon and / or oxygen), at a temperature preferably below 615° C., preferably below 610° C., preferably below 605° C. Above 570° C., limiting the amount of oxygen below 100 ppm, preferably below 50 ppm, may allow improving the brazing quality.

[0020] - preferably ensure cooling at the end of the brazing cycle, preferably at a rate higher than 25°C / min, preferably higher than 40°C / min, preferably higher than 50°C / min to below 380°C and up to 100°C. Rapid cooling can allow avoiding or reducing the formation of coarse precipitates (Mg, Si), for example larger than 150 nm, which could reduce the hardening potential of the alloy, in particular Rp 0.2 .

[0021] - optionally adding a post-braze tempering step, preferably at a temperature of 180 to 220°C, preferably for a duration shorter than 6 hours, preferably shorter than 3 hours, preferably shorter than or equal to 2 hours (e.g. 195°C for 2 hours or 205°C for 30 minutes).

[0022] One object of the present invention is therefore a strip or sheet intended for the manufacture of a brazed heat exchanger, preferably an electric vehicle battery cooler, comprising, preferably consisting of: a core layer; possibly a cover layer on one or both surfaces of the core layer; and possibly an interlayer between the core layer and the cover layer on one or both surfaces of the core layer, the core layer being made of an aluminum alloy of the 6xxx series having the following composition (in wt. %):

[0023] -Si: 0.45 to 0.75; preferably 0.50 to 0.70%; preferably 0.55 to 0.65%;

[0024] -Fe: 0.10 to 0.40%; preferably 0.12 to 0.35%; preferably 0.14 to 0.30%; preferably greater than 0.18 to 0.26%;

[0025] - Cu: according to a first variant, ≤0.50%; preferably ≤0.45%; preferably ≤0.25%; preferably ≤0.15%; and preferably >0.05%; or according to a second variant, preferably 0.25 to 0.45%; preferably 0.29 to 0.40%;

[0026] -Mn: ≤0.30%; preferably ≤0.20%; preferably ≤0.15%; preferably ≤0.10%;

[0027] -Mg: 0.25 to 0.56%; preferably 0.25 to 0.45%; preferably 0.30 to 0.39%;

[0028] -Ti: <0.050%; preferably <0.045%; preferably <0.040%;

[0029] -optionally V: 0.05 to 0.16%;

[0030] - Unavoidable impurities: <0.05% each and <0.15% in total;

[0031] -The rest is aluminum.

[0032] Another object of the invention is a set of two sheets or strips, comprising, preferably consisting of, the following components:

[0033] - a flat component formed from the strip or sheet of the invention;

[0034] - stamped parts formed from the strip or sheet material of the invention;

[0035] The two parts are intended to be assembled together by brazing, and the channel is formed due to the deformation of the stamped part, the outermost layer of the stamped part and / or the outermost layer of the flat part in contact with the other part being the brazing layer.

[0036] Another object of the present invention is a method for manufacturing a strip or sheet according to the invention, comprising the following successive steps:

[0037] - casting of plates made of the core alloy;

[0038] - Optionally, homogenizing the plate at a temperature of 450 to 580° C., preferably 520 to 560° C., for 1 to 24 hours;

[0039] - possibly, coating one or both surfaces of the core layer with a covering aluminum alloy, and possibly, coating one or both surfaces of the core layer with an interlayer aluminum alloy;

[0040] - preheating at a temperature of 400 to 550° C., preferably 450 to 530° C., preferably 480 to 510° C., preferably kept at the maximum temperature for a time of less than 30 hours, preferably less than 20 hours, preferably less than 12 hours, more preferably less than 3 hours;

[0041] - hot rolling the possibly homogenized and possibly electroplated sheet at a temperature of 390 to 530° C., preferably 470 to 530° C., to a thickness of 2 to 6 mm,

[0042] - cold rolled to the desired thickness, the thickness of the strip or plate after cold rolling is preferably 0.15 to 3 mm, and

[0043] - Heat treatment in a tunnel furnace at a temperature of 250 to 560°C, preferably 320 to 430°C, preferably 320 to 360°C, wherein the maximum temperature is maintained for a time of less than 5 minutes, preferably less than 1 minute, preferably less than 30 seconds and preferably more than 15 seconds, or in a batch furnace (i.e. a discontinuously operated furnace) at a temperature of 250 to 390°C, preferably 310 to 360°C, wherein the maximum temperature is maintained for a time of preferably less than 3 hours, preferably less than 2 hours and preferably less than 1 hour, to obtain small grain recrystallization.

[0044] Another object of the invention is a heat exchanger at least partially made from a strip or sheet according to the invention, or from a set of two sheets or strips according to the invention.

[0045] A further object of the invention is the use of a strip or sheet material according to the invention or a set of two sheets or strip materials according to the invention for producing a heat exchanger, preferably a battery cooler for an electric vehicle. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] Figure 1 A cross-sectional view illustrating a prior art design of an electric vehicle battery cooler.

[0047] Figure 2 A cross-sectional view illustrating the design of an electric vehicle battery cooler of the present invention.

[0048] Figure 3 This is a diagram illustrating the installation of the plates used in the brazeability test of Example 1.

[0049] Figure 4 The figure describes the installation and penetration analysis in the SWAAT corrosion test of Example 3. DETAILED DESCRIPTION

[0050] In the description and claims, unless otherwise stated:

[0051] - The names of aluminum alloys conform to the nomenclature of the Aluminum Association;

[0052] -The content of chemical elements is expressed as weight percentage.

[0053] Core aluminum alloy

[0054] The composition limits of the 6xxx series aluminum alloy of the core layer used in the present invention are expressed in weight percent and can be explained as follows.

[0055] Silicon: A minimum Si content of 0.45% allows to improve the mechanical properties, in particular by forming hardening precipitates containing magnesium and silicon during tempering after brazing. Therefore, the silicon content is preferably higher than or equal to 0.45%, or higher than or equal to 0.46%, or higher than or equal to 0.47%, or higher than or equal to 0.48%, or higher than or equal to 0.49%, or higher than or equal to 0.50%, or higher than or equal to 0.51%, or higher than or equal to 0.52%, or higher than or equal to 0.53%, or higher than or equal to 0.54%, or higher than or equal to 0.55%.

[0056] Too high Si content will reduce the solidus temperature of the core and impair brazing. Therefore, it is preferred to limit the Si content to less than or equal to 0.75%, or less than or equal to 0.74%, or less than or equal to 0.73%, or less than or equal to 0.72%, or less than or equal to 0.71%, or less than or equal to 0.70%, or less than or equal to 0.69%, or less than or equal to 0.68%, or less than or equal to 0.67%, or less than or equal to 0.66%, or less than or equal to 0.65%.

