Method for producing lithium sulfide
By vibrating the container during the lithium sulfide manufacturing process, the powder reacts with the gas, and controlling the pressure and gas ejection position, the problems of low gas use efficiency and powder adhesion are solved, and efficient lithium sulfide manufacturing is achieved.
Patent Information
- Application Number
- CN202380032117.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-04-07
- Filing Date
- 2023-03-30
- Publication Date
- 2024-11-22
AI Technical Summary
In the existing lithium sulfide manufacturing methods, the gas usage efficiency is low, and the powder is prone to adhere to the wall of the device, resulting in high maintenance costs and poor filling rate and reaction efficiency.
By placing the powder containing lithium elements into a closed container and vibrating the container outside, the powder reacts with the gas containing sulfur elements, and controlling the pressure during the reaction and the gas ejection position to avoid gas leakage and powder adhesion.
It improves the manufacturing efficiency of lithium sulfide and gas use efficiency, reduces maintenance costs, ensures uniform flow and high filling rate of powder, and reduces moisture aggregation and powder adhesion.
Smart Images

Figure CN119013224A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for producing lithium sulfide. Background Art
[0002] Lithium sulfide is known as a raw material of a solid electrolyte used in, for example, an all-solid lithium ion secondary battery.
[0003] As a method for producing lithium sulfide, for example, a method of reacting a substance (powder) containing lithium element such as lithium hydroxide with a gas containing sulfur element such as hydrogen sulfide is known.
[0004] For example, Patent Document 1 describes a method for producing lithium sulfide in which lithium sulfide is synthesized by reacting lithium hydroxide with a gaseous sulfur source, and describes that a solid-gas reaction is performed in a fluidized bed.
[0005] Patent Document 2 describes that lithium sulfide particles are generated by reacting hydrogen sulfide gas with lithium hydroxide by bringing a reaction gas into contact with granular lithium hydroxide. Here, as a configuration in which lithium hydroxide is arranged inside a reaction tank, a configuration in which granular lithium hydroxide is preliminarily spread on the surface of a porous sheet is described.
[0006] Patent Document 3 describes a method for producing lithium sulfide in which lithium sulfide is continuously produced by reacting a lithium raw material with hydrogen sulfide gas, and describes that a rotary kiln can be used as a reaction tank.
[0007] Patent Document 4 describes an apparatus for producing lithium sulfide including a reaction vessel for bringing lithium hydroxide powder into contact with hydrogen sulfide gas and a stirring blade located inside the reaction vessel.
[0008] Patent Document 5 describes a method for producing lithium sulfide, which includes the step of reacting lithium hydroxide and hydrogen sulfide in a tray dryer without using a solvent.
[0009] Prior art literature
[0010] Patent Literature
[0011] Patent Document 1: Japanese Patent Application Laid-Open No. 9-278423
[0012] Patent Document 2: Japanese Patent Application Publication No. 2016-150859
[0013] Patent Document 3: Japanese Patent Application Publication No. 2018-35045
[0014] Patent Document 4: International Publication No. 2016 / 098351
[0015] Patent Document 5: Japanese Patent Application Publication No. 2017-222567 Summary of the invention
[0016] When manufacturing lithium sulfide, for example, when reacting a substance (powder) containing lithium elements such as lithium hydroxide with a gas containing sulfur elements such as hydrogen sulfide, water is sometimes generated as a by-product. Here, in the methods described in Patent Documents 1 and 2, a gas volume exceeding the flow start speed is required to make the particles of the substance containing lithium elements flow, and the gas use efficiency is sometimes poor. In addition, water is sometimes easy to condense on the wall of a device with a slow gas flow rate, and the powder is easy to adhere to the wall of the device when the powder is scattered by the gas. If the adhesion of powder is easy to occur in the device, the maintenance cost is easy to increase.
[0017] In the method described in Patent Document 3, since the entire device is rotated at a relatively low speed, the powder is easily attached to the wall surface of the device along with the condensation of water. Moreover, when a rotary kiln is used, the filling rate of the powder is low, so the manufacturing efficiency is sometimes poor. In addition, since the space not filled with powder is also filled with gas, the proportion of gas that does not contribute to the reaction is likely to become high, and the gas use efficiency is sometimes poor.
[0018] In the methods described in Patent Documents 4 and 5, gas is easily leaked from the shaft of the stirring blade, and the efficiency of gas use is sometimes poor. In addition, when using toxic gas, countermeasures for gas leakage are required, so the cost of the equipment is also likely to increase. In addition, the part without stirring blades in the device is prone to adhesion of powder accompanied by the condensation of water.
[0019] Therefore, an object of the present invention is to provide a method for producing lithium sulfide with excellent productivity.
[0020] That is, the present invention relates to the following 1 to 8.
[0021] 1. A method for producing lithium sulfide, comprising the following steps:
[0022] Put the powder containing lithium into the container, and
[0023] In a state where the container is sealed, the container is vibrated from the outside to drive the powder, and the powder is reacted with the gas containing sulfur element.
[0024] 2. The method for producing lithium sulfide according to item 1 above, comprising the steps of temporarily making the pressure in the container lower than the pressure in the container during the reaction, or making the pressure in the container lower than the pressure in the container during the reaction after the reaction.
[0025] 3. The method for producing lithium sulfide according to 1 or 2 above, wherein the pressure in the container during the reaction is 0.100 MPa or more.
[0026] 4. The method for producing lithium sulfide according to item 3 above, wherein the pressure in the container is lower than the pressure in the container during the reaction and is less than 0.100 MPa.
[0027] 5. A method for producing lithium sulfide according to 1 or 2 above, which comprises the following steps: introducing the gas containing elemental sulfur into the container from a nozzle arranged in the container; the ejection position of the gas containing elemental sulfur in the nozzle is within 50% of the height of the gas phase and within 50% of the depth of the powder with respect to the surface of the powder.
[0028] 6. The method for producing lithium sulfide according to 1 or 2 above, wherein the average particle size of the powder is 200 μm or more.
[0029] 7. The method for producing lithium sulfide according to 1 or 2 above, further comprising the step of adding particles other than powder containing lithium element into the container.
