Optical module and manufacturing method thereof

By forming electrode pads on optical semiconductor elements and insulating substrates and ultrasonic bonding using Au bumps, the characteristics deterioration and thermal stress problems caused by lead connection in optical modules are solved, and the optical modules are miniaturized and high-density and high-speed and large-capacity, improving reliability and yield.

CN119013856APending Publication Date: 2024-11-22MITSUBISHI ELECTRIC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280094532.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-04-28
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the process of improving the installation density and transmission capacity of existing optical modules, there are deterioration in characteristics caused by lead connection, thermal stress problems, and insufficient reliability of bump joints, making it difficult to achieve miniaturization, high density and high-speed and large-capacity. Optical module.

Method used

Electrode pads are formed on the surface of the optical semiconductor element and the back of the insulating substrate, and ultrasonic bonding is performed through Au bumps. The back electrode pads of the insulating substrate are connected to the surface electrode pads through through holes to realize electrical and mechanical bonding and reduce leads. In combination, the frequency characteristics are improved and thermal stress is reduced by optimizing bump configuration and manufacturing methods.

Benefits of technology

The optical module is miniaturized, high-densified and high-speed and large-capacity, which improves reliability and yield, reduces the area and load required for installation, and avoids the deterioration of characteristics and thermal stress caused by the bonding of leads.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119013856A_ABST
    Figure CN119013856A_ABST
Patent Text Reader

Abstract

An optical semiconductor device is provided with an optical semiconductor element (10) having electrode pads (10b) formed on the front surface thereof, an insulating substrate (30) having electrode pads (30b, 30c) formed on the front surface and the rear surface thereof, and Au bumps (50) that join the electrode pads (30b) on the rear surface of the insulating substrate (30) and the electrode pads (10b) of the semiconductor element (10), the rear surface of the insulating substrate (30) being disposed so as to face the front surface of the semiconductor element (10). The electrode pad (30b) on the rear surface of the insulating substrate (30) is connected to the electrode pad (30c) on the front surface of the insulating substrate (30) via the through-hole (30d).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to an optical module and a method for manufacturing the same. Background Art

[0002] Optical transceivers with built-in optical modules are indispensable components in optical communication systems. However, in order to accommodate the increasing data traffic, optical communication networks are required to be high-speed and high-capacity. Although the transmission capacity can be increased by improving the installation density and characteristics of optical modules, in order to increase the installation density, the miniaturization of components in optical modules and high-density installation technology are required.

[0003] Conventionally, optical semiconductor elements are assembled by wire bonding. However, since wire bonding connects the optical semiconductor element to the insulating substrate via wires, other components cannot overlap the surface where the electrode pads are formed. Furthermore, since a backward wave is generated between the optical semiconductor element and the insulating substrate, there is a problem of significant characteristic degradation.

[0004] In order to solve this problem, for example, Patent Document 1 discloses a flip chip bonding technology in which an optical semiconductor element is inverted and connected to an insulating substrate via a terminal on a protrusion called a bump, and in particular, a technology using ultrasonic bonding is disclosed as a method that is generally excellent in terms of cost, connection reliability, bonding load, connection pitch accuracy, etc. Flip chip bonding using ultrasonic bonding is usually performed by attaching the inverted back surface of the optical semiconductor element to a suction chuck, and mounting the optical semiconductor element on the surface of an insulating substrate having a larger projection area than the optical semiconductor element.

[0005] Patent Document 1: Japanese Patent Application Laid-Open No. 2012-009599 (Paragraphs 0026 to 0029, Figure 2 )

[0006] However, since the wiring for electrically connecting the insulating substrate to the electronic circuit outside the optical module uses wire bonding as in the past, there is a problem that in addition to the electrode pads connected to the optical semiconductor element, an area for forming the electrode pads for wire bonding with other surrounding components must be ensured on the same surface of the insulating substrate. In addition, in order to fix the optical semiconductor element in the optical module, it is necessary to bond it with components such as submounts by solder, etc., so there is a problem that the reliability of the bump joint is impaired due to the increase in thermal stress caused by preheating during flip-chip mounting, heat caused by driving the optical semiconductor element, and the difference in linear expansion coefficient between the surrounding components caused by cooling. In addition, there is a problem that stress is generated in the bump joint due to the pressure and vibration generated when wire bonding is performed on the surface of the insulating substrate mounted on the optical semiconductor element, which easily causes the joint to be damaged. Summary of the invention

[0007] The present application has been made to solve the above-mentioned problems, and an object of the present application is to provide an optical module that is small in size and high in density, has high speed and large capacity, and has high reliability, and a method for manufacturing the same.