[0057] Preferably, the Mg / Si weight ratio is from 0.4 to 1.0, preferably from 0.5 to 0.9.

[0058] Iron: A maximum Fe content of 0.40%, or 0.39%, or 0.38%, or 0.37%, or 0.36%, or 0.35%, or 0.34%, or 0.33%, or 0.32%, or 0.31%, or 0.30%, or 0.29%, or 0.28%, or 0.27%, or 0.26% may also be beneficial for corrosion resistance and formability, in particular by reducing the proportion of coarse Fe-containing precipitates. However, it is not necessary to go down to very low contents, such as below 0.08%, which would result in a high cost price. Therefore, a preferred minimum Fe content is 0.10%, or 0.11%, or 0.12%, or 0.13%, or 0.14%, or 0.15%, or 0.16%, or 0.17%, or 0.18%.

[0059] Copper: Copper is a hardening element which contributes to the mechanical strength. When an additional layer is present, a copper gradient is created during brazing and has the effect of reducing corrosion on the inside of the exchanger, i.e. on the side of the fluid circulation channels. However, above a given content, the risk of crack formation during casting is higher and the susceptibility of the core to corrosion may increase. Coarse intermetallic compounds may also be formed during casting, which change the homogeneity of the metal and may constitute a starting point for corrosion. Copper is also an element that lowers the solidus temperature. Therefore, the Cu content is lower than or equal to 0.50%, or lower than or equal to 0.49%, or lower than or equal to 0.48%, or lower than or equal to 0.47%, or lower than or equal to 0.46%, or lower than or equal to 0.45%, or lower than or equal to 0.40%, or lower than or equal to 0.35%, or lower than or equal to 0.30%, or lower than or equal to 0.25%, or lower than or equal to 0.20%, or lower than or equal to 0.15%. Preferably, the Cu content is higher than 0.05%, or higher than or equal to 0.20%, or higher than or equal to 0.21%, or higher than or equal to 0.22%, or higher than or equal to 0.23%, or higher than or equal to 0.24%, or higher than or equal to 0.25%, or higher than or equal to 0.26%, or higher than or equal to 0.27%, or higher than or equal to 0.28%, or higher than or equal to 0.29%.

[0060] Manganese: Adding Mn can allow the solidus to be increased. For this reason, the Mn content is preferably higher than or equal to 0.01%, or higher than or equal to 0.02%, or higher than or equal to 0.025%, or higher than or equal to 0.03%, or higher than or equal to 0.04%, or higher than or equal to 0.05%, or higher than or equal to 0.06%, or higher than or equal to 0.07%, or higher than or equal to 0.08%, or higher than or equal to 0.09%, or higher than or equal to 0.10%. To avoid the formation of a large amount of coarse phases (which can reduce formability) and dispersoids (which can deteriorate hardenability during brazing cooling) during the casting process, which become sites for the occurrence of Mg-containing precipitates, it is recommended to limit the amount of Mn to less than or equal to 0.30%, or less than or equal to 0.29%, or less than or equal to 0.28%, or less than or equal to 0.27%, or less than or equal to 0.26%, or less than or equal to 0.25%, or less than or equal to 0.24%, or less than or equal to 0.23%, or less than or equal to 0.22%, or less than or equal to 0.21%, or less than or equal to 0.20%, or less than or equal to 0.19%, or less than or equal to 0.18%, or less than or equal to 0.17%, or less than or equal to 0.16%, or less than or equal to 0.15%, or less than or equal to 0.14%, or less than or equal to 0.13%, or less than or equal to 0.12%, or less than or equal to 0.11%, or less than or equal to 0.10%. To maximize mechanical properties, especially Rp 0.2, it is preferred to limit the amount of Mn to less than or equal to 0.10%.

[0061] Magnesium: The present invention controls the Mg content so as to be able to braze together two parts (a flat part and a stamped part), each of which has a core made of an aluminum from the 6xxx series. The situation would be different if one of the two cores was made of an aluminum alloy from the 3xxx series. Mg is an element that, in combination with silicon, allows structural hardening to occur during post-braze tempering. In addition, the minimum Mg content of the present invention is preferably greater than or equal to 0.25%, or greater than or equal to 0.26%, or greater than or equal to 0.27%, or greater than or equal to 0.28%, or greater than or equal to 0.29%, or greater than or equal to 0.30%, or greater than or equal to 0.31%, or greater than or equal to 0.32%, or greater than or equal to 0.33%. Furthermore, the maximum Mg content of the present invention is preferably lower than or equal to 0.56%, or lower than or equal to 0.55%, or lower than or equal to 0.54%, or lower than or equal to 0.53%, or lower than or equal to 0.52%, or lower than or equal to 0.51%, or lower than or equal to 0.50%, or lower than or equal to 0.49%, or lower than or equal to 0.48%, or lower than or equal to 0.47%, or lower than or equal to 0.46%, or lower than or equal to 0.45%, or lower than or equal to 0.44%, or lower than or equal to 0.43%, or lower than or equal to 0.42%, or lower than or equal to 0.41%, or lower than or equal to 0.40%, or lower than or equal to 0.39%.

[0062] Titanium: Ti allows the grain size to be controlled during casting. Preferably, according to the present invention, its content is less than 0.050%, or less than 0.049%, or less than 0.048%, or less than 0.047%, or less than 0.046%, or less than 0.045%, or less than 0.044%, or less than 0.043%, or less than 0.042%, or less than 0.041%, or less than 0.040%.

[0063] Vanadium: Vanadium may be optionally added to ensure supplementary hardening and to increase the solidus temperature of the alloy. If its content exceeds 0.16%, primary grains may form during casting. Preferably, according to the invention, its content is lower than 0.16%, or lower than 0.15%, or lower than 0.14%, or lower than 0.13%, or lower than 0.12%, or lower than 0.11%, or lower than 0.10%. Preferably, when the latter is added, the minimum content of V is 0.05%.

[0064] Preferably, the solidus temperature of the 6xxx series aluminum of the core layer is higher than 595° C., preferably higher than 600° C., preferably higher than 605° C., preferably higher than 610° C., preferably higher than 615° C. Preferably, the solidus temperature of the core layer made of the 6xxx series alloy is at least 20° C., preferably at least 30° C., preferably at least 40° C. relative to the solidus temperature of the brazing layer. The solidus temperature of the 6xxx series aluminum of the core layer should be adjusted according to the brazing conditions in a manner known to a person skilled in the art.

[0065] It should be noted that the 6xxx series aluminum alloy of the core layer of the flat plate component and the stamped component can be the same alloy or two different alloys, preferably the same alloy.