[0030] 8. The method for producing lithium sulfide according to 1 or 2 above, wherein the amplitude of the vibration is 1 mm to 10 mm.
[0031] According to the present invention, a method for producing lithium sulfide with excellent productivity can be provided. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 This is a flow chart illustrating the method for producing lithium sulfide according to the present embodiment.
[0033] Figure 2 is a diagram schematically illustrating a method for producing lithium sulfide according to this embodiment. Figure 2 (a) is a schematic cross-sectional view of the side of the container during the reaction. Figure 2 (b) is related to Figure 2 (a) Schematic cross-sectional view of the front side of the same container.
[0034] Figure 3 This is a flow chart illustrating the method for producing lithium sulfide according to the present embodiment.
[0035] Figure 4 is a diagram schematically illustrating a method for producing lithium sulfide according to this embodiment. Figure 4 (a) is a schematic cross-sectional view of the side of the container during the reaction. Figure 4 (b) is related to Figure 4 (a) Schematic cross-sectional view of the front side of the same container.
[0036] Figure 5 This is a flow chart illustrating the method for producing lithium sulfide according to the present embodiment.
[0037] Figure 6 is a flow chart illustrating a method for producing lithium sulfide according to this embodiment. Figure 6 (a) is a flow chart illustrating a method including a step of temporarily making the pressure in the container lower than the pressure in the container during the reaction, Figure 6 (b) is a flow chart illustrating a method including the step of making the pressure in the container lower than the pressure in the container during the reaction after the reaction. DETAILED DESCRIPTION
[0038] Hereinafter, the present invention will be described in detail, but the present invention is not limited to the following embodiments, and can be arbitrarily deformed and implemented within the scope of the gist of the present invention. In addition, the " to " representing a numerical range is used to include the numerical value recorded before and after it as the meaning of the lower limit and the upper limit.
[0039] The method for producing lithium sulfide of the present embodiment (hereinafter also referred to as the present production method) comprises the following steps: placing powder containing lithium element into a container, and in a sealed state, vibrating the container from the outside to drive the powder while causing the powder to react with a gas containing sulfur element.
[0040] The production method includes the steps of reacting a powder containing lithium element with a gas containing sulfur element. Hereinafter, the "powder containing lithium element" and the "gas containing sulfur element" may be referred to as "powder" and "gas", respectively.
[0041] As the powder containing lithium element, lithium hydroxide, lithium carbonate, lithium oxide, etc. can be cited. From the viewpoint of being able to process at a low temperature, lithium hydroxide is preferably contained. In addition, as the gas containing sulfur element, a gas containing a component containing sulfur element can be cited. For example, a gas containing one or more selected from hydrogen sulfide and carbon disulfide as a component containing sulfur element can be cited. Among them, the gas containing sulfur element is preferably a gas containing hydrogen sulfide from the viewpoint of being easy to handle because it is a gas at normal temperature and pressure.
[0042] For example, the reaction of lithium hydroxide and hydrogen sulfide is represented by the following reaction formula (1). In this case, lithium hydroxide (LiOH) reacts with hydrogen sulfide (H2S) to generate lithium sulfide (Li2S), and water (H2O) is produced as a by-product.
[0043] 2LiOH+H2S→Li2S+2H2O (1)
[0044] The above reaction is typically a reaction of hydrogen sulfide gas and solid lithium hydroxide to generate solid lithium sulfide and water vapor. For example, the above reaction can be carried out by bringing hydrogen sulfide gas into contact with solid lithium hydroxide and heating them.
[0045] When the powder containing lithium element includes lithium hydroxide, as lithium hydroxide, any one of lithium hydroxide anhydrate and lithium hydroxide monohydrate can be used, and a mixture thereof can be used. When lithium hydroxide monohydrate is used, from the viewpoint of improving reaction efficiency, it is preferred to heat the lithium hydroxide monohydrate in advance to remove crystal water. The heat treatment can be carried out in a vibration container for lithium sulfide synthesis, or in other devices.
[0046] The manufacturing method includes the following steps: putting a powder containing lithium element into a container, and in a sealed state, vibrating the container from the outside to drive the powder while reacting the powder with a gas containing sulfur element. That is, the manufacturing method includes the following steps: the reaction between the powder and the gas is carried out in a sealed container and the container is vibrated from the outside to drive the powder in the container.
[0047] Figure 1 This is a flow chart illustrating the present production method. Figure 1 The manufacturing method illustrated in the example includes: step S11 of placing a powder containing lithium element in a container, and step S12 including (i) vibrating the container from the outside while the container is sealed, and (ii) reacting the powder with a gas containing sulfur element. That is, in step S12, the powder is reacted with the gas containing sulfur element while the container is vibrated from the outside while the container is sealed.
[0048] As previously illustrated, in the reaction of the powder containing lithium element and the gas containing sulfur element, water (water vapor) is sometimes generated as a byproduct. If the above-mentioned water condenses in the reaction container, the powder is easily attached to the container due to the condensed water, etc., resulting in increased maintenance costs. In contrast, in the present manufacturing method, since the container itself is vibrated from the outside during the reaction, the adhesion of the powder is suppressed by vibrating the part to which the powder can be attached. Thus, the maintenance cost can be suppressed. In addition, since the powder inside is driven by the vibration of the container, it is not necessary to use gas to make the powder flow, and there is no need for excessive gas flow. Thus, the efficiency of gas use can be improved in the present manufacturing method. In addition, in the present manufacturing method, since there is no need to have a rotating mechanism, a rotating shaft of a stirring blade, etc. in the container, which are easily the cause of gas leakage, the container can be sealed. Thus, the gas used in the reaction is not easy to leak, and the efficiency of gas use is excellent. In addition, the present manufacturing method is a method that can provide a force that makes the powder flow more efficiently in the up and down directions, so the filling rate of the powder in the container can be higher, and the manufacturing efficiency of lithium sulfide is excellent.
[0049] In the present production method, vibrating the container from the outside means, for example, vibrating the container by vibrating a member such as a vibrator provided outside the container and directly or indirectly connected to the container.