[0008] The optical module disclosed in the present application is characterized in that it comprises: a semiconductor element having electrode pads formed on the surface; an insulating substrate having electrode pads formed on the surface and the back surface; and a bump for joining the electrode pads on the back surface of the insulating substrate to the electrode pads of the semiconductor element, wherein the back surface of the insulating substrate is configured to be opposite to the surface of the semiconductor element, and the electrode pads on the back surface of the insulating substrate are connected to the electrode pads on the surface of the insulating substrate via a through hole.

[0009] The manufacturing method of the optical module disclosed in the present application is characterized in that it includes the following steps: providing a bump on the surface of an electrode pad formed on the surface of a semiconductor element, or on the surface of an electrode pad formed on the back side of an insulating substrate, and placing the insulating substrate on the semiconductor element at a position where the electrode pad of the semiconductor element and the electrode pad of the insulating substrate are opposite to each other; heating the bump while the insulating substrate is placed on the semiconductor element; and performing ultrasonic bonding while pressurizing the electrode pad of the insulating substrate or the electrode pad of the semiconductor element and the bump.

[0010] According to the present application, it is possible to obtain an optical module that can achieve miniaturization and high density, high speed, large capacity, and high reliability. BRIEF DESCRIPTION OF THE DRAWINGS

[0011] Figure 1 It is a cross-sectional view showing the structure of the optical module according to the first embodiment.

[0012] Figure 2 This is an enlarged cross-sectional view showing the structure of the optical module according to the first embodiment.

[0013] Figure 3 It is a plan view showing the structure of a conventional optical module.

[0014] Figure 4 It is a plan view showing another structure of a conventional optical module.

[0015] Figure 5 It is a plan view showing the structure of the optical module according to the first embodiment.

[0016] Figure 6 It is a plan view showing the structure of an optical module according to the second embodiment.

[0017] Figure 7It is a plan view showing the arrangement of bumps of the optical module according to the second embodiment and other optical modules.

[0018] Figure 8 This is a diagram showing the relationship between the arrangement of bumps and stress in the optical module according to the second embodiment.

[0019] Fig. 9 It is a cross-sectional view showing a method for manufacturing an optical module according to the third embodiment.

[0020] Fig.10 It is a plan view showing the optical module manufacturing method according to the fourth embodiment. DETAILED DESCRIPTION

[0021] Hereinafter, the optical module involved in the embodiment will be described with reference to the accompanying drawings. In addition, the same reference numerals are marked for the same structural components or the same structural components in each figure. In addition, in order to avoid the following description being insufficient and lengthy and to facilitate the understanding of the parties, detailed descriptions of well-known matters and repeated descriptions of substantially the same structure are sometimes omitted. In addition, the contents of the following description and the accompanying drawings are not intended to limit the subject matter recorded in the scope of the claims.

[0022] In addition, the sizes or scales of the corresponding structural parts are independent of each other between the figures. For example, the sizes or scales of the same structural part are sometimes different between the figure obtained by changing a part of the structure and the figure without changing it. In addition, although the structure of the optical module is equipped with multiple parts in practice, in order to simplify the description, only the parts required for the description are recorded, and the description of other parts is omitted.

[0023] In the following description, although an optical module is used as an example, each embodiment is also applicable to a semiconductor device for power or a semiconductor device for handling normal current that has the same problem instead of light.

[0024] Implementation Method 1

[0025] Figure 1 It is a cross-sectional view showing the structure of an optical module 1001 according to the first embodiment of the present application. Figure 1 (a) is a cross-sectional view of the optical module 1001. Figure 1 (b) is the optical module 1001 in Figure 1 (a) is a cross-sectional view taken at the AA position. Figure 2 yes Figure 1 An enlarged cross-sectional view of region B in (a).