[0066] Covering aluminum alloy

[0067] According to the present invention, the cover layer may be a sacrificial layer or a brazing layer.

[0068] Sacrificial layer:

[0069] According to a variant of the invention, the strip or sheet comprises a covering layer which is a sacrificial layer 16 on at least one surface of the core layer 18. Preferably, the aluminium alloy of the sacrificial layer 16 contains less than 2.50 wt. %, preferably at least 0.50 wt. % Zn.

[0070] According to a variant of the invention, the aluminium alloy of the sacrificial layer is selected from aluminium alloys of the 1xxx, 7xxx or 3xxx series, preferably from aluminium alloys of the 7xxx or 3xxx series.

[0071] According to one variant, the aluminum alloy of the sacrificial layer may be an aluminum alloy of the 7xxx series, preferably having the following composition (in weight percentage): less than 0.50% Si; less than 0.50% Fe; less than 0.25% Cu; less than 0.30% Mn; less than 0.20%, preferably less than 0.15% Mg; 0.70 to 5.00%, preferably 0.70 to less than 4.50%, according to one variant 0.50 to less than 2.50%, preferably 0.70 to less than 2.50%, preferably greater than 0.80 to less than 1.30% Zn; less than 0.15% Ti; other elements each less than 0.05%, less than 0.15% in total; the rest is aluminum.

[0072] For example, the AA7072 composition is an aluminum alloy that can be used as the sacrificial layer of the present invention. Its composition is as follows by weight percentage: less than 0.05% Si; less than 0.05% Fe; less than 0.10% Cu; less than 0.10% Mn; less than 0.10% Mg; 0.80 to 1.30% Zn; other elements are less than 0.05% each and less than 0.15% in total; the rest is aluminum.

[0073] According to another variant, the aluminum alloy of the sacrificial layer may be an aluminum alloy of the 3xxx series, preferably having the following composition (in weight percentage): 0.10 to 0.35% Si; less than 0.70% Fe; less than 0.20% Cu; 0.70 to 2.00%, preferably 0.90 to 1.30% Mn; 0.70 to 5.00%, preferably 0.70 to less than 4.50%, preferably 0.70 to less than 2.50%, preferably more than 0.80 to less than 1.30% Zn; less than 0.15% Ti; other elements are each less than 0.05% and the total is less than 0.15%; the rest is aluminum.

[0074] Preferred values ​​(in weight percent) for the elements in 3xxx series or 7xxx series alloys that may be suitable for use as sacrificial anodes in the present invention are given as examples in Table 1 below (columns 3xxx-1, 7xxx-1 and 7xxx-2).

[0075] [Table 1]

[0076]

[0077] Brazing layer:

[0078] Preferably, the aluminum alloy of the brazing layer is an aluminum alloy of the 4xxx series, whose liquidus temperature is sufficiently low compared to the solidus of the core alloy, so as to have a sufficient brazing temperature range, acceptable mechanical strength and good wettability. These alloys may contain additive elements, such as strontium, preferably with a weight content of less than 0.05%.

[0079] According to a variant, the brazing alloy of the invention comprises Y, Sn and / or Bi. In particular, this variant facilitates fluxless brazing. Preferably, the brazing alloy comprises:

[0080] - 0.01 to 0.10%, preferably 0.015 to 0.08%, preferably 0.02 to 0.065% Y;

[0081] - 0.01 to 0.10%, preferably 0.015 to 0.08%, preferably 0.02 to 0.065% Sn; and / or

[0082] - according to a first variant, at most 0.04%, preferably at most 0.03%, preferably at most 0.02% Bi; or according to a second variant, at most 0.15%, preferably at most 0.12%, preferably less than 0.10% and preferably at least 0.05%, preferably more than 0.06% Bi.

[0083] Preferably, the brazing layer aluminum alloy does not contain Bi.

[0084] Preferably, the brazing layer aluminum alloy is a 4xxx series alloy containing 4.00 to 13.00 wt. % Si and less than 1.00 wt. % Fe.

[0085] Preferably, the brazing layer aluminum alloy of the 4xxx series comprises (in weight %):

[0086] - Si: 5.00 to 13.00%, preferably 6.00 to 11.00%;

[0087] - Fe: less than 0.60%, preferably less than 0.50%, preferably less than 0.30%;

[0088] -Cu: less than 0.40%, preferably less than 0.10%, preferably less than 0.05%;

[0089] - Mn: less than 0.20%, preferably less than 0.10%, preferably less than 0.05%;

[0090] Mg: according to a first variant, less than 0.20%, preferably less than 0.10%, preferably less than 0.05%; or according to a second variant, from 0.50 to 2.50%, preferably from 1.00 to 2.00%;

[0091] - Zn: less than 0.20%, preferably less than 0.10%, preferably less than 0.05%, preferably less than 0.02%;

[0092] -Ti: less than 0.30%, preferably less than 0.10%, preferably less than 0.05%;

[0093] - may contain Bi, Y, Sr and / or Sn;

[0094] - Other elements: less than 0.05% for each element and less than 0.15% for the total amount;

[0095] -The rest is aluminum.

[0096] For example, the AA4045 composition is an aluminum alloy that may be suitable for use as the brazing layer alloy of the present invention. Its composition is, by weight percentage, 9.0 to 11.0% Si, less than 0.80% Fe, less than 0.30% Cu, less than 0.05% Mn, less than 0.05% Mg, less than 0.10% Zn, less than 0.20% Ti, other elements are less than 0.05% each, less than 0.15% in total, and the rest is aluminum.

[0097] For example, the former composition preferably contains less than 0.60% Fe.

[0098] For example, the former composition preferably contains less than 0.10% Cu.

[0099] For example, the AA4343 composition is an aluminum alloy that may be suitable for use as the brazing alloy of the present invention. Its composition is, by weight percentage, 6.80% to 8.20% Si, less than 0.80% Fe, less than 0.25% Cu, less than 0.10% Mn, less than 0.05% Mg, less than 0.05% of each other element and less than 0.15% in total, and the rest is aluminum.

[0100] For example, the former composition preferably contains less than 0.30% Fe.

[0101] For example, the former composition preferably contains less than 0.10% Cu.

[0102] For example, the AA4004 composition is an aluminum alloy that may be suitable for use as the brazing alloy of the present invention. Its composition is, by weight percentage, 9.00 to 10.50% Si, less than 0.80% Fe, less than 0.25% Cu, less than 0.10% Mn, 1.00 to 2.00% Mg, less than 0.20% Zn, less than 0.05% each of the other elements and less than 0.15% in total, and the remainder is aluminum.

