Composite fiber and preparation method thereof

By controlling the pH value and conductivity of calcium carbonate precipitation during papermaking, calcium carbonate adheres to nanocellulose fibers in a partial triangular form, the problem of insufficient mineral adhesion is solved and the high adhesion of composite fibers is achieved and excellent papermaking performance.

CN119013450APending Publication Date: 2024-11-22SPECIALTY MINERALS MICHIGAN INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380033684.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-27
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the process of precipitating calcium carbonate, it is difficult to effectively improve the amount of mineral adhesion and fiber surface coverage, resulting in poor application of composite materials in papermaking.

Method used

Prepare calcium hydroxide ripe by diluting lime in water and mixing it with CO2 gas and aqueous fiber slurry to precipitate calcium carbonate onto nanocellulose fibers, control pH and conductivity, and ensure that minerals are partially triangular. The morphological adhesion forms a high adhesion amount of composite fibers.

Benefits of technology

显著提高了矿物质附着量和纤维表面覆盖率,改进了复合纤维的膨松度、强度和刚度,适用于造纸填料,提供了更高的物理强度和良好的自然保留和排水性能。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013450A_ABST
    Figure CN119013450A_ABST
Patent Text Reader

Abstract

A method of making a composite fiber may include mixing a calcium hydroxide condensate and a carbon dioxide-containing gas with a fiber-containing aqueous slurry wherein the addition of the condensate is controlled to maintain electrical conductivity below saturation, this results in a composite fiber having improved bulkiness and stiffness characteristics when used as a filler in papermaking.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] The benefit of priority to U.S. Provisional Patent Application No. 63 / 326,240, filed on March 31, 2022, is hereby claimed, and the disclosure is incorporated herein by reference in its entirety. Technical Field

[0003] The present disclosure relates to composite fibers and methods for preparing composite fibers, and more particularly to methods of mineralizing nanocellulose with calcium carbonate and precipitating calcium carbonate to attach to the nanocellulose. Background Art

[0004] Various techniques for precipitating calcium carbonate are known in the art. Precipitated calcium carbonate (PCC) is used in various fine paper manufacturing, such as copy paper, mechanical grade paper such as SC, containers and paperboard. Various forms of precipitated calcium carbonate and cellulose calcium composites have been used as filler materials in the paper industry. Conventional cellulose calcium carbonate materials incorporate calcium carbonate, thereby maintaining the basic fiber properties of the cellulose component. It is generally recognized in the art that the fiber properties of composite materials are needed in order to better incorporate the composite materials into the fiber matrix of paper.

[0005] U.S. Patent No. 9,150,738 teaches a reverse carbonation process for forming precipitated calcium carbonate of various crystalline forms. It has been found that the reverse carbonation process is beneficial for particularly targeting the scalenohedral morphology. The '738 patent teaches a key feature, namely the initial addition of carbon dioxide to the reaction vessel until a controlled pH of 5-7 is obtained. After such pH control, a calcium hydroxide slurry is added at a rate such that the target conductivity is reached, thereby precipitating the calcium carbonate.

[0006] WO 97 / 01670 teaches porous aggregates of calcium carbonate particles deposited on the surface of cellulose fibers. EP 0 930 345 and EP 0 935 020 teach similar fillers, but without precipitation of calcium carbonate on the fiber surface, but mixed with the fibers. U.S. Pat. No. 10,683,616 teaches a method of producing a composite material by introducing microfibrillated cellulose during the calcium carbonate precipitation process after part of the calcium hydroxide has been reacted with carbon dioxide.

[0007] Surface mineralized fibers are also known, as disclosed in WO 2021 / 252572. Such fibers are typically produced by carbonation using sodium carbonate and have low fiber attachment. Summary of the invention

[0008] There is still a need in the art for improved filler materials. The fibers produced according to the methods of the present disclosure have significant improvements in mineral attachment. For various applications, minerals can be beneficially provided as long chains of scalenohedral PCC attached to nanocellulose fibers to improve properties.