[0026] like Figure 1As shown in (a) and (b) of FIG. 1 , the optical module 1001 includes an optical semiconductor element 10, a submount 20, and an insulating substrate 30 as basic components. The back surface of the optical semiconductor element 10 is bonded to the electrode pad 20b on the surface of the submount 20 via the electrode pad 10c by solder 70, and the back surface of the insulating substrate 30 is ultrasonically bonded to the surface of the optical semiconductor element 10 opposite to the back surface bonded to the submount 20 via the electrode pad 10b and the electrode pad 30b by Au bumps 50, respectively. The surface of the insulating substrate 30 is provided with an Au lead 60 via the electrode pad 30c, and is electrically connected to the outside via the IC 110 bonded to the housing 100 by solder 70.

[0027] The electrode pad 20c of the submount 20 is bonded to the surface of the thermal module 40 via the metallized portion 40a and through the Ag paste 80, and the lens 120 and the combiner 130 are bonded to the same surface of the thermal module 40 as the surface to which the submount 20 is bonded and at a position corresponding to the laser output direction of the optical semiconductor element 10, respectively, by a resin adhesive 90.

[0028] The thermal module 40 is accommodated in the housing 100 , and the rear surface of the thermal module 40 opposite to the surface on which the submount 20 and the lens 120 are provided is bonded to the housing 100 by the Ag paste 80 via the metallization portion 40 b .

[0029] The following is a more detailed description. Figure 1 Only basic components of the optical module 1001 are shown, and other components such as optical semiconductor elements, ICs, Au leads, capacitors, and FPCs are not shown.

[0030] The optical semiconductor element 10 is equivalent to LD (Laser Diode) and PD (Photo Diode) that convert electrical signals into optical signals or perform reverse conversion, and is composed of, for example, InP, GaAs, GaN, InGaAs, Ge, Si, etc. In the first embodiment, a Mach-Zehnder modulator (hereinafter referred to as MZ modulator) composed of InP is used. Among them, the number of laser generating parts of the optical semiconductor element 10 is not limited, but in the first embodiment, a plurality of laser generating parts are formed, which makes the effect of the present application more effective.

[0031] Since the optical semiconductor element 10 is electrically and mechanically bonded to the insulating substrate 30 via the Au bumps 50 , the dummy pads for mechanically fixing the electrode pads 10 b electrically connectable to the insulating substrate 30 and the insulating substrate 30 are formed of the Au metallization portion.

[0032] In the first embodiment, one MZ modulator is mounted in the optical module 1001 . However, other optical semiconductor elements not described in this application because they do not need to be described are also mounted in the optical module 1001 , and the number of optical semiconductor elements 10 is not limited to one.

[0033] like Figure 1 As shown in (b), the submount 20 includes a ceramic substrate 20a, an electrode pad 20b formed on the surface of the ceramic substrate 20a, and an electrode pad 20c formed on the back surface. The ceramic substrate 20a is an electrical insulator, and in order to effectively cool the optical semiconductor element 10, a material with high thermal conductivity is preferably used, such as AlN, Al 2 O 3 And other ceramic plates.

[0034] In the first embodiment, the number of submounts 20 mounted on the optical module 1001 is one, but the number of submounts 20 is not limited to one. A plurality of optical semiconductor elements may be bonded to one submount.

[0035] Usually, the electrode pads 20b and 20c are made of the same material. The optical semiconductor element 10 is soldered to the electrode pad 20b formed on the circuit surface side by solder 70, and the electrode pad 20b forms a joint with the Au wire 60, etc., thereby being electrically connected to the surrounding components and the surface of the optical semiconductor element 10. Since such an electrode pad 20b is a wiring component for electrically connecting the optical semiconductor element 10 to an external circuit, a metal with low resistance is preferably used.

[0036] Regarding the electrode pads 20b and 20c, a metallization portion based on Au or the like with a thickness of 3.0 μm or less can be used. In the first embodiment, a submount 20 is used in which an electrode pad 20b composed of Au with a thickness of 1.0 μm is metallized on a ceramic substrate 20a composed of AlN with a thickness of 0.5 mm, and AuSn solder 70 with a thickness of 5 μm is pre-coated on the electrode pad 20b at a location to be soldered to the optical semiconductor element 10.