[0050] In the present production method, the state in which the container is sealed refers to a state in which there is no gas leakage except for intentionally made openings such as an inlet for the powder containing lithium element, a gas inlet for introducing the gas containing sulfur element, a gas outlet for discharging the gas discharged after the reaction, and an outlet for the lithium sulfide powder synthesized after the reaction. In the present production method, the container does not have a member such as a rotating shaft of the stirring blade.
[0051] In the present production method, suppressing the adhesion of powder into the container means both suppressing the adhesion of powder containing lithium element into the container and suppressing the adhesion of powder of lithium sulfide obtained by the reaction.
[0052] Figure 2 It is a figure which schematically illustrates this manufacturing method. Figure 2 (a) is a schematic cross-sectional view of the side of the container during the reaction. Figure 2 (b) is related to Figure 2 (a) is a schematic cross-sectional view of the front side of the same container as (a). For the sake of convenience, some parts are only shown in (a) or (b), and are omitted in (b) or (a). Figure 4 The same is true in Figure 2 and the following Figure 4 In the figure, the arrows represented by the black solid lines schematically indicate the direction of gas flow. Figure 2 In the embodiment, the production apparatus 1 includes a container 10, and the container 10 includes a powder 5 containing lithium element therein.
[0053] There is no particular limitation on the method of placing the powder containing lithium in the container. For example, there may be a method of providing an openable and closable portion such as a raw material inlet in the container and placing the raw material therein, or a method of introducing the powder containing lithium in the form of a powder liquid together with an air flow. Figure 2 In the example of FIG. 1 , the container 10 includes a powder material introduction port 11 . For example, the powder 5 containing lithium element is charged into the container 10 from the powder material introduction port 11 .
[0054] The filling amount of the powder containing lithium element in the container is preferably 30 volume % to 100 volume %, more preferably 50 volume % to 90 volume %, and further preferably 70 volume % to 80 volume % relative to the volume of the container. Here, from the viewpoint of increasing the processing amount per unit time to improve the production efficiency of lithium sulfide, the above filling amount is preferably 30 volume % or more, more preferably 50 volume % or more, and further preferably 70 volume % or more relative to the volume of the container. On the other hand, from the viewpoint of improving the homogeneity of the reaction and the viewpoint of making the powder flow stably, the filling amount is preferably 100 volume % or less, more preferably 90 volume % or less, and further preferably 80 volume % or less.
[0055] After putting the powder containing the lithium element into a container, the container is sealed, and the powder is driven by vibrating the container from the outside, and the powder is reacted with the gas containing the sulfur element. There is no particular limitation on the method of sealing the container, and examples thereof include using a container without a component having a rotating shaft such as a stirring blade, and using a container made of a component that does not permeate gas.
[0056] In addition, the method of vibrating the container is not particularly limited. Figure 2 In the configuration of, for example, the container 10 can be arranged on a base 90 having a vibrator 9, and the vibrator 9 can be vibrated to vibrate the container 10 from the outside. In this case, the container is vibrated in such a way that the powder inside the container moves (flows) due to the vibration. Figure 2 In the configuration of FIG. 1 , when the container 10 is vibrated from the outside by placing the container 10 on a base 90 or the like having a vibrator 9 and vibrating the vibrator 9, the powder in the container can be Figure 2 The direction (b) is the direction in which the liquid flows in a rotating manner in the container when viewed from the front. Figure 2 In the structure of Figure 2 The direction of the arrow represented by the hollow in the figure is vibrated in the up-down direction of the figure. As a device capable of such vibration, a vibration drying device can be cited, for example, a vibration drying machine VH type and VHC type manufactured by Central Chemical Industry Co., Ltd. can be cited.
[0057] The following is an explanation of an example of the structure of a vibration drying device. The vibration dryer, for example, has the following structure: a drying container of a roughly cylindrical shape with a heating jacket installed on substantially the entire surface is arranged in a direction substantially parallel to the axial direction of the cylinder and the horizontal direction, and is supported by a spring. A vibration source (vibrator) is installed at the bottom of the drying container. When a powdery or granular raw material is added to the drying container and the vibration source is operated in a circular motion along the circumferential direction, the powdery or granular layer is given a motion mainly in the circumferential up and down directions. The drying container can supply heat to the powdery or granular layer from the container wall by supplying steam or warm water or temperature-controlled oil to the heating jacket.
[0058] In the present manufacturing method, the amplitude of the vibration is preferably 1 mm to 10 mm, more preferably 1.5 mm to 7 mm, and further preferably 2 mm to 4 mm. Here, from the viewpoint of allowing the powder to flow sufficiently, the above-mentioned amplitude is preferably 1 mm or more, more preferably 1.5 mm or more, and further preferably 2 mm or more. On the other hand, from the viewpoint of easy manufacture of the device, the amplitude is preferably 10 mm or less, more preferably 7 mm or less, and further preferably 4 mm or less. It should be noted that the amplitude of the vibration refers to the amplitude of the displacement in the up and down direction (along the direction of vibration) of the container.
[0059] In addition, the frequency of vibration is preferably 10Hz to 100Hz, more preferably 15Hz to 80Hz, and further preferably 20Hz to 60Hz. Here, from the viewpoint of making the powder flow fully and stabilizing the flow, the above frequency is preferably above 10Hz, more preferably above 15Hz, and further preferably above 20Hz. On the other hand, from the viewpoint of easy manufacture of the device, the frequency of vibration is preferably below 100Hz, more preferably below 80Hz, and further preferably below 60Hz. It should be noted that the frequency of vibration is the number of reciprocating times that the container vibrates up and down (along the direction of vibration) within 1 second.
[0060] In this sealed state, the container is vibrated from the outside to drive the powder, and the powder and the gas are reacted. Figure 2 As shown, a gas containing sulfur element is introduced into the container 10 from a nozzle 7 arranged in the container 10 . Figure 2 The nozzle 7 is arranged in a continuous manner from the outside of the container to the inside of the container, and has a gas inlet 12a on the outside of the container and a gas outlet 12b on the inside of the container. It should be noted that the nozzle 7 is fixed in the container. However, the method of introducing the gas containing sulfur element into the container is not limited to this. In addition, the container 10 may be appropriately equipped with a mechanism for introducing the gas containing sulfur element and a mechanism for discharging the gas in the container 10. For example, in Figure 2 In the structure of FIG. 1 , the container 10 includes a gas exhaust port 13 .