[0009] The filler according to the present disclosure may comprise composite fibers, each composite fiber comprising a mineral attached to the fiber, wherein the mineral is at least about 90 wt % based on the total weight of the composite fibers, the average length of the uncoated fibers is less than 300 μm, and the Horiba d of the composite fibers is 90 is at least 10 μm. For example, the fibers may be nanocellulose and the mineral may be calcium carbonate.

[0010] A method for preparing composite fibers according to the present disclosure may include: preparing calcium hydroxide slake by diluting lime in water; mixing an aqueous fiber slurry with dilution water in a reactor; adding the calcium hydroxide slake and a gas containing CO2 to the reactor containing the aqueous fiber slurry mixed with the dilution water to precipitate calcium carbonate onto the fibers; and continuing to flow the gas containing CO2 into the mixture after starting the addition of the calcium hydroxide slake until the pH reaches 7.0. The calcium hydroxide slake is added at a rate to maintain a target conductivity, the target conductivity being 50% to 80% saturation, and the target conductivity is maintained until the addition of the calcium hydroxide slake is completed, the fiber slurry includes fibers having a length of 300 μm or less, and the fiber slurry includes an amount of fibers such that the fiber content in the composite fiber is 10 wt% or less based on the total weight of the composite fiber. The calcium hydroxide slake may be added simultaneously, before, or after starting the addition of CO2. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1A and 1B is a scanning electron microscopy (SEM) image of a composite fiber according to the present disclosure.

[0012] Figure 2 is a graph showing the changes in pH, conductivity, temperature, and gas flow over time for a process in accordance with the present disclosure.

[0013] Figure 3A and 3B is a SEM image of precipitated calcium carbonate (PCC) containing conventional fibers.

[0014] Figure 4Ais a graph showing comparative bulk properties of handsheets prepared with composite fiber fillers according to the present disclosure, precipitated calcium carbonate without nanocellulose, or PCC with added nanocellulose.

[0015] Figure 4B is a graph showing the comparative breaking lengths of handsheets prepared with composite fiber fillers according to the present disclosure, precipitated calcium carbonate without nanocellulose, and PCC with added nanocellulose.

[0016] Figure 4C is a graph showing the comparative bending resistance index of handsheets prepared with composite fiber fillers according to the present disclosure, precipitated calcium carbonate without nanocellulose, or PCC with added nanocellulose.

[0017] Figure 5A and 5B is a SEM image of a composite fiber according to the present disclosure.

[0018] Figure 5C and 5D is a SEM image of calcium carbonate precipitated using a reverse carbonation process at 50% saturation but without the presence of fibers.

[0019] Figure 6 is a SEM image of precipitated fiber-free calcium carbonate produced at 50% saturation and an initial carbonation temperature of 42°C.

[0020] Figure 7 is a SEM image of composite fibers produced according to the present disclosure using 50% saturation, with 0.5 wt% fiber and an initial carbonation temperature of 39°C.

[0021] Figure 8 is a SEM image of composite fibers produced according to the present disclosure using 50% saturation, with 0.5 wt% fiber and an initial carbonation temperature of 11°C.

[0022] Fig. 9 is a SEM image of composite fibers produced according to the present disclosure using 50% saturation, with 0.5 wt% fiber and an initial carbonation temperature of 26.5°C.

[0023] Fig.10 is a SEM image of composite fibers produced using 70% saturation, with 0.5 wt% fiber and an initial carbonation temperature of 26.5°C. DETAILED DESCRIPTION

[0024] When used as fillers in the manufacture of paper products, the composite fibers and methods of the present disclosure unexpectedly and beneficially provide improved bulk and strength properties. Typically, high-strength fillers are expected to densify the paper, adversely affecting the stiffness of the paper. Surprisingly, it has been found that the composite fibers of the present disclosure can improve both bulk and strength, thereby producing improved stiffness. In addition, the methods of the present disclosure can beneficially significantly increase the percentage of attached minerals. Still further, the methods of the present disclosure can allow for control of the mineral morphology, and can beneficially provide composite fibers in which all or substantially all of the minerals are present in a desired morphology, such as a scalenohedral morphology.