[0037] The electrode pad 20 c on the back surface corresponding to the heat dissipation surface side is mechanically and thermally connected to the inner wall of the case 100 via solder or Ag paste, etc. In the first embodiment, the connection is made by Ag paste 80 .

[0038] like Figure 2 As shown, similar to the submount 20, the insulating substrate 30 includes a ceramic substrate 30a, an electrode pad 30b formed on the back of the ceramic substrate 30a, and an electrode pad 30c formed on the surface. The ceramic substrate 30a is an electrical insulator, and AlN, Al 2 O 3In the first embodiment, the insulating substrates 30 mounted in the optical module 1001 are ultrasonically bonded to the optical semiconductor element 10 via the Au bumps 50 , but the number of insulating substrates 30 is not limited and may be one or more.

[0039] Usually, the electrode pad 30b and the electrode pad 30c are made of the same material. The electrode pad 30b formed on the back of the ceramic substrate 30a is bonded to the electrode pad 10b on the surface of the optical semiconductor element 10 through the Au bump 50, and the electrode pad 30b bonded to the optical semiconductor element 10 is electrically connected to the electrode pad 30c on the surface through the through hole 30d and the side metallization part. The electrode pad 30c electrically connected to the electrode pad 30b forms a joint with the Au lead 60, etc., thereby further electrically connected to the surrounding components. Since such electrode pads 30b and 30c are wiring components for electrically connecting the optical semiconductor element 10 to an external circuit, metal with low resistance is preferably used.

[0040] Electrode pads 30b and 30c are usually metallized with Au or the like with a thickness of 3.0 μm or less, for example. In the first embodiment, electrode pads 30b and 30c made of Au with a thickness of 1.0 μm are metallized on a ceramic substrate 30a made of AlN with a thickness of 0.25 mm, and the electrode pads 30b and 30c are electrically connected via a through hole 30d provided in the ceramic substrate 30a. In addition, the electrode pad 30c is electrically connected to the IC 110 via an Au wire 60.

[0041] The thermal module 40 transfers the heat received by the heat absorbing part to the heat dissipating part via the Peltier element, and releases the heat from the heat dissipating part to, for example, the housing 100. Thus, the temperature of the optical semiconductor element 10 is controlled by the thermal module 40. Thus, the optical semiconductor element 10 can continue to operate stably.

[0042] like Figure 1 As shown, the thermal module 40 has the surface bonded to the submount 20 as the main surface, and is bonded to the housing 100 by the Ag paste 80 in a manner such that the main surface faces the positive direction of the Z axis. To this end, a metallized portion 40a is formed on the bonding surface of the submount 20, the lens 120, and the combiner 130 with the thermal module 40, and a metallized portion 40b is formed on the bonding surface bonded to the housing 100 by the Ag paste 80.

[0043] The metallization parts 40a and 40b are usually made of the same material. For example, Au or the like having a thickness of about 3.0 μm or less is used for the metallization parts 40a and 40b.

[0044] The Au bump 50 electrically and mechanically connects the electrode pad 10b and the dummy pad (not shown) formed on the surface of the optical semiconductor element 10 to the electrode pad 30b formed on the back surface of the insulating substrate 30. A metal with a high thermal conductivity is preferably used as the material of the Au bump 50. For this purpose, Au, Cu, Al, solder, etc. are usually used alone or in combination, and joined by heating, pressurization, ultrasonic waves, soldering, etc.

[0045] In the first embodiment, the bumps formed by cutting the wires after first bonding the electrode pads 30b formed on the insulating substrate 30 by Au wire bonding (ball bonding) are bonded to the electrode pads 10b and dummy pads of the optical semiconductor element 10 by ultrasonic waves. diameter Au lead, the bump size is The height to the end is about 45 μm.

[0046] The Au wire 60 electrically connects the electrode pad 30c formed on the surface of the insulating substrate 30 to the IC 110 and the electrode pad 20b formed on the surface of the submount 20. A metal with low resistance is preferably used as the material of the Au wire 60. For this purpose, Au, Cu, Al and other materials are usually used alone or in combination, and are mainly bonded by ultrasonic waves.