[0103] For example, the AA4104 composition is an aluminum alloy that may be suitable for use as the brazing alloy of the present invention. Its composition is, by weight percentage, 9.00 to 10.50% Si, less than 0.80% Fe, less than 0.25% Cu, less than 0.10% Mn, 1.00 to 2.00% Mg, less than 0.20% Zn, 0.02 to 0.20% Bi, other elements each less than 0.05% and less than 0.15% in total, and the remainder is aluminum.

[0104] Laminated aluminum alloy

[0105] According to one embodiment, the strip or sheet of the invention is electroplated, on one or both surfaces of the core layer, with a so-called sandwich aluminium alloy, preferably with a sandwich aluminium alloy of the 1xxx or 3xxx series, placed between the core layer and a covering layer, preferably a brazing layer, preferably comprising (in wt. %):

[0106] - Si: less than 0.50%, more preferably less than 0.20%;

[0107] - Fe: less than 0.70%, more preferably less than 0.30%, even more preferably less than 0.20%;

[0108] - Mn: 0.30 to 1.40%, more preferably 0.50 to 0.90%, more preferably 0.60 to 0.80% or, according to a variant, 1.00 to 1.30%;

[0109] - Cu: less than 0.30%, preferably less than 0.10%, even more preferably less than 0.05%;

[0110] - may contain Mg, Zn and / or In;

[0111] - Other elements < 0.05% each and < 0.15% in total;

[0112] -The rest is aluminum.

[0113] Preferably, the aluminum sandwich alloy of the strip or plate according to the invention comprises (in weight %): Si<0.15%; Fe<0.20%; Cu<0.10%; Mn is 0.60 to 0.80%; Mg<0.02% according to the first variant, or Mg<0.50% according to the second variant, preferably <0.25%; other elements each <0.05% and a total of <0.15%, the remainder being aluminum.

[0114] Preferably, the interlayer aluminum alloy is an AA3xxx series alloy.

[0115] According to a variation, the sandwich aluminum alloy may further comprise:

[0116] - a Zn content of 1.5 to 2.3%; and / or

[0117] - In content of 0.005 to 0.04%.

[0118] According to a variant, only in the case where the cover layer is a brazing layer, the strip or sheet of the invention comprises an interlayer situated between the core and the cover layer.

[0119] According to a variant, the strip or sheet of the invention comprises no interlayer.

[0120] Strips or plates and sets of two strips or plates

[0121] Strip or plate:

[0122] The strip or sheet of the invention is a so-called brazing strip or sheet, which can be used for manufacturing different parts of heat exchangers, such as tubes, plates, manifolds, battery cooling systems for electric vehicles, etc.

[0123] The strip or sheet material according to the invention can have a multi-layer construction, in particular a 2-layer, 3-layer, 4-layer or 5-layer construction.

[0124] The two-layer construction comprises a core layer, a single surface of which is coated with a covering layer, in particular a brazing layer or a sacrificial layer.

[0125] The three-layer structure may include:

[0126] - alternatively, a core layer, with a brazing layer plated on both surfaces of the core layer;

[0127] - alternatively, a core layer, with sacrificial layers coated on both surfaces of the core layer;

[0128] - alternatively, a core layer, on a single surface of which an interlayer is coated, the interlayer itself being coated with a brazing layer or a sacrificial layer, preferably a brazing layer;

[0129] - or a core layer, on a first surface of which a brazing layer is applied and on another surface of which a sacrificial layer is applied.

[0130] The four-layer construction may include:

[0131] - alternatively, a core layer, on a first surface of which a sandwich layer is coated, the sandwich layer itself being coated with a brazing layer or a sacrificial layer, preferably a brazing layer, and on another surface being coated with a brazing layer;

[0132] Alternatively, a core layer, on a first surface of which a sandwich layer is coated, the sandwich layer itself being coated with a solder layer or a sacrificial layer, preferably a solder layer, and on another surface being coated with a sacrificial layer.

[0133] The five-layer construction comprises a core layer coated on both surfaces with an interlayer, which itself is coated with a braze layer or a sacrificial layer, preferably a braze layer.

[0134] In each of the above configurations, when two brazing layers, two interlayers or two sacrificial layers are provided, they may be identical or different in composition. Preferably, the layers are identical in composition.

[0135] The preferred structure is a three-layer structure, including:

[0136] - alternatively, a core layer, with sacrificial layers coated on both surfaces of the core layer;

[0137] - Alternatively, a core layer having a sacrificial layer coated on one surface and a brazing layer coated on the other surface.

[0138] According to a variant, there may be at least one interlayer between the core layer and the sacrificial layer or brazing layer. Preferably, however, no interlayer is present in the strip or sheet of the invention.

[0139] Preferably, the strip or plate of the present invention consists of: a core layer made of a 6xxx series aluminum alloy; a covering layer located on one or both surfaces of the core layer; and possibly, an interlayer located between the core layer and the covering layer on one or both surfaces of the core layer.

[0140] According to a first variant, the strip or sheet of the invention comprises a covering layer on a single surface of the core layer, and:

[0141] - the covering layer is a brazing layer; or

[0142] - The cover layer is a sacrificial layer.

[0143] According to a second variant, the strip or sheet according to the invention comprises covering layers on both surfaces of the core layer, and:

[0144] - one covering layer is a sacrificial layer and the other covering layer is a brazing layer; or

[0145] - Both covering layers are sacrificial layers; or

[0146] - Both covering layers are brazing layers.

[0147] As for the total thickness of the strip or sheet of the present invention, it is preferably 0.40 to 2.50 mm.

[0148] The thicknesses discussed here correspond to the thickness before brazing. With regard to the thickness of the individual layers, it should be noted that these are target values ​​and that a margin of error of about 2% is generally accepted in the field of coated sheets or strips for heat exchangers.

[0149] According to a first variant, in which the strip or sheet of the invention is intended for the manufacture of flat parts, the minimum overall thickness of the strip or sheet is 1.05 mm, or 1.15 mm, or 1.25 mm, or 1.35 mm, or 1.45 mm, or 1.55 mm, or 1.65 mm, or 1.75 mm, or 1.85 mm or 1.95 mm. According to this first variant, the maximum overall thickness of the strip or sheet is preferably 2.50 mm, or 2.40 mm, or 2.30 mm, or 2.20 mm, or 2.10 mm.

[0150] According to a second variant, wherein the strip or sheet of the present invention is intended to be used for manufacturing stamped parts, the minimum overall thickness of the strip or sheet is 0.50 mm, or 0.60 mm, or 0.70 mm, or 0.80 mm, or 0.90 mm. According to this second variant, the maximum overall thickness of the strip or sheet is preferably 2.50 mm, or 2.30 mm, or 2.10 mm, or 1.90 mm, or 1.70 mm, or 1.50 mm, or 1.30 mm, or 1.10 mm.