[0025] For example, the composite fibers of the present disclosure can have long chain scalenohedral minerals, such as scalenohedral calcium carbonate, attached to the fiber template, which can advantageously allow the composite fibers to maintain fibrous qualities when used as fillers in papermaking.

[0026] When used as fillers in papermaking, the composite fibers of the present disclosure can provide high bulk and stiffness, as well as good natural retention and drainage, while imparting higher physical strength. The process of the present disclosure results in significantly increased surface coverage of the fibers, wherein all or substantially all of the precipitated minerals are attached to the fibers.

[0027] Composite fibers according to the present disclosure comprise fibers and minerals attached thereto. For example, the minerals may be in the form of long chains attached to and surrounding the fibers, thereby covering the fibers, as shown in FIG1 . Based on the total weight of the fibers, the composite fibers have at least 90 wt % of the minerals. For example, based on the total weight of the composite fibers, the composite fibers may have about 0.5 wt % to about 10 wt % of the fibers. There must be a sufficient amount of fiber to precipitate all or substantially all of the minerals directly onto the fibers. It has been found that an amount of fiber less than 0.5 wt % results in too many unattached minerals. However, it has been found that an amount of fiber exceeding 10 wt % adversely affects the ability of the minerals to grow into scalenohedrons, and instead results in rhombic or cubic morphologies.

[0028] When included as a filler, the composite fiber according to the present disclosure advantageously exhibits fibrous properties. 90 At least about 10 μm, at least about 20 μm, at least about 25 μm, at least about 30 μm, at least about 40 μm or at least about 50 μm.

[0029] The fiber can be nanocellulose. Nanocellulose is a cellulose material having at least one dimension, such as nanometer fibril particle size or width, for example 100 nm or less. The length of the fiber is 300 μm or less. For example, before coating with a mineral, the length of the fiber can be about 100 μm to about 300 μm. For example, the length of the fiber can be about 200 μm. Any nanostructured cellulose can be used as a fiber.

[0030] The method for forming a composite fiber according to the present disclosure comprises forming an aqueous slurry containing fibers. Based on the total weight of the composite fiber, the amount of the fibers in the aqueous slurry is selected so that the fibers are present in the composite fiber in an amount of about 0.1 wt % to about 10 wt %, about 0.25 wt % to about 5 wt %, about 0.5 wt % to about 8 wt %, about 0.25 wt % to about 1 wt %. For example, based on the total weight of the composite fiber, the fiber can be present in an amount of about 0.1, 0.15, 0.2, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85, 0.9, 0.95, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, 5, 5.5, 6, 6.5, 7, 7.5, 8, 8.5, 9, 9.5, 10 wt%, or any range defined by such values. The solid content of the slurry can be about 0.1% to about 3%, about 0.1% to about 1%, about 0.5% to about 1.5%, about 0.1% to about 6%. Other suitable solids contents include 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.2, 1.4, 1.6, 1.8, 2, 2.2, 2.4, 2.6, 2.8, 3, or any range defined by such values. The aqueous fiber slurry is added to the reactor as a heel.

[0031] The mineral slake can be prepared by mixing a suitable mineral-containing material with water. For example, the mineral slake can be a calcium hydroxide slake. The calcium hydroxide slake is prepared by mixing lime with water. The ratio of water to lime can be about 4:1 to about 15:1, about 5:1 to about 10:1 or about 5:1 to about 7:1. For example, the ratio of water to lime can be 7:1. Lime and water can be mixed to form the slake. In various embodiments, the initial temperature of the water does not need to be controlled and can depend on the process water in the factory. For example, the initial water temperature can be 32°C. Once mixed, the slake can be optionally screened to remove larger sand particles. For example, the slake can be screened through a 30 mesh sieve, a 60 mesh sieve or a 200 mesh sieve.

[0032] The tailings may be mixed in a reactor, and then slaked and CO2-containing gas are added to precipitate minerals onto the fibers present in the tailings. The initial temperature of the reactor may be from about 1°C to about 50°C, from about 11°C to 45°C, or from about 35°C to about 50°C, but does not need to be controlled during the process.