[0061] The gas containing sulfur element may be any gas containing a component containing sulfur element as described above. When the gas containing sulfur element is introduced into the container, the concentration of the component containing sulfur element may be adjusted by further containing an inert gas or the like. Examples of the inert gas include nitrogen gas and argon gas. From the viewpoint of allowing the powder and the gas to react sufficiently, the concentration of the component containing sulfur element in the gas containing sulfur element (the concentration of the gas containing sulfur element) is preferably 20% by volume or more, more preferably 50% by volume or more, and even more preferably 80% by volume or more.
[0062] When the powder and the gas are reacted, it is preferred to heat the container to an appropriate temperature. Specifically, the temperature when the powder and the gas are reacted is preferably 140°C to 240°C, more preferably 160°C to 230°C, and further preferably 180°C to 220°C. Here, from the viewpoint of allowing the reaction to proceed sufficiently and avoiding condensation of the generated moisture, the temperature is preferably 140°C or more, more preferably 160°C or more, and further preferably 180°C or more. On the other hand, from the viewpoint of the heat resistance of the component, the temperature is preferably 240°C or less, more preferably 230°C or less, and further preferably 220°C or less. The heating method is not particularly limited, and may be a known method such as a method using the above-mentioned heating jacket.
[0063] The time for reacting the powder with the gas varies depending on conditions such as the pressure in the container, the concentration of the gas containing sulfur element, the filling amount of the powder, and is therefore not particularly limited. As an example, it is preferably 10 minutes to 600 minutes, more preferably 30 minutes to 300 minutes, and further preferably 60 minutes to 180 minutes. Here, from the viewpoint of allowing the reaction to proceed sufficiently, the time for reacting the powder with the gas is preferably more than 10 minutes, more preferably more than 30 minutes, and further preferably more than 60 minutes. On the other hand, from the viewpoint of production tact, the reaction time is preferably less than 600 minutes, more preferably less than 300 minutes, and further preferably less than 180 minutes.
[0064] The pressure in the container when the powder reacts with the gas is not particularly limited, and is preferably normal pressure or slightly pressurized, and more preferably slightly pressurized. Specifically, the above pressure is preferably 0.100MPa~0.200MPa, more preferably 0.105MPa~0.200MPa, further preferably 0.110MPa~0.160MPa, and particularly preferably 0.120MPa~0.140MPa. Here, the reaction of the powder and the gas is made easier by making the pressure in the container higher. Specifically, the pressure in the container during the reaction is preferably 0.100MPa or more, more preferably 0.105MPa or more, further preferably 0.110MPa or more, and particularly preferably 0.120MPa or more. On the other hand, from the viewpoint of easy manufacture of the device, the pressure in the container during the reaction is preferably 0.200MPa or less, more preferably 0.160MPa or less, and further preferably 0.140MPa or less.
[0065] For the powder containing lithium element used in the reaction, for example, the average particle size is preferably about 100μm to 1500μm, more preferably 200μm to 1000μm, further preferably 250μm to 800μm, and particularly preferably 300μm to 800μm. Here, the average particle size is preferably 100μm or more, more preferably 200μm or more, further preferably 250μm or more, and particularly preferably 300μm or more. By making the average particle size above the above lower limit, the powder becomes easy to flow stably when the container is vibrated. As a result, the powder and the gas are easy to react more homogeneously. In addition, since the flow retardation in the container is suppressed, it is not easy for moisture to condense in the container, and the adhesion of the powder to the container can be suppressed. In addition, by making the average particle size relatively large, the powder becomes less likely to scatter, and the adhesion of the powder to the container is suppressed. On the other hand, from the viewpoint of improving the reaction efficiency, the average particle size is more preferably 1500μm or less, more preferably 1000μm or less, and particularly preferably 800μm or less.
[0066] Here, the average particle size of the powder containing lithium element refers to the median particle size (D50) obtained from the volume-based particle size distribution diagram obtained by measuring the particle size distribution using a laser diffraction particle size distribution analyzer MT3300EXII manufactured by Microtrac.
[0067] In addition, the D90 of the powder containing lithium element is preferably 300μm to 3000μm, more preferably 500μm to 2500μm, and further preferably 800μm to 2000μm. Here, the above D90 is preferably 300μm or more, more preferably 500μm or more, and further preferably 800μm or more. By making D90 above the above lower limit, the powder becomes easy to flow stably when the container is vibrated. As a result, the powder and the gas are easy to react more homogeneously. In addition, since the flow retardation in the container is suppressed, it is not easy for moisture to condense in the container, and the adhesion of the powder to the container can be suppressed. In addition, by making D90 above the above lower limit, the powder becomes less likely to scatter, and the adhesion of the powder to the container is suppressed. On the other hand, in order to avoid the residue of unreacted particles, D90 is preferably 3000μm or less, more preferably 2500μm or less, and further preferably 2000μm or less.
[0068] Here, D90 refers to a value of D90 obtained from a volume-based particle size distribution diagram obtained by measuring the particle size distribution using a laser diffraction particle size distribution analyzer MT3300EXII manufactured by Microtrac.
[0069] The angle of repose of the powder containing lithium element is preferably 50° or less, more preferably 45° or less, and further preferably 40° or less. In general, the larger the average particle size of the powder, the smaller the angle of repose of the powder tends to be. That is, by making the angle of repose below the above value, the powder becomes easy to flow stably when the container is vibrated. As a result, the powder and the gas are easy to react more homogeneously. In addition, since the flow retardation in the container is suppressed, it is not easy for moisture to condense in the container, and the adhesion of the powder to the container can be suppressed. In addition, by making the average particle size relatively large, the powder becomes less likely to scatter, and the adhesion of the powder to the container is suppressed. Here, the angle of repose of the powder refers to a value measured, for example, according to JIS R9301-2-2:1999.