[0047] In this embodiment 1 Figure 1 In the present invention, the electrode pad 30c formed on the insulating substrate 30 is joined to the IC 110, and the IC 110 is joined to the housing 100 by Au wire bonding (ball welding). However, since it is also used in the connection between other components that are omitted in the present application because no explanation is needed, the specification parts of the Au wire 60 are not limited to two parts.

[0048] The solder 70 joins the electrode pad 20b formed on the surface of the submount 20 with the electrode pad 10c formed on the back surface of the optical semiconductor element 10. When the optical semiconductor element 10 and the submount 20 are joined by the solder 70, the submount 20 is not yet bonded to the thermal module 40 by the Ag paste 80. Therefore, in order to prevent the solder 70 from melting again when joining by the Ag paste 80, the material of the solder 70 is preferably a metal having a melting point higher than the solidification temperature of the Ag paste 80 and a large thermal conductivity. For this purpose, the solder 70 generally uses an alloy containing Sn, Pb, Au, Ag, Cu, Zn, Ni, Sb, Bi, In, Ge, etc. and having a melting point lower than 450°C, and preferably uses an alloy mainly containing Sn, Au, Ag, Cu, etc. and having a melting point of 200°C or more. In addition, from the viewpoint of the inclination and bending of the element, the thickness of the solder 70 is preferably 0.1 mm or less. In the first embodiment, eutectic solder of Sn and Au is used.

[0049] The Ag paste 80 bonds the electrode pad 20c formed on the back of the submount 20 to the metallized portion 40a formed on the surface of the thermal module 40, and the metallized portion 40b formed on the back of the thermal module 40 to the housing 100. When the submount 20 and the thermal module 40 are bonded by the Ag paste 80, the optical semiconductor element 10 is already bonded to the submount 20 by the solder 70. Therefore, in order to prevent the solder 70 from melting again during the bonding of the Ag paste 80, the material of the Ag paste 80 is preferably a material having a lower curing temperature than the melting point of the solder 70 and having a high thermal conductivity. For this reason, the Ag paste 80 is generally made of a conductive adhesive in which a conductive filler made of a metal such as Au, Ag, Cu in a spherical or flake shape is blended in an organic adhesive such as epoxy and phenol. However, as long as bonding or bonding can be performed at a temperature at which the solder 70 is no longer melted and the thermal conductivity is high, bonding based on metal materials such as solder and sintered materials and insulating adhesives that do not contain metals may also be used. In the first embodiment, Ag paste 80 in which flaky Ag particles are blended in an epoxy-based adhesive is used.

[0050] The resin adhesive 90 bonds the lens 120 to the metallized portion 40a formed on the surface of the thermal module 40, and the combiner 130 to the metallized portion 40a, respectively. When the components are bonded by the resin adhesive 90, the optical semiconductor element 10 is already bonded to the submount 20 by the solder 70. Therefore, in order to prevent the solder 70 from melting again when the resin adhesive 90 is bonded, the material of the resin adhesive 90 is preferably a material having a curing temperature lower than the melting point of the solder 70, and having a viscosity to the extent that it does not wet and spread around, and a viscosity to the extent that the lens 120 and the combiner 130 do not move when mounted. More preferably, a resin that can be cured and bonded by a method other than heating, such as ultraviolet irradiation, is preferred. In addition, in the first embodiment, since the metallized portion 40a and the lens 120, and the metallized portion 40a and the combiner 130 bonded by the resin adhesive 90 are not conductive paths, the resin adhesive 90 does not need to have conductivity.

[0051] The housing 100 is a flat box having a flat bottom bonded to the metallized portion 40b formed on the back of the thermal module 40 by the Ag paste 80, a plurality of side portions connected to the outer edge of the bottom, and an opening surrounded by the plurality of side portions. Figure 1 As shown, an emission portion is provided on one side of the housing 100 , and the emission portion is used to guide the laser beams multiplexed by the multiplexer 130 to an optical fiber (not shown).

[0052] The lens 120 is made of glass or transparent resin, and focuses the laser light emitted from the optical semiconductor element 10. In the first embodiment, only one lens 120 is shown, but the number of lenses 120 may vary depending on the number of light sources of the optical semiconductor element 10. Figure 1 There are multiple ones installed in the depth direction, not limited to one.