[0033] For example, the slake can be added and then the CO2-containing gas can be flowed. Alternatively, the CO2-containing gas can be flowed and then the slake can be added shortly thereafter. For example, the two components can be added in any order within a few seconds (e.g., within 10 seconds) of each other.

[0034] The method of the present disclosure utilizes reverse addition, in which calcium hydroxide slake is metered into the tailings of the aqueous fiber, wherein the addition rate is controlled to limit the conductivity to about 50% to 80% saturation. The addition rate of the calcium hydroxide slake is controlled throughout the precipitation process to maintain the target conductivity. As used herein, "saturation" refers to the conductivity of the starting calcium hydroxide slurry in fully saturated form. A conductivity of about 70% saturation refers to a conductivity less than 70% of the conductivity of the starting calcium hydroxide slurry. Control of conductivity can be achieved within a range of about 1% of the reaction being completed. For example, the target conductivity can be 50% saturation, 60% saturation, 70% saturation, or 80% saturation. For example, the target conductivity can be 50% saturation. The actual conductivity value can vary depending on the conductivity of the starting slake and the reactor. However, the actual conductivity value for controlling the reaction at 70% saturation can be easily determined by measuring the conductivity of the slaked material before addition and setting the conductivity to less than 70% of the measured value. For example, 50% saturation can be maintained at a conductivity value of about 3000 μs / cm to 5500 μs / cm, depending on the starting conductivity of the slaked material as shown in the various examples.

[0035] It has been found that there is no need to strictly control the pH during the precipitation process. Once all the slaking material has been added, the flow of the CO2-containing gas can continue until the pH reaches 7.0.

[0036] The CO2-containing gas can be, for example, a blend of CO2 and air. For example, the gas or blended gas can contain from about 5% CO2 to about 100% CO2.

[0037] The process of the present disclosure can obtain composite fibers in a slurry. Due to the fiber properties of the resulting composite fibers, the slurry cannot be screened. The slurry can be used as is, for example, as a filler in papermaking. Alternatively, the composite fiber slurry can be dried to obtain a dried product, which can be used for other purposes.

[0038] Examples

[0039] Example 1

[0040] Mineralized nanocellulose fibers are prepared according to the method of the present disclosure. Calcium hydroxide slake is prepared by mixing water and lime in a mass ratio of 7:1. Specifically, 357g of lime is mixed with 2500ml of water. The starting temperature of the water is 32°C. The lime is added to the water while mixing at 750rpm and continued to mix for 15 minutes. The resulting slurry is screened through a number 200 mesh sieve to remove +200 mesh grit.

[0041] 147.48 g of nanocellulose with a solid content of 0.5% was diluted in 800 ml of water to form a slurry with a solid content of 0.5%-8% solids. The target PCC% in the PCC / fiber composition was 99. The addition amount of nanocellulose template was calculated as 1 wt% of the final product weight. Nanocellulose was first added to the reactor as a carbonator tailing and mixed at 1250 rpm. The initial temperature was 40.8°C. CO2 gas flowed into the reactor at a flow set point of 0.76 slm CO2 and 3.1 slm air. Within 10 seconds, the calcium hydroxide slake was then pumped to the carbonator tailing at a rate of 14 ml / min over 120 minutes. The addition rate of the slake was adjusted to maintain a conductivity of 4.5-5.0 ms / cm, which was 50% of the conductivity of the starting slake. Once all the slake was added, CO2 was continued to be added until the end point reaction of pH 7.0. Due to the fiber properties, the resulting product could not be screened at 325 mesh. FIG1 is a SEM image of the obtained composite fiber.

[0042] The Horiba particle size and BET surface area of ​​the obtained product were characterized. The characterization is shown in Table 1:

[0043]

[0044]

[0045] Figure 2 is a graph of the pH, conductivity and temperature trends during the reaction. It was found that pH at saturation was not a critical parameter controlling the process.