[0070] The manufacturing method may further include placing a medium into the container. As the medium, for example, particles other than powder containing lithium element may be cited. From the viewpoint of not easily reacting with gas containing sulfur element and powder containing lithium element, at least one of aluminum oxide particles and zirconium oxide particles is preferred. By placing the medium into the container, the powder becomes easy to flow stably when the container is vibrated. As a result, the powder and the gas are easy to react more homogeneously. In addition, since the flow retardation in the container is suppressed, it is not easy for moisture to condense in the container, and the adhesion of the powder to the container can be suppressed. The timing of placing the medium into the container is not particularly limited, for example, it may be before the powder and the gas are reacted.
[0071] Figure 3 This is a flowchart illustrating the manufacturing method including the step of placing particles (medium) other than the powder containing lithium element into the container. In this case, the manufacturing method includes, for example, step S21 of placing the powder containing lithium element into the container, step S22 of placing particles other than the powder containing lithium element into the container, and step S23 including (i) vibrating the container from the outside while the container is sealed and (ii) reacting the powder with the gas containing sulfur element. Step S21 and step S22 may be performed sequentially, or step S21 may be performed after step S22. In addition, step S21 and step S22 may be performed in parallel or simultaneously.
[0072] When introducing sulfur-containing gas into the container from a nozzle disposed in the container, the ejection position L4 of the sulfur-containing gas in the nozzle is preferably within 50% of the height H1 of the gas phase and within 50% of the depth H2 of the powder based on the surface L2 of the powder. The ejection position L4 of the gas is within 50% of the height H1 of the gas phase based on the surface L2 of the powder, which means the following. That is, Figure 2In this case, when the gas ejection position L4 in the nozzle 7 is not buried in the layer of the powder 5 but is located in the gas phase, the distance from the surface L2 of the powder 5 to the gas ejection position L4 is within 50% of the height H1 of the gas phase. Here, the surface L2 of the powder refers to the height of the surface of the powder when the powder in the container is made uniform without vibrating the container. In addition, the height H1 of the gas phase refers to the distance from the surface of the powder to the top of the container. Figure 2 and the following Figure 4 The middle refers to the distance H1 from L2 to L1.
[0073] in addition, Figure 4 is a diagram schematically illustrating the present manufacturing method, and is a diagram showing Figure 2 This is a diagram showing an example in which only the position of the nozzle 7 is changed. Figure 2 and Figure 4 In the drawings, there are places where common parts and configurations are represented by common symbols.
[0074] Figure 4 (a) is a schematic cross-sectional view of the side of the container during the reaction. Figure 4 (b) is related to Figure 4 (a) is a schematic cross-sectional view of the front side of the same container. The gas ejection position L4 is within 50% of the depth H2 of the powder based on the surface L2 of the powder. Figure 4 In this case, when the gas ejection position L4 in the nozzle 7 contacts or is buried in the layer of the powder 5, the distance from the surface L2 of the powder 5 to the gas ejection position L4 is within 50% of the depth H2 of the powder. Here, the depth of the powder refers to the distance from the surface L2 of the powder to the bottom of the container. Figure 2 and Figure 4 The middle refers to the distance H2 from L2 to L3.
[0075] The gas ejection position is preferably within 50% of the height of the gas phase, more preferably within 40%, and even more preferably within 30%. This makes it easy to efficiently discharge the water in the container after the reaction.
[0076] In addition, the gas ejection position is preferably within 50% of the depth of the powder, more preferably within 40%, and further preferably within 30%. This can prevent the water generated during the reaction from reacting in the container and hindering the formation reaction of lithium sulfide. In addition, the flow of the gas can be suppressed and the condensation of water in the container can be suppressed.
[0077] In addition, when introducing the gas containing elemental sulfur into the container from a nozzle disposed in the container, the ejection position of the gas containing elemental sulfur in the nozzle is preferably located within a height of ±100 mm, more preferably within a height of ±80 mm, and further preferably within a height of ±60 mm, based on the surface of the powder. Thus, it is easy to effectively discharge the water in the container after the reaction. In addition, it is possible to suppress the water generated during the reaction from reacting in the container and hindering the formation reaction of lithium sulfide. In addition, it is possible to suppress the flow retardation of the gas and suppress the condensation of water in the container.
[0078] Here, the + direction of the height based on the surface of the powder refers to the direction from the surface of the powder to the gas phase side (i.e., the upper side of the container) in the height direction of the powder layer. On the other hand, the - direction refers to the direction from the surface of the powder to the side where the powder layer is located (i.e., the bottom side of the container) in the height direction of the powder layer. For example, based on the surface L2 of the powder, Figure 2 and Figure 4 The upward direction in the paper is the + direction of height, Figure 2 and Figure 4 The downward direction in the paper is the - direction of height.
[0079] The gas ejection position is preferably within 50% of the depth of the powder. Therefore, when the depth of the powder is 200 mm or more, it is particularly preferably within ±100 mm in height relative to the surface of the powder.
[0080] It is preferred that multiple gas ejection positions are arranged in the container. This makes it easier to evenly supply the sulfur-containing gas to a wider range in the container, and makes it easier to homogenize and efficiently carry out the reaction between the powder and the gas. Figure 2 and Figure 4 In FIG. 1 , the nozzle 7 has a plurality of gas ejection ports 12 b, and the configuration of ejecting gas from a plurality of positions of the nozzle 7 is shown. Figure 2 and Figure 4 In the embodiment, a plurality of gas ejection positions are arranged in the container. In addition, the direction of ejecting the gas from each ejection position is preferably toward the surface of the powder (the surface of the layer of the powder).
[0081] Figure 5 The flowchart of the present manufacturing method is exemplified in the case where a gas containing sulfur element is introduced into the container from a nozzle disposed in the container and the ejection position of the gas containing sulfur element in the nozzle is set to the predetermined position as described above. In this case, the present manufacturing method includes, for example, a step S31 of setting the ejection position of the gas by placing a predetermined amount of powder containing lithium element in the container, and a step S32 of (i) vibrating the container from the outside in a sealed state, (ii) introducing a gas containing sulfur element into the container from a nozzle disposed in the container, and (iii) reacting the powder with the gas containing sulfur element.