[0151] As for the thickness of the interlayer or sacrificial layer, it is preferably 4% to 15% of the total thickness of the strip or sheet of the present invention. Preferably, the minimum thickness of the interlayer or sacrificial layer is 5%, or 6%, or 7%, or 8%, or 9% of the total thickness of the strip or sheet of the present invention. Preferably, the maximum thickness of the interlayer or sacrificial layer is 14%, or 13%, or 12%, or 11% of the total thickness of the strip or sheet of the present invention.

[0152] As for the thickness of the brazing layer, it is preferably 3% to 15% of the total thickness of the strip or sheet of the present invention. Preferably, the minimum thickness of the brazing layer is preferably 4% of the total thickness of the strip or sheet of the present invention. Preferably, the maximum thickness of the brazing layer is 14%, or 13%, or 12%, or 11%, or 10%, or 9%, or 8%, or 7%, or 6% of the total thickness of the strip or sheet of the present invention.

[0153] Kit of two sheets or strips:

[0154] The sheets or strips of the invention can be combined together, possibly after forming, to form a heat exchanger with channels. A set of two sheets or strips of the invention can be a set after assembly but before brazing, or a set after brazing. Brazing does not change the construction, i.e. the sequence of the different layers and the relative position of the flat parts with respect to the stamped parts.

[0155] According to the invention, the set of two sheets or strips comprises, preferably consists of, the following components:

[0156] - a flat component formed from the strip or sheet of the invention;

[0157] - stamped parts formed from the strip or sheet material of the invention;

[0158] The two parts are intended to be assembled together by brazing, and the channel is formed due to the deformation of the stamped part, the outermost layer of the stamped part and / or the outermost layer of the flat part in contact with the other part being the brazing layer.

[0159] The set of two sheets or strips according to the invention can have different variants.

[0160] According to a preferred first variant:

[0161] - a component, a flat component or a stamped component, consisting of a core according to the invention, which is coated with a sacrificial layer on both surfaces, and

[0162] Another component, a flat or stamped component, consisting of a core according to the invention coated on one surface with an optional interlayer and a brazing layer and on the other surface with a sacrificial layer.

[0163] According to a second preferred variant, both parts (the flat part and the stamped part) consist of a core according to the invention coated on one surface with the optional interlayer and the brazing layer and on the other surface with a sacrificial layer.

[0164] In each of the above variations, the brazing layer of at least one component is located between the flat component and the stamped component.

[0165] method

[0166] Another object of the present invention is a method for manufacturing a strip or sheet according to the invention, comprising the following successive steps:

[0167] - casting of plates made of the core alloy;

[0168] - Optionally, homogenizing the plate at a temperature of 450 to 580° C., preferably 520 to 560° C., for 1 to 24 hours;

[0169] - the core layer may be plated with a covering aluminum alloy on one or both surfaces, and the core layer may be plated with an interlayer aluminum alloy on one or both surfaces;

[0170] - preheating at a temperature of 400 to 550° C., preferably 450 to 530° C., preferably 480 to 510° C., preferably kept at the maximum temperature for a period of less than 30 hours, preferably less than 20 hours, preferably less than 12 hours, more preferably less than 3 hours;

[0171] - hot rolling the possibly homogenized and possibly electroplated sheet at a temperature of 390 to 530° C., preferably 470 to 530° C., to a thickness of 2 to 6 mm,

[0172] - cold rolled to a desired thickness, the thickness of the cold rolled strip or plate preferably being 0.15 to 3 mm, and

[0173] - Heat treatment in a tunnel furnace at a temperature of 250 to 560°C, preferably 320 to 430°C, preferably 320 to 360°C, wherein the maximum temperature is maintained for less than 5 minutes, preferably less than 1 minute, preferably less than 30 seconds and preferably more than 15 seconds, or in a batch furnace at a temperature of 250 to 390°C, preferably 310 to 360°C, wherein the maximum temperature is maintained for preferably less than 3 hours, preferably less than 2 hours and preferably less than 1 hour, to obtain small grain recrystallization.

[0174] Specifically, the covering alloy of the method of the present invention can be a brazing alloy, or a sacrificial layer, or two brazing alloys, or two sacrificial layers, or a brazing alloy and a sacrificial layer.

[0175] Preferably, there is no intermediate annealing during the rolling step in the method of the invention.

[0176] Before any coating material is installed, the alloy plate of the core layer may be homogenized at a temperature of 450 to 580° C., preferably 520 to 560° C., preferably for 1 to 24 hours.

[0177] use

[0178] Another object of the invention is a heat exchanger at least partially made of a strip or sheet according to the invention, or of a set of sheets or strips according to the invention.

[0179] A further object of the invention is the use of a strip or sheet according to the invention or a set of two strips or sheets according to the invention for producing a heat exchanger, preferably a battery cooler for an electric vehicle.

[0180] The strip or sheet of the invention can be used for producing brazed heat exchangers, in particular brazed heat exchangers for motor vehicles, such as engine cooling radiators, evaporators, heating radiators and charge air coolers, manifolds, battery coolers for electric vehicles and air conditioning systems.

[0181] Specifically, the manufacture of the heat exchanger of the present invention may include at least one of the following steps:

[0182] - brazing in a CAB furnace (controlled atmosphere), preferably at a temperature of 590 to 615° C., preferably 590 to 610° C., preferably 590 to 605° C., preferably 590 to 600° C.;

[0183] - ensuring cooling at the end of the brazing cycle, preferably at a rate higher than 25°C / min, preferably higher than 35°C / min, preferably higher than 50°C / min, to below 380°C and to a maximum of 100°C;

[0184] - A post-braze tempering step is carried out at a temperature of 150 to 240°C, preferably 180 to 220°C, for a duration preferably shorter than 6 hours, preferably shorter than 3 hours, preferably shorter than or equal to 2 hours (for example at about 195°C for 2 hours or at 205°C for 30 minutes). Preferably, the minimum temperature of the post-braze tempering is higher than 180°C, or higher than or equal to 181°C, or higher than or equal to 182°C, or higher than or equal to 183°C, or higher than or equal to 184°C, or higher than or equal to 185°C, or higher than or equal to 186°C, or higher than or equal to 187°C, or higher than or equal to 188°C, or higher than or equal to 189°C, or higher than or equal to 190°C. An increase in the temperature of the post-braze tempering may allow reducing the duration of this tempering. For example, for a post-braze tempering temperature higher than or equal to 185°C, the duration may be shorter than 4 hours.