[0046] Example 2

[0047] Composite fibers were produced according to the method described in Example 1, except that CO2 addition was started after the calcium hydroxide slake was started. It was found that the order of CO2 addition and slake addition did not affect the composite fiber characteristics, and significantly, it was not necessary to control the pH before the calcium hydroxide slake to obtain good fiber properties. The following table provides a comparison of the fiber properties prepared according to Example 1 (CO2 was added before the slake) and this Example 2 (CO2 was added after the slake). Both examples were produced by maintaining 50% saturation of the tailing within 1% of the total reaction time.

[0048] <![CDATA[CO2 before ripening]]> <![CDATA[Pre-cured material before CO2]]> PCC content (%) 95.1 95.2 <![CDATA[Horiba d 90 (μm)]]> 11.99 11.96 <![CDATA[Horiba d 50 (μm)]]> 6.14 6.43 <![CDATA[Horiba d 20 (μm)]]> 3.78 4.04 <![CDATA[Horiba d 10 (μm)]]> 2.83 2.99 <![CDATA[(d 90 -d d10 ) / d 50 ]]> 1.49 1.40 <![CDATA[SSA(m2 / g)]]> 3.8 2.6

[0049] Example 3

[0050] Composite fibers produced according to Example 1 were tested in the production of copy paper handsheets. Composite fibers of the present disclosure were compared to standard precipitated calcium carbonate, and methods of adding nanocellulose were provided.

[0051] Conventional nanocellulose containing precipitated calcium carbonate is formed by adding nanocellulose as a precursor additive to the calcium hydroxide slurry before passing CO2 gas through it to precipitate calcium carbonate at 100% saturation. Referring to Figure 3, conventional nanocellulose-containing PCC shows less attachment and a very different morphology as compared to the composite fibers of the present disclosure. As shown in the table below, there are significant differences in the particle size distribution of conventional nanocellulose PCC and the composites of the present disclosure, especially in terms of d90 and d50, which indicates that there is less fiber material in conventional nanocellulose PCC. Conventional nanocellulose PCC exhibits a loose hanging monohedral morphology. In Figure 4, nanocellulose 1 and nanocellulose 2 refer to samples prepared using the same method of the present disclosure, but with different fiber types of similar particle sizes. It was found that this morphology is more sensitive to the shear force of the paper machine.

[0052]

[0053] Copy paper handsheets were prepared with eucalyptus pulp refined to 400 Canadian Standard Freeness. The handsheets were produced at a target basis weight of 80 gsm. The filler level was adjusted to reach a target level of 15%, 25%, 35% or 50%. Additives were added as follows: cationic starch (Stalok 310) was added at 3 kg / ton of paper, filler was added at a target level, and retention aid (Percol 175) was added at 0.01 kg / ton of paper. All chemicals were added dry-to-dry. The handsheets were formed on a Formax (Nobel and Wood) paper former. The paper was pressed at 4 psi while it was still on the forming line sandwiched between several sheets of paper machine felt material. The handsheet was then removed from the forming line and sandwiched between two unsized blotting papers and pressed at 25 psi. The handsheet was then dried on a drum dryer at 125°C for 1 minute. Finally, the handsheets were conditioned at 23°C and 50% relative humidity.

[0054] The composite fibers of the present disclosure show unexpected improvements in both bulk properties and strength. Figure 4A , compared with the use of conventional nanocellulose ( Figure 4A Compared with the hand sheets produced by using the nanocellulose 1 and nanocellulose 2 in the present invention, the hand sheets produced by using the composite fibers of the present invention have significant improvements in bulkiness. Figure 4B and 4C The handsheets produced using the composite fibers also exhibited higher strength, as compared to handsheets produced using standard PCC, and improved flexural properties, as compared to handsheets produced using standard PCC or conventional nanocellulose.