[0082] It is preferred that the flow of gas in the container suppresses precipitation and stagnation. By suppressing precipitation and stagnation by the flow of gas, it is difficult for water to condense in the container, and it is possible to suppress the adhesion of powder into the container. As a method for suppressing precipitation and stagnation, for example, the method of making the powder flow more stably during the reaction as described above can be cited.
[0083] By reacting the powder containing the lithium element and the gas containing the sulfur element in this manner, lithium sulfide is obtained in a solid form.
[0084] In the present production method, it is preferred to remove moisture in the container during or after the reaction between the powder and the gas. By removing moisture in the container, it is possible to suppress the adhesion of the powder into the container.
[0085] As a method for removing moisture in the container, for example, the following method can be cited: temporarily lowering the pressure in the container during the reaction between the powder and the gas than the pressure in the container during the reaction, or lowering the pressure in the container after the reaction between the powder and the gas than the pressure in the container during the reaction. The above method is called a temporary decompression process. By utilizing the temporary decompression process to make the pressure in the container lower than the pressure in the container during the reaction, the gas containing moisture can be discharged from the mechanism for discharging the gas in the container. The discharge of the gas can be carried out, for example, through the gas discharge port 13 provided in the container 10. At this time, the gas containing sulfur element remaining after the reaction can be discharged together. In this manufacturing method, a sealable container is used, so it is easy to adjust the pressure in the container. It should be noted that when removing moisture by temporarily lowering the pressure in the container during the reaction than the pressure in the container during the reaction, the gas containing sulfur element can also be supplied to the container in parallel by increasing the exhaust volume.
[0086] Specifically, the pressure in the container is preferably 0.010MPa to 0.100MPa, more preferably 0.010MPa or more and less than 0.100MPa, more preferably 0.020MPa to 0.080MPa, and particularly preferably 0.030MPa to 0.060MPa. That is, the pressure in the container is preferably 0.100MPa or less, more preferably less than 0.100MPa, more preferably 0.080MPa or less, and particularly preferably 0.060MPa or less, temporarily during the reaction of the powder and the gas or after the reaction of the powder and the gas. On the other hand, from the viewpoint of manufacturing tact, the pressure in the container after the reaction is preferably 0.010MPa or more, more preferably 0.020MPa or more, and more preferably 0.030MPa or more.
[0087] In addition, the difference between the pressure during the reaction of the powder and the gas and the pressure after the reaction is preferably 0.005MPa to 0.100MPa, more preferably 0.010MPa to 0.080MPa, and further preferably 0.020MPa to 0.060MPa. Here, from the viewpoint of effectively discharging the gas containing water, the above-mentioned pressure difference is preferably 0.005MPa or more, more preferably 0.010MPa or more, and further preferably 0.020MPa or more. On the other hand, from the viewpoint of manufacturing tact, the difference between the pressure during the reaction and the pressure after the reaction is preferably 0.100MPa or less, more preferably 0.080MPa or less, and further preferably 0.060MPa or less.
[0088] When removing the water in the container, it is also preferred that the flow of gas suppresses precipitation and stagnation, as in the case of the reaction. This makes it difficult for the water to condense in the container, and it is possible to suppress the adhesion of the powder into the container.
[0089] Figure 6 This is a flow chart showing an example of the present production method including a step of removing moisture from a container. Figure 6 (a) is a flow chart illustrating a method including a step of temporarily making the pressure in the container lower than the pressure in the container during the reaction, Figure 6 (b) is a flow chart illustrating a method including the step of making the pressure in the container lower than the pressure in the container during the reaction after the reaction. That is, Figure 6 The manufacturing method illustrated in (a) includes: step S411 of placing a powder containing lithium element in a container, and step S412 of (i) vibrating the container from the outside while the container is sealed, (ii) reacting the powder with a gas containing sulfur element, and (iii) temporarily lowering the pressure in the container during the reaction to a pressure lower than the pressure in the container during the reaction. Figure 6 The manufacturing method illustrated in (b) includes: step S421 of placing a powder containing lithium element in a container, including step S422 of (i) vibrating the container from the outside while the container is sealed, and (ii) reacting the powder with a gas containing sulfur element, and step S423 of making the pressure in the container lower than the pressure in the container during the reaction. It should be noted that in this manufacturing method, it is also possible to place Figure 6 A combination of (a) and (b), such as Figure 6 In the manufacturing method of (a), after step S412, a further step may be provided. Figure 6 The same process as step S423 of (b).
[0090] The sulfur-containing gas used in the reaction can be recovered or circulated within the device for reuse, thereby further improving the utilization efficiency of the sulfur-containing gas.
[0091] After the reaction between the powder and the gas, the water in the container is preferably removed and then the lithium sulfide is recovered from the container. The recovery can be performed by a known method, but the recovery operation is preferably performed in an environment where the lithium sulfide is not in contact with the air, such as an inert gas atmosphere. Figure 2 and Figure 4 The container 10 in the embodiment includes a powder material discharge port 14. For example, lithium sulfide after the reaction can be recovered through the powder material discharge port.
[0092] The recovered lithium sulfide can be identified by, for example, X-ray diffraction measurement.
[0093] It should be noted that the present production method can be carried out in a batch manner or in a continuous manner. Even in the case of a continuous manner, by appropriately dividing the process, the pressure can be appropriately adjusted while the container is sealed, such as by reducing the pressure to remove the moisture in the container after the reaction. For example, a VH type vibration dryer of Central Chemical Industry Co., Ltd. can be used for batch reaction, and a VHC type vibration dryer can be used for continuous reaction.
[0094] The lithium sulfide obtained by the present production method can be suitably used as a raw material for a solid electrolyte used in an all-solid lithium ion secondary battery, a raw material for a positive electrode active material, a raw material for a negative electrode active material, an intermediate raw material for chemicals, and the like.
[0095] As described above, the present specification discloses the following matters.
[0096] 1. A method for producing lithium sulfide, comprising the following steps:
[0097] Put the powder containing lithium into the container, and
[0098] In a state where the container is sealed, the container is vibrated from the outside to drive the powder, and the powder is reacted with the gas containing sulfur element.
[0099] 2. The method for producing lithium sulfide according to item 1 above, comprising the steps of temporarily making the pressure in the container lower than the pressure in the container during the reaction, or making the pressure in the container lower than the pressure in the container during the reaction after the reaction.