[0185] Example

[0186] Embodiment 1: Brazing

[0187] Different aluminum alloy ingots for core layer, brazing layer and sacrificial layer were cast using a vertical semi-continuous casting (DC casting) method using aluminum alloys having the compositions given in Table 2 below, in weight percentage:

[0188] Table 2

[0189]

[0190] Before assembling the different layers together:

[0191] - The core aluminum alloy ingot is homogenized (temperature greater than 530°C, time greater than 2 hours and less than 24 hours) and hot rolled at a temperature of 380 to 500°C to a thickness of about 30 mm;

[0192] - The brazing layer alloy ingot is stripped of the surface layer, and then hot rolled at a temperature of about 480-500°C to a thickness of 1.8 mm;

[0193] - The sacrificial layer alloy ingot is hot rolled at a temperature of about 480-500°C to a thickness of about 3.5 mm.

[0194] After brushing the contact surface, a sandwich with a thickness of 35.3 mm was produced, which had the following structure: brazing layer / core layer / sacrificial layer. The brazing layer was about 5% of the total thickness of the sandwich, and the sacrificial layer was about 10% of the total thickness of the sandwich.

[0195] The following two sandwiches were made:

[0196] - Structure-1: Brazing layer-1 / core layer-1 / sacrificial layer;

[0197] - Structure-2: Brazing layer-1 / core layer-2 / sacrificial layer.

[0198] Subsequently, the sandwich is preheated to a temperature of about 490° C. for a period of less than 5 hours and then hot rolled to a thickness of about 1.5 mm or about 0.8 mm.

[0199] Annealing was performed at about 360° C. for 2 hours.

[0200] The sandwich with a thickness of about 0.8 mm is punched to form two lines and obtain a punched plate, such as Figure 3 The sandwich layer with a thickness of about 1.5 mm was not punched to obtain a non-punched plate or a flat plate.

[0201] Subsequently, the brazing properties of the different sandwiches were evaluated. Brazing tests were carried out according to the following protocol, which allows simulating assembly brazing between stamped and non-stamped sheets. For this purpose, 50 mm × 60 mm sheets were punched without lubricant to add two longitudinal punching lines 3, as Figure 3 As shown. Subsequently, the stamped and non-stamped plates were degreased using an acetone solution and then air dried. Figure 3 As shown, the stamped plates and non-stamped plates having the same structure and composition are assembled. Figure 3, reference number 1 corresponds to a stamped sheet, reference number 2 corresponds to a non-stamped sheet, reference number 3 corresponds to two stamped lines, reference number 16 corresponds to a sacrificial layer, reference number 17 corresponds to a brazing layer made of a 4xxx series aluminum alloy, and reference number 18 corresponds to a core made of a 6xxx series aluminum alloy. Subsequently, 0, 2, or 5 g / m 2 of The assembled panels were brazed flat with a type flux on the brazing layer 17. The brazing cycle was performed in a controlled atmosphere (O2 < 50 ppm) at about 600°C for about 2 minutes.

[0202] Subsequently, the length of each brazed joint is measured. For each configuration, three samples are made. For each sample, two measurements are made at the level of the two longitudinal lines of the punching. The results can be expressed in terms of brazed length (in mm) or in terms of percentage of brazed length relative to the maximum possible length. "A" corresponds to more than 90%; "B" corresponds to the interval from 50% to 90%; "C" corresponds to the interval from 10% to less than 50%; "D" corresponds to less than 10%.

[0203] The results of the brazing tests are disclosed in Table 3 below.

[0204] Table 3

[0205]

[0206] All constructions use 5g / m 2 The fluxes have all achieved good brazing properties.

[0207] Embodiment 2: Mechanical properties of three-layer sandwich

[0208] For the samples of Example 1 above (according to the configurations "Configuration-1" and "Configuration-2"), after cold rolling to a thickness of 1.5 mm, different annealings were performed: strip-type annealing (at about 400°C for 30 seconds or at about 550°C for 45 seconds) or intermittent annealing (at about 360°C for 2 hours).

[0209] CAB-type (controlled atmosphere) brazing was performed at about 600°C for about 2 minutes, with cooling to below 380°C and to 100°C at a rate of more than 40°C / min.

[0210] Subsequently, tempering is performed at about 195° C. for 2 hours.

[0211] According to ISO 6892-1 standard, the tensile mechanical properties along the rolling direction were measured after annealing and after annealing + brazing + tempering.

[0212] Table 4

[0213]

[0214] Annealing time and annealing temperature seem to have an effect on Rp after annealing + brazing + tempering 0.2 In all cases, the Rp of the kit 0.2 The Rp of the set with the core made of 6xxx-1 alloy (Construction-1) containing more magnesium is higher than that of the set with the core made of 6xxx-2 alloy (Construction-2). 0.2 High value.

[0215] Embodiment 3: corrosion

[0216] The corrosion resistance of the configurations Configuration-1 and Configuration-2 described in the above Examples 1 and 2 was measured according to the SWAAT test on a sample having a thickness of about 1 mm, on a surface plated with a sacrificial layer, after annealing at about 360°C for 2 hours, then brazing at about 600°C for 2 minutes, and then tempering at about 195°C for 2 hours.

[0217] Corrosion resistance is determined according to the following scheme:

[0218] - Prepare a sample of size 126 mm (L direction) × 90 mm (TL direction) for each configuration, degreased in advance with white absorbent paper soaked in acetone;

[0219] - Protect the untested surface (the surface coated with the solder layer) and the four edges with a width of about 0.5 cm with a transparent vinyl adhesive (e.g. 3M Vinyl Type 764);

[0220] - Clean the surface to be tested (the surface coated with the sacrificial layer) with absorbent paper soaked in acetone;

[0221] - placing the sample thus prepared on a stand inclined at about 60° relative to the horizontal;

[0222] - Each sample was subjected to a SWAAT (Sea Water Acidified Acetic Acid Test) cycle test according to standard ASTM G85A3, notably comprising alternating a 30 minute salt spray phase and a 1 hour 30 minute wetting phase at a temperature of about 49°C.

[0223] The number of perforations in each sample was monitored daily throughout the test period (i.e., 20 days). Figure 4 As shown, perforations are visible on the back of each sample because they would have formed bubbles in the adhesive applied to the untested surface. Figure 4 , reference number 6 corresponds to the sample; reference number 7 corresponds to the adhesive; reference number 8 corresponds to the perforation; and reference number 9 corresponds to the bubble formed by the perforation.

[0224] The results obtained were that after 20 days of testing, no perforations existed in either Configuration-1 or Configuration-2.

[0225] Subsequently, the polished sections of the samples were observed under a microscope, and for both Structure-1 and Structure-2, the pit depth (non-penetration) was less than 60 μm.