[0055] Example 4

[0056] To analyze the performance benefits imparted by the presence of fibers, composite fibers were prepared according to the method described in Example 1 (maintaining 50% saturation) and compared with precipitated calcium carbonate produced using the same method (except that no fibers were present in the tailings). The following table shows the properties of the resulting calcium carbonate produced with and without fibers:

[0057]

[0058] It was found that in the absence of nanocellulose, the precipitated calcium carbonate was in the form of non-fibrous macro-calcium carbonate structures, e.g. Figure 5C and 5D In contrast, the fiber properties of the composite fibers disclosed herein can be Figure 5A and 5BCalcium carbonate produced without fibers also does not scatter light due to the larger structure. Without intending to be bound by theory, it is believed that calcium carbonate produced without fibers will densify the paper, thereby reducing bulk and stiffness. Further, without intending to be bound by theory, it is believed that non-fibrous calcium carbonate is not well retained in paper due to its low specific surface area and non-acicular nature.

[0059] Example 5

[0060] The composite material produced on a large scale according to the present disclosure was produced using nanocellulose produced at the University of Maine. The average fiber length of the nanocellulose was 224 μm and the fiber width was 21.9 μm. The product had 74.7% fines, a kink index of 1.2, a kink angle of 13.96, and an average curl of 0.114.

[0061] The slake was prepared by diluting lime to a target slake solids of 15-17% and screened through a 60 mesh screen and then discharged to 470 gallons. The slake was maintained at about 50-55°C using heating coils in the slake storage tank.

[0062] Water was added to the reactor and heated to the target starting temperature if necessary. The starting temperature was 11°C, 25°C or 40°C. Once the target starting temperature was reached, the water was discharged to 202 gallons as the target starting volume. The water was stirred at half speed and Aqua nanocellulose was added at an addition rate of 0.5 wt% dry nanocellulose based on the slake volume and slake concentration (MO) by dry total final product weight. The stirring was then adjusted to full speed and the tailing of the aqueous fiber was mixed for 5 minutes.

[0063] The CO2-containing gas was flowed into the reactor as a blend of CO2 and air at the target flow rates specified in the table below. Once the gas reached its full flow rate, the slake addition was pumped from the slake storage tank into the reactor using a Moyno pump. Slake was added at a rate to maintain about 50% saturation (conductivity values ​​of 3.0-3.5 ms / cm) or about 70% saturation (conductivity values ​​of 4.0-4.5 ms / cm). Once all the slake was added, the reaction mixture was aerated until pH 7.0 was reached. One liter and five gallon samples were collected for characterization.

[0064] A comparative sample without added fiber was also produced using the same procedure except that no fiber was added to the aqueous tailings. The conditions tested and the resulting calcium carbonate properties are shown in the table below.

[0065]

[0066]

[0067]

[0068]

[0069]

[0070] Figure 6 is a SEM image of precipitated calcium carbonate without fibers. Figure 7-9 Contains SEM images of composite fibers produced according to the present disclosure using 50% saturation at different starting hydrothermal temperatures. The resulting composite fibers have a precipitated calcium carbonate morphology, primarily a mixture of scalenohedral and prismatic calcite. A starting temperature of 11°C results in a smaller, narrower particle size distribution and slightly higher surface area than using a higher tailing starting temperature.

[0071] Fig.10 Contains SEM images of composite fibers produced at 70% saturation. The resulting composite fibers have a narrower particle size distribution, higher surface area, and more scalenohedral morphology than the product prepared at 50% saturation.

[0072] aspect

[0073] Aspect 1. A filler comprising composite fibers, each composite fiber comprising a mineral attached to the fiber, wherein the mineral is at least about 90 wt% based on the total weight of the composite fibers, the average length of the uncoated fibers is less than 300 μm, and the Horiba d of the composite fibers is 90 is at least 10 μm.

[0074] Aspect 2. The filler according to aspect 1, wherein the mineral is calcium carbonate and the fiber is nanocellulose.

[0075] Aspect 3: The filler according to aspect 1 or 2, wherein the Horiba d 90 is at least 20 μm.

[0076] Aspect 4. The filler according to any one of aspects 1 to 3, wherein the fiber is present in an amount of about 0.1 wt% to about 10 wt% based on the total weight of the composite fiber.

[0077] Aspect 5. The filler according to any one of aspects 1 to 4, wherein the average length of the fibers is from 100 μm to less than 300 μm.

[0078] Aspect 6. The filler according to aspect 5, wherein the average length of the fibers is about 200 μm.