[0100] 3. The method for producing lithium sulfide according to 1 or 2 above, wherein the pressure in the container during the reaction is 0.100 MPa or more.
[0101] 4. The method for producing lithium sulfide according to item 3 above, wherein the pressure in the container is lower than the pressure in the container during the reaction and is less than 0.100 MPa.
[0102] 5. A method for producing lithium sulfide according to any one of 1 to 4 above, which comprises the following steps: introducing the gas containing elemental sulfur into the container from a nozzle arranged in the container; the ejection position of the gas containing elemental sulfur in the nozzle is within 50% of the height of the gas phase and within 50% of the depth of the powder based on the surface of the powder.
[0103] 6. The method for producing lithium sulfide according to any one of 1 to 5 above, wherein the average particle size of the powder is 200 μm or more.
[0104] 7. The method for producing lithium sulfide according to any one of 1 to 6 above, further comprising the step of placing particles other than the powder containing lithium element into the container.
[0105] 8. The method for producing lithium sulfide according to any one of 1 to 7 above, wherein the amplitude of the vibration is 1 mm to 10 mm.
[0106] Example
[0107] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited thereto.
[0108] Examples 1 to 8 are all implementation examples.
[0109] (Example 1)
[0110] Lithium hydroxide powder (manufactured by Tokyo Chemical Industry Co., Ltd.) was placed in a vibration drying device (product name VH-10, manufactured by Central Chemical Industry Co., Ltd.). The average particle size (D50) of the lithium hydroxide powder was 400 μm, and D90 was 1000 μm. The powder was added to a position at a height of 50% of the height from the bottom of the reaction container to the height of the container ceiling. After the addition, the vibration of the vibration drying device was started with an amplitude of 3 mm and a vibration frequency of 24 Hz. It was confirmed that under this vibration condition, the powder was stably rotating and flowing.
[0111] Next, use a vacuum pump to extract the gas in the reaction vessel from the gas exhaust port so that the pressure in the reaction vessel is 0.005 MPa. Then, nitrogen is flowed in from the gas inlet to make a nitrogen atmosphere in the reaction vessel. The flow rate of nitrogen flowing in from the gas inlet is set to 1SLM (Standard Litter Min), and the pressure in the reaction vessel is adjusted to a pressure of 0.105 MPa inside the container. While maintaining the gas flow rate and pressure, the temperature of the jacket covering the reaction vessel is raised to 200°C. After the temperature is reached, the gas flowing in from the gas inlet is switched to 0.5SLM nitrogen and 0.5SLM hydrogen sulfide, and the reaction of lithium hydroxide and hydrogen sulfide is started.
[0112] The pressure in the reaction container during the reaction was adjusted to 0.105 MPa. The position of the gas outlet was 25% of the height of the gas phase from the powder surface to the container ceiling based on the powder surface. The gas flowed for 4 hours. Then, the introduced gas was replaced with nitrogen 1 SLM and maintained for 1 hour, and then the heating was stopped, the temperature was restored to room temperature, the vibration was stopped, and the sample was recovered.
[0113] The reaction rate of the recovered lithium sulfide was investigated by powder X-ray diffraction (XRD) measurement described later and the result was 94%. In addition, after recovery, the adhesion to the container wall was observed and found to be non-adherent, so the next batch test could be started.
[0114] (Example 2)
[0115] In (Example 1), the reaction with the gas is continuously carried out for 4 hours. The synthesis of lithium sulfide is carried out by the same method except that the gas is first allowed to flow for 2 hours for reaction, the introduction of the gas is temporarily stopped to make the pressure in the reaction container 0.020 MPa (temporary decompression step), the gas is introduced again to make the pressure in the reaction container 0.105 MPa, and the reaction with the gas is further carried out for 2 hours.
[0116] The reaction rate of the recovered lithium sulfide was investigated and found to be 99%. In addition, after recovery, the adhesion to the container wall was observed and found to be non-adherent, so the next batch test could be started.
[0117] (Example 3)
[0118] Lithium sulfide was synthesized in the same manner as in Example 1 except that the pressure in the reaction container during the reaction with the gas was changed from 0.105 MPa to 0.120 MPa.
[0119] The reaction rate of the recovered lithium sulfide was investigated and found to be 96%. In addition, after recovery, the adhesion to the container wall was observed and found to be non-adherent, so the next batch test could be started.
[0120] (Example 4)
[0121] Lithium sulfide was synthesized in the same manner as in Example 1 except that the lithium hydroxide used in Example 1 was crushed in a mortar and classified to a powder having an average particle size of 200 μm. Although the rotational motion of the powder was disturbed during vibration compared to Example 1, lithium sulfide was synthesized.
[0122] The reaction rate of the recovered lithium sulfide was investigated and found to be 90%. In addition, after recovery, the adhesion to the container wall was observed and found to be non-adherent, so the next batch test could be started.
[0123] (Example 5)
[0124] The lithium hydroxide having an average particle size of 200 μm used in Example 4 was mixed with the same weight of alumina particles as a medium. Alumina particles having a diameter of 3 mm were used. The mixture was placed in a vibration drying device as a powder raw material, and lithium sulfide was synthesized in the same manner as in Example 1.
[0125] Although the rotational motion of the powder was disturbed during vibration in (Example 4), it became a stable rotational motion flow by adding alumina particles as a medium. After synthesis, the mixture of lithium sulfide and alumina particles was recovered, and the alumina particles were removed by a sieve to recover only lithium sulfide.
[0126] The reaction rate of the recovered lithium sulfide was investigated and found to be 97%. In addition, after recovery, the adhesion to the container wall was observed and found to be non-adherent, so the next batch test could be started.
[0127] (Example 6)
[0128] In (Example 1), the position of the gas outlet was set at 25% of the height of the gas phase from the powder surface to the ceiling of the container, but here the position was set at 50% of the height of the gas phase. Except for this, lithium sulfide was synthesized using the same method as (Example 1).
[0129] The reaction rate of the recovered lithium sulfide was investigated and found to be 90%. In addition, after recovery, the adhesion to the container wall was observed and found to be non-adherent, so the next batch test could be started.