[0226] Embodiment 4: Mechanical properties

[0227] Unplated 6xxx series aluminum alloy (see Table 5 below) cores with different compositions were tested with simulated brazing cycles (heating to about 600°C, holding for 2 minutes, then cooling from 380°C and down to 100°C at a rate greater than 50°C / min) and simulated post-braze tempering (several temperatures and holding times were tested - see Table 6 below). Plates made of 6xxx series aluminum alloys were obtained by homogenizing at temperatures greater than 500°C for more than 3 hours, then hot rolling at 350 to 450°C to a thickness of about 2.8 mm, then cold rolling to a thickness of about 0.8 mm, then annealing at 440 to 500°C for 30 to 45 seconds.

[0228] Table 5

[0229]

[0230] According to standard ISO 6892-1, the tensile mechanical properties in the rolling direction after annealing+brazing+tempering were measured and the results are disclosed in Table 6 below.

[0231] Table 6

[0232]

[0233]

[0234] The 6xxx-4 alloy exhibits improved post-braze mechanical properties compared to those of the 6xxx-3 alloy, but the solidus temperature is reduced to 618°C (see Table 6 above).

[0235] Embodiment 5: Mechanical properties

[0236] 6xxx series aluminum alloys with different compositions were cast. Table 7 below shows the element contents of the different alloys in weight percent.

[0237] [Table 7]

[0238]

[0239] The 6xxx series aluminum alloy plates are obtained by homogenizing at a temperature of about 540°C for about 6 hours (except for the B' alloy, which has not been homogenized), then hot rolling at a temperature of about 490°C to a thickness of about 4.5 mm, then cold rolling to a thickness of about 2.0 mm, and then annealing at a temperature of about 360°C for about 2 hours.

[0240] Alloys A to G in Table 7 above were tested with a simulated brazing cycle (heating to about 600°C, holding for 2 minutes, then cooling from 380°C and up to 100°C at a rate greater than 50°C / min) and a simulated post-braze tempering (195°C for 1 hour, 195°C for 4 hours, 205°C for 2 hours or 210°C for 2 hours - see Table 8 below). The oxygen content during the brazing simulation was less than 50 ppm.

[0241] The tensile mechanical properties in the rolling direction after annealing + brazing + tempering were measured according to standard ISO 6892-1. The results obtained are disclosed in Table 8 below, where Rp 0.2 The values ​​of and Rm are expressed in MPa.

[0242] Table 8

[0243]

[0244] On the other hand, the core alloys A, B, F and G sandwiched between the brazing layer-1 of Table 2 above (7.5% of the total thickness of the sandwich) and the sacrificial layer of Table 2 above (10% of the total thickness of the sandwich) were subjected to corrosion resistance tests (not described herein). The SWAAT test was carried out according to standard ASTM G85 A3 (as described in Example 3 above). The results were obtained by microscopic analysis of polished sections after 40 days of testing. The total thickness of the sandwich was about 0.8 mm. It has been noted that the corrosion resistance of the sandwich containing the core alloy F is not as good as that of the sandwich containing the core alloys A, B and G, because a larger pitting depth was observed for the core alloy F.

[0245] Furthermore, it should be noted that the core alloy G contains Fe content that is not very suitable for recycling.

[0246] Embodiment 6: Mechanical properties

[0247] Simulated brazing cycles (heating to about 600°C, holding for 2 minutes, then cooling from 380°C and up to 100°C at a rate greater than 50°C / min) and simulated post-braze tempering (several temperatures and holding times were tested - see Table 10 below) were tested on a plate comprising a core made of a 6xxx series aluminum alloy (6xxx-5 alloy) and plated on both surfaces with a sacrificial layer made of a 7xxx series aluminum alloy (7xxx-1 alloy) - each of the two sacrificial layers representing 10% of the plate thickness. The composition of the aluminum alloy is given in Table 9 below, in weight percent.

[0248] [Table 9]

[0249] Si Fe Cu Mn Mg Zn Ti 6xxx-5 0.62 0.24 0.09 0.16 0.36 0.02 0.03 7xxx-1 0.13 0.3 - - - 1.01 0.03

[0250] The core layer made of 6xxx series aluminum alloy is homogenized at a temperature of 540 to 600°C for more than 3 hours and then assembled with two previously hot-rolled sacrificial layers made of 7xxx series aluminum alloy. The sandwich thus obtained is preheated, then hot-rolled to a thickness of about 4 mm, then cold-rolled to a thickness of about 2 mm, and then annealed at a temperature of about 350°C for about 30 minutes.

[0251] The tensile mechanical properties in the rolling direction were measured after annealing+brazing+tempering according to standard ISO 6892-1. The results obtained are disclosed in Table 10 below.

[0252] [Table 10]

[0253] Tempering time Temperature T°(℃) <![CDATA[Rp 0.2 (MPa)]]> Rm(MPa) A% 4 hours 195 171 208 12.0 1 hour 210 152 191 12.6 45 minutes 225 143 180 14.2

Claims

1. Strip or sheet material intended for the production of a brazed heat exchanger, preferably a battery cooler for an electric vehicle, comprising, preferably consisting of: A core layer (18); possibly, a covering layer (16, 17) on one or both surfaces of the core layer (18); and, possibly, an interlayer on one or both surfaces of the core layer (18), the interlayer being located between the core layer (18) and the covering layers (16, 17), the core layer (18) being made of a 6xxx series aluminum alloy having the following composition, in percentage by weight: -Si: 0.45 to 0.75; preferably 0.50 to 0.70%; preferably 0.55 to 0.65%; -Fe: 0.18 to 0.40%; preferably 0.18 to 0.35%; preferably 0.18 to 0.30%; preferably greater than 0.18 to 0.26%; - Cu: ≤0.40%; preferably ≤0.25%; preferably ≤0.15%; and preferably >0.05% according to the first variant; or preferably 0.25 to 0.40% according to the second variant; preferably 0.29 to 0.40%; -Mn: ≤0.30%; preferably ≤0.20%; preferably ≤0.15%; preferably ≤0.10%; -Mg: 0.25 to 0.56%; preferably 0.25 to 0.45%; preferably 0.30 to 0.39%; -Ti: <0.050%; preferably <0.045%; preferably <0.040%; -optionally V: 0.05 to 0.16%; - Unavoidable impurities: <0.05% each and <0.15% in total; -The rest is aluminum.

2. The strip or plate according to claim 1, characterized in that It consists of the core layer (18) made of 6xxx series aluminum alloy, covering layers (16, 17) on one or both surfaces of the core layer (18), and possibly an interlayer on one or both surfaces of the core layer (18), the interlayer being located between the core layer (18) and the covering layers (16, 17).