[0079] Aspect 7. The filler according to any one of aspects 1 to 6, wherein the fiber is nanocellulose.

[0080] Aspect 8. The filler according to any one of aspects 1 to 7, wherein the mineral has a scalenohedral morphology.

[0081] Aspect 9. A method for preparing a composite fiber, the method comprising:

[0082] Calcium hydroxide slake is prepared by diluting lime in water;

[0083] mixing an aqueous fiber slurry with dilution water in a reactor;

[0084] adding the calcium hydroxide slake and a CO2-containing gas to the reactor containing the aqueous fiber slurry mixed with the dilution water to precipitate calcium carbonate onto the fibers; and

[0085] After starting the addition of the calcium hydroxide slaked material, continuing to flow the CO2-containing gas into the mixture until the pH reaches 7.0, wherein:

[0086] adding the calcium hydroxide slake at a rate to maintain a target conductivity, the target conductivity being 50% to 80% saturation, and maintaining the target conductivity until the addition of the calcium hydroxide slake is complete,

[0087] The fiber slurry includes fibers having a length of 300 μm or less, and

[0088] The fiber slurry includes fibers in an amount such that a fiber content in the composite fibers is 10 wt% or less based on the total weight of the composite fibers.

[0089] Aspect 10. The method according to aspect 9, wherein the calcium carbonate has a scalenohedral morphology.

[0090] Aspect 11. The method according to aspect 9 or 10, wherein the addition of the calcium hydroxide slaked material is started before the addition of the gas including carbon dioxide is started.

[0091] Aspect 12. The method according to aspect 9 or 10, wherein the adding of the calcium hydroxide slaked material is started after the adding of the gas including carbon dioxide is started.

[0092] Aspect 13. The method according to any one of aspects 9 to 12, wherein the aqueous fiber slurry is mixed while adding the calcium hydroxide slaked material and the gas including carbon dioxide.

[0093] Aspect 14. The method according to any one of aspects 9 to 13, wherein the solids content of the aqueous fiber slurry is about 0.1% to 3% solids.

[0094] Aspect 15. The method of aspect 14, wherein the aqueous fiber slurry has a solids content of less than about 1%.

[0095] Aspect 16. The method according to any one of aspects 9 to 15, wherein the calcium hydroxide slaked material comprises water and lime in a mass ratio of about 4:1 to about 15:1.

[0096] Aspect 17. The method according to any one of aspects 9 to 16, wherein the calcium hydroxide slake is screened through a 40-200 mesh size screen before being added to the aqueous fiber slurry.

[0097] Aspect 18. The method according to any one of aspects 9 to 17, wherein the calcium hydroxide is added at a rate to maintain a certain conductivity, the conductivity being about 50% to about 70% of saturation.

[0098] Aspect 19. The method according to any one of aspects 9 to 18, wherein the target conductivity is reached and maintained after 1% or less of the reaction is completed.

[0099] Aspect 20. The method according to any one of aspects 9 to 19, wherein the gas comprising carbon dioxide comprises about 5% to about 100% carbon dioxide.

[0100] Aspect 21. The method according to any one of aspects 9 to 20, wherein the fiber is nanocellulose.

[0101] Modifications and other embodiments disclosed herein will occur to those skilled in the art of the disclosed compositions and methods having benefit of the teachings presented in the foregoing description. Therefore, it should be understood that the disclosure should not be limited to the specific embodiments disclosed, and modifications and other embodiments are intended to be included within the scope of the appended claims. Although specific terms are employed herein, they are used in a general and descriptive sense only, and not for the purpose of limitation.

[0102] It should also be understood that the terminology used herein is for the purpose of describing particular aspects only and is not intended to be limiting. As used in the specification and in the claims, the term "comprising" may include the aspect "consisting of". Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the disclosed compositions and methods belong. In this specification and the claims that follow, reference will be made to a number of terms that shall be defined herein.

[0103] As will be apparent to those skilled in the art upon reading this disclosure, each of the individual embodiments described and illustrated herein has discrete components and features that can be readily separated or combined with the features of any other several embodiments without departing from the scope or spirit of the present disclosure. Any recited method can be performed in the order of events recited or in any other order that is logically possible.