[0130] (Example 7)
[0131] In (Example 1), the position of the gas outlet is set at 25% of the height of the gas phase from the surface of the powder to the ceiling of the container, but here the gas outlet is buried in the powder at a position that is 25% of the thickness of the powder layer, i.e., 25% of the depth of the powder, away from the surface of the powder. Other than this, lithium sulfide is synthesized using the same method as in (Example 1).
[0132] The reaction rate of the recovered lithium sulfide was investigated and found to be 95%. In addition, after recovery, the adhesion to the container wall was observed and found to be non-adherent, so the next batch test could be started.
[0133] (Example 8)
[0134] In (Example 1), the position of the gas outlet is set at 25% of the height of the gas phase from the surface of the powder to the ceiling of the container, but here the gas outlet is buried in the powder at a position that is 50% of the thickness of the powder layer, i.e., 50% of the depth of the powder, away from the surface of the powder. Other than this, lithium sulfide is synthesized using the same method as in (Example 1).
[0135] The reaction rate of the recovered lithium sulfide was investigated and found to be 91%. In addition, after recovery, the adhesion to the container wall was observed and found to be non-adherent, so the next batch test could be started.
[0136] According to the above results, lithium sulfide can be synthesized with a reaction rate of more than 90% by performing the synthesis under appropriate vibration conditions. In addition, after the synthesis is implemented, no raw materials adhere to the wall of the reaction container, and the container can be used directly when synthesizing the next batch, thereby improving manufacturing efficiency.
[0137] In (Example 2), the reaction rate can be improved compared with (Example 1), which is believed to be because the water generated in the synthesis reaction of lithium sulfide is reduced by reducing the pressure during the synthesis. The generated water causes a reverse reaction that returns lithium sulfide to lithium hydroxide, which causes a decrease in the reaction rate. Therefore, it is believed that the reaction rate can be increased by reducing the pressure during the reaction to remove the generated water.
[0138] (Example 3) shows that the reaction rate to lithium sulfide can be increased by increasing the pressure during the reaction.
[0139] In Example 4, when a fine-particle raw material was used, the rotational flow of the powder during the vibration operation became unstable. Therefore, it is considered that the powder reacted with the gas unevenly, and the reaction efficiency to lithium sulfide was slightly reduced.
[0140] In (Example 5), a medium was added to stabilize the flow and the synthesis was performed. It is considered that the unstable swirling flow in (Example 4) was stabilized by adding a medium, thereby improving the reaction rate.
[0141] In (Example 6), the position of the gas ejection port was changed. It was found that the reaction efficiency would decrease when the gas ejection position was separated from the powder surface.
[0142] (Example 7) and (Example 8) are examples in which the gas ejection port is buried in the powder.
[0143] (Calculation of reaction rate)
[0144] The reaction rate to lithium sulfide is determined by XRD measurement (device name: SmartLab manufactured by Rigaku Corporation). Specifically, first, a sample obtained by mixing lithium hydroxide in lithium sulfide at a known mass % is measured separately from the analysis of the sample to be measured. Then, the peak intensity of lithium hydroxide of the sample to be measured is compared with the peak intensity of lithium hydroxide of the sample obtained by mixing lithium hydroxide in lithium sulfide at a known mass %, thereby calculating the mass % of lithium hydroxide contained in the sample to be measured.
[0145] The reaction rate to lithium sulfide was calculated as (100 - mass % of lithium hydroxide)%.
[0146] [Table 1]
[0147]
[0148] Although the present invention is described in detail with reference to specific embodiments, it is obvious to those skilled in the art that various changes and modifications can be added without departing from the spirit and scope of the present invention. This application is based on Japanese patent application (Japanese Patent Application No. 2022-064100) filed on April 7, 2022, the contents of which are incorporated herein by reference.
[0149] Explanation of symbols
[0150] 1. Manufacturing device
[0151] 10 containers
[0152] 11 Powder raw material inlet
[0153] 12a Gas inlet
[0154] 12b Gas outlet
[0155] 13 Gas outlet
[0156] 14 Powder raw material discharge port
[0157] 5. Powder containing lithium
[0158] 7 Nozzles
[0159] 9 Vibrators
[0160] 90 base
Claims
1. A method for producing lithium sulfide, comprising the following steps: Put the powder containing lithium into the container, and In a state where the container is sealed, the container is vibrated from the outside to shake the powder, thereby causing the powder to react with the gas containing elemental sulfur.
2. The method for producing lithium sulfide according to claim 1, wherein: The method comprises the steps of temporarily making the pressure in the container lower than the pressure in the container during the reaction during the reaction, or making the pressure in the container lower than the pressure in the container during the reaction after the reaction.
3. The method for producing lithium sulfide according to claim 1 or 2, wherein: The pressure in the container during the reaction is 0.100 MPa or more.
4. The method for producing lithium sulfide according to claim 3, wherein: The pressure when the pressure in the container is made lower than the pressure in the container during the reaction is less than 0.100 MPa.
5. The method for producing lithium sulfide according to claim 1 or 2, wherein: The method comprises the following steps: introducing the gas containing sulfur element into the container from a nozzle arranged in the container, The ejection position of the gas containing elemental sulfur in the nozzle is within 50% of the height of the gas phase and within 50% of the depth of the powder, based on the surface of the powder.
6. The method for producing lithium sulfide according to claim 1 or 2, wherein: The average particle size of the powder is greater than 200 μm.
7. The method for producing lithium sulfide according to claim 1 or 2, wherein: The method further comprises the following step: adding particles other than powder containing lithium element into the container.
8. The method for producing lithium sulfide according to claim 1 or 2, wherein: The amplitude of the vibration is 1 mm to 10 mm.
Citation Information
Patent Citations
Preparation method of 3,6-dichlorosalicylic acid
CN102838482A
Method and device for fluidizing powder and granular material bed in hermetic vessel
JP2001212448A
Method of producing fluorinated lithium-containing composite metallic oxide particle
JP2012116698A
Method of producing metal sulfide
JP2015003843A
Manufacturing method of lithium sulfide
JP2017141129A
Cited By
Lithium sulfide and preparation method thereof
CN120987268A