[0053] The multiplexer 130 multiplexes the outgoing light from the optical semiconductor element 10 and outputs the multiplexed light. The multiplexed light output from the multiplexer 130 passes through the lens 120 provided in the housing 100 as a wavelength division multiplexed signal and is transmitted to an optical waveguide such as an optical fiber.

[0054] Figure 3 This is a top view showing the structure of a conventional optical module. Conventional optical modules are equipped with a plurality of optical semiconductor elements 10 in order to increase transmission capacity, and many components such as lenses and combiners must be mounted. However, since the outer diameter of the housing of the optical module is determined, a high-density mounting technology is required in order to mount all the mounted components in the housing.

[0055] In the conventional optical module, the optical semiconductor element 10 and the submount 20 are connected to the insulating substrate 30 by wire bonding using Au wires 60. However, in wire bonding, it is difficult to arrange the components in an overlapping manner, and a reverse wave is generated between the optical semiconductor element 10 and the insulating substrate 30, which may cause significant degradation of characteristics.

[0056] In order to prevent the generation of the reverse wave and improve the characteristics, the components are arranged in an overlapping manner, and a flip-chip mounting technology is used to connect the inverted optical semiconductor element 10 and the insulating substrate 30 through Au bumps 50, among which ultrasonic bonding, which is a method that is generally excellent in terms of cost, connection reliability, bonding load, connection pitch accuracy, etc., is particularly used.

[0057] Figure 4 1 is a top view showing the structure of a conventional optical module using a flip-chip mounting technology based on ultrasonic bonding. In the flip-chip mounting based on ultrasonic bonding, the reversed back surface of the optical semiconductor element 10 is usually adsorbed by a chuck, and the optical semiconductor element 10 is mounted on the surface of a submount 20 having a larger projection area than the optical semiconductor element 10. However, for example, wiring from the submount 20 and the insulating substrate 30 to a feedthrough for electrical connection to an external electronic circuit provided in a housing uses conventional wire bonding using Au wires 60 as in the past.

[0058] Therefore, in addition to the electrode pads 20b connected to the optical semiconductor element 10, the electrode pads 20b for wire bonding to other surrounding components need to be formed on the same surface of the submount 20. Since the electrode pads 20b must be formed outside the projection area of ​​the optical semiconductor element 10, the submount 20 needs to have a larger area of ​​the electrode pads 20b for wire bonding to other components than the optical semiconductor element 10. Figure 4 Other components cannot be mounted within the surface of the optical semiconductor element 10 shown.

[0059] Figure 5 FIG. 1 is a top view showing the structure of the basic structural parts of the optical module involved in Embodiment 1 of the present application. Figure 5 and Figure 2 As shown, the optical module 1001 includes, in its basic configuration, an optical semiconductor element 10 having electrode pads 30 b and 30 c formed on both surfaces and electrically connected to each other via a through hole 30 d.

[0060] This structure not only allows the optical semiconductor element 10 to be miniaturized by removing the electrode pads for wire bonding mounting from the optical semiconductor element 10 as in the conventional flip-chip mounting, but also allows the optical semiconductor element 10 to be miniaturized by mounting an insulating substrate 30 that is smaller than the optical semiconductor element 10 on the optical semiconductor element 10. Figure 3 and Figure 4 The optical semiconductor element 10 and the insulating substrate 30 mounted in the XY direction shown are all mounted in the Z direction, thereby mounting the components at a high density. On this basis, since the electrode pads 30c for wire bonding to other surrounding components can be formed on the surface of the insulating substrate 30 mounted on the optical semiconductor element 10, the components can be more densely packed and miniaturized than the conventional flip-chip mounting. In addition, the surface of the insulating substrate 30 having a smaller projection area than the optical semiconductor element 10 can be adsorbed by the chuck and mounted on the surface of the optical semiconductor element 10.