[0104] Unless otherwise indicated, the terms "a / an", "the" and similar referents used in the context of the disclosure herein (particularly in the context of the claims) should be interpreted as covering both the singular and the plural. Unless otherwise indicated herein, the recitation of a range of values ​​herein is intended only to serve as a shorthand method of individually referring to each individual value falling within the range, and each individual value is incorporated into this specification as if individually recited herein. Unless otherwise indicated, the use of any and all examples or exemplary language (e.g., "such as") provided herein is intended to better illustrate the disclosure herein and is not a limitation on the scope of the disclosure herein. No language in this specification should be interpreted as indicating any unclaimed element as being essential to practicing the disclosure herein.

Claims

1. A filler comprising composite fibers, each composite fiber comprising a mineral attached to the fiber, wherein the mineral is at least about 90 wt% based on the total weight of the composite fibers, the average length of the uncoated fibers is less than 300 μm, and the Horiba d of the composite fibers is 90 is at least 10 μm.

2. The filler according to claim 1, wherein the mineral is calcium carbonate and the fibers are nanocellulose.

3. The filler according to claim 1 or 2, wherein the Horiba d 90 is at least 20 μm.

4. The filler of claim 1, wherein the fiber is present in an amount of about 0.1 wt% to about 10 wt% based on the total weight of the composite fiber. 5 . The filler according to claim 1 , wherein the average length of the fibers is from 100 μm to less than 300 μm.

6. The filler of claim 5, wherein the average length of the fibers is about 200 μm. The filler according to claim 1 , wherein the fibers are nanocellulose.

8. The filler of claim 1, wherein the mineral has a scalenohedral morphology.

9. A method for preparing a composite fiber, the method comprising: Calcium hydroxide slake is prepared by diluting lime in water; mixing an aqueous fiber slurry with dilution water in a reactor; adding the calcium hydroxide slake and a CO2-containing gas to the reactor containing the aqueous fiber slurry mixed with the dilution water to precipitate calcium carbonate onto the fibers; as well as After starting the addition of the calcium hydroxide slaked material, continuing to flow the CO2-containing gas into the mixture until the pH reaches 7.0, wherein: adding the calcium hydroxide slake at a rate to maintain a target conductivity, the target conductivity being 50% to 80% saturation, and maintaining the target conductivity until the addition of the calcium hydroxide slake is complete, The fiber slurry includes fibers having a length of 300 μm or less, and The fiber slurry includes fibers in an amount such that a fiber content in the composite fibers is 10 wt% or less based on the total weight of the composite fibers.

10. The method of claim 9, wherein the calcium carbonate has a scalenohedral morphology.

11. The method according to claim 9 or 10, wherein the addition of the calcium hydroxide slake is started before the addition of the gas comprising carbon dioxide is started.

12. The method according to claim 9 or 10, wherein said adding of calcium hydroxide slake is started after said adding of said gas comprising carbon dioxide is started.

13. The method of claim 9, wherein the aqueous fiber slurry is mixed while adding the calcium hydroxide slaked material and the gas comprising carbon dioxide.

14. The method of claim 9, wherein the solids content of the aqueous fiber slurry is about 0.1% to 3% solids.

15. The method of claim 14, wherein the aqueous fiber slurry has a solids content of less than about 1%.

16. The method of claim 9, wherein the calcium hydroxide slake comprises water and lime in a mass ratio of about 4:1 to about 15:

1.

17. The method of claim 9, wherein the calcium hydroxide slake is screened through a 40 to 200 mesh size screen before being added to the aqueous fiber slurry.

18. The method of claim 9, wherein the calcium hydroxide is added at a rate to maintain a conductivity of about 50% to about 70% saturation.

19. The method of claim 9, wherein the target conductivity is achieved and maintained after 1% or less of the reaction is complete.

20. The method of claim 9, wherein the gas comprising carbon dioxide comprises from about 5% to about 100% carbon dioxide.

21. The method of claim 9, wherein the fibers are nanocellulose.