3. The strip or plate according to claim 2, characterized in that It comprises a covering layer (16, 17) on one surface of a core layer and is characterized in that: - the covering layer (16, 17) is a brazing layer (17); or The covering layer (16, 17) is a sacrificial layer (16).

4. The strip or plate according to claim 2, characterized in that: It comprises covering layers (16, 17) on both surfaces of a core layer and is characterized in that: - one of the covering layers (16, 17) is a sacrificial layer (16) and the other covering layer (16, 17) is a brazing layer (17); or - Both covering layers (16, 17) are sacrificial layers (16); or - Both covering layers (16, 17) are brazing layers (17).

5. The strip or plate according to any one of claims 2 to 4, characterized in that It comprises a covering layer which is a sacrificial layer (16) on at least one surface of the core layer (18), the aluminum alloy of the sacrificial layer (16) preferably containing less than 2.50 wt. % and preferably at least 0.50 wt. % Zn.

6. The strip or plate according to any one of claims 3 to 5, characterized in that The aluminum alloy of the sacrificial layer (16) is selected from 1xxx, 7xxx or 3xxx series alloys.

7. The strip or plate according to claim 6, characterized in that The aluminum alloy of the sacrificial layer (16) is a 7xxx series alloy, preferably having the following composition, in weight percentage: - less than 0.50% Si; - Fe less than 0.50%; - Less than 0.25% Cu; - less than 0.30% Mn; - less than 0.20%, preferably less than 0.15% Mg; - 0.50 to less than 2.50%, preferably 0.70 to less than 2.50%, preferably more than 0.80 to less than 1.30% Zn; - less than 0.15% Ti; - Other elements are less than 0.05% each and less than 0.15% in total; -The rest is aluminum.

8. The strip or plate according to claim 6, characterized in that The aluminum alloy of the sacrificial layer (16) is a 3xxx series alloy, preferably having the following composition, in weight percentage: - 0.10 to 0.35% Si; - Fe less than 0.70%; - Less than 0.20% Cu; - 0.70 to 2.00%, preferably 0.90 to 1.30% Mn; -0.80 to less than 1.30% Zn; - less than 0.15% Ti; - Other elements are less than 0.05% each and less than 0.15% in total; -The rest is aluminum.

9. The strip or plate according to any one of claims 3 or 4, characterized in that The aluminum alloy of the brazing layer (17) is a 4xxx series alloy, preferably containing 4.00 to 13.00 wt. % Si and less than 1.00 wt. % Fe, and more preferably has the following composition, in weight percentage: - Si: 5.00 to 13.00%, preferably 6.00 to 11.00%; - Fe: less than 0.60%, preferably less than 0.50%, preferably less than 0.30%; -Cu: less than 0.40%, preferably less than 0.10%, preferably less than 0.05%; - Mn: less than 0.20%, preferably less than 0.10%, preferably less than 0.05%; Mg: according to a first variant, less than 0.20%, preferably less than 0.10%, preferably less than 0.05%; or according to a second variant, from 0.50 to 2.50%, preferably from 1.00 to 2.00%; - Zn: less than 0.20%, preferably less than 0.10%, preferably less than 0.05%, preferably less than 0.02%; -Ti: less than 0.30%, preferably less than 0.10%, preferably less than 0.05%; - may contain Bi, Y, Sr and / or Sn; - Other elements: less than 0.05% each and less than 0.15% in total; -The rest is aluminum.

10. A set of two sheets or strips, comprising, preferably consisting of, the following components: - a flat part (11) formed from a strip or sheet according to any of the preceding claims, preferably according to any of claims 2 to 9; - a stamped part (12) formed from a strip or sheet material according to any of the preceding claims, preferably according to any of claims 2 to 9; The two parts are intended to be assembled by brazing and the channel is formed due to the deformation of the stamped part (12), the outermost layer of the stamped part (12) and / or the outermost layer of the flat part (11) in contact with the other part being a brazing layer (17).

11. A method for producing a strip or sheet as claimed in any one of claims 1 to 9, comprising the following consecutive steps: - a cast core alloy plate (18); - optionally homogenizing the plate at a temperature of 450 to 580° C., preferably 520 to 560° C., for 1 to 24 hours; - a covering aluminum alloy (16, 17) may be plated on one or both surfaces of the core layer (18), and an interlayer aluminum alloy may be plated on one or both surfaces of the core layer (18); - preheating at a temperature of 400 to 550° C., preferably 450 to 530° C., preferably 480 to 510° C., preferably kept at the maximum temperature for a time of less than 30 hours, preferably less than 20 hours, preferably less than 12 hours, more preferably less than 3 hours; - hot rolling the possibly homogenized and possibly electroplated sheet at a temperature of 390 to 530° C., preferably 470 to 530° C., to a thickness of 2 to 6 mm, - cold-rolled to a desired thickness, the thickness of the cold-rolled strip or sheet preferably being 0.15 to 3 mm, and - Heat treatment in a tunnel furnace at a temperature of 250 to 560°C, preferably 320 to 430°C, preferably 320 to 360°C, wherein the maximum temperature is maintained for less than 5 minutes, preferably less than 1 minute, preferably less than 30 seconds and preferably more than 15 seconds, or heat treatment in a batch furnace at a temperature of 250 to 390°C, preferably 310 to 360°C, wherein the maximum temperature is maintained for preferably less than 3 hours, preferably less than 2 hours and preferably less than 1 hour, to obtain small grain recrystallization.

12. A heat exchanger at least partially made from a strip or sheet according to any one of claims 1 to 9, preferably any one of claims 2 to 9, or from a set of two sheets or strips according to claim 10.

13. Use of a strip or sheet material according to any one of claims 1 to 9, preferably any one of claims 2 to 9, or a set of two sheets or strip materials according to claim 10 for producing a heat exchanger, preferably a battery cooler for an electric vehicle.

14. The use according to claim 13, comprising at least one of the following steps: - brazing in a CAB (controlled atmosphere) furnace, preferably at a temperature of 590 to 615° C., preferably 590 to 610° C., preferably 590 to 605° C., preferably 590 to 600° C.; - at the end of the brazing cycle, cooling to below 380°C and to a maximum of 100°C at a rate preferably higher than 25°C / min, preferably higher than 35°C / min, preferably higher than 50°C / min; Post-braze tempering is preferably carried out at a temperature of 150 to 240° C., preferably 180 to 220° C., for a duration of preferably less than 6 hours, preferably less than 3 hours.

Citation Information

Cited By

  • A quick locking tool for heat welding of plate heat exchanger

    CN122829512A