[0061] As described above, according to the optical module 1001 of the first embodiment, the optical semiconductor element 10 having the electrode pads 10b formed on the surface, the insulating substrate 30 having the electrode pads 30c and 30b formed on the surface and the back surface, and the Au bumps 50 for bonding the electrode pads 30b on the back surface of the insulating substrate 30 to the electrode pads 10b of the semiconductor element 10 are provided. The back surface of the insulating substrate 30 is arranged opposite to the front surface of the semiconductor element 10, and the electrode pads 30b on the back surface of the insulating substrate 30 are connected to the electrode pads 30c on the front surface of the insulating substrate 30 via the through holes 30d. Therefore, the electrode pads for wire bonding mounting can be removed from the optical semiconductor element to reduce the size of the optical semiconductor element. Furthermore, the optical semiconductor element and the insulating substrate are electrically and mechanically bonded by Au bumps instead of by conventional wire bonding using Au wires, thereby improving the frequency characteristics compared with the case of bonding by wire bonding. Furthermore, by mounting the insulating substrate in the thickness direction of the optical semiconductor element, the area required for mounting the optical semiconductor element, the submount, and the insulating substrate can be reduced, thereby achieving a high-density optical module. Therefore, a higher-speed and larger-capacity optical module can be obtained than before.

[0062] Implementation Method 2

[0063] In the first embodiment, the Au bumps 50 are uniformly arranged in the surface of the insulating substrate 30 , but in the second embodiment, a case where the Au bumps 50 are arranged at both ends of the insulating substrate 30 will be described.

[0064] Figure 6 FIG. 1 is a top view showing the structure of the optical module 1001 according to Embodiment 2 of the present application. Figure 6 As shown, in the optical module 1001 according to the second embodiment, the Au bumps 50 are arranged in a concentrated manner along the sides at both ends of the insulating substrate 30 .

[0065] The basic structure of the optical module 1001 of the second embodiment is the same as that of the optical module 1001 of the first embodiment. Figure 6 The configuration of the Au bump 50 shown is different. Therefore, here, the differences are mainly described, and the description of the same structural parts is omitted. Figure 6 Only the optical semiconductor element 10 , the submount 20 , the insulating substrate 30 , and the Au bumps 50 in the optical module 1001 according to the second embodiment are shown, and description of other components is omitted.

[0066] In the optical module 1001 of Embodiment 1 and Embodiment 2, thermal stress is generated due to heating when the submount 20 is joined to the solder 70, preheating during flip-chip mounting, and heat generated by driving the optical semiconductor element 10. In addition, thermal stress is sometimes generated due to the difference in linear expansion coefficient between the submount 20 and the surrounding components caused by cooling. In order to reduce the thermal stress generated at the joint of the Au bump 50, a method such as uniformly arranging the Au bump 50 within the surface of the insulating substrate 30 as shown in the present embodiment 1 in which the number of the Au bump 50 is increased can be considered.

[0067] In the case where a plurality of laser generating units are formed in the optical semiconductor element 10 in order to increase the capacity of the optical module 1001, Figure 1 As shown in FIG. 1 , a plurality of laser beams output from the optical semiconductor element 10 are focused by the lens 120 and combined by the combiner 130. Therefore, in order to stably output the combined light, it is preferable to position the electrode pads 10b formed on the optical semiconductor element 10 as shown in FIG. Figure 6 As shown, they are arranged in one row relative to the laser generating section.

[0068] Figure 7 1 is a top view showing another arrangement of bumps of the optical module. In the case where a plurality of laser generating units are formed on one optical semiconductor element 10 in order to increase the capacity of the optical module 1001, if it is desired to evenly arrange dummy electrodes for mechanically fixing the insulating substrate 30 and the optical semiconductor element 10 on the surface of the insulating substrate 30 after stably outputting the combined light, the electrodes on the surface of the insulating substrate 30 are arranged as follows. Figure 7 As shown in FIG. 5( a ), for example, the Au bumps 50 are arranged in one row at one end of one side of the insulating substrate 30 , and the other Au bumps 50 are evenly arranged in the surface of the insulating substrate 30 .

[0069] In such an arrangement of the Au bumps 50 , when thermal stress is generated at the joints of the Au bumps 50 , the thermal stress generated at the joints of the Au bumps 50 arranged within the surface of the insulating substrate 30 may deviate, and the joints of the Au bumps 50 with the highest thermal stress may be easily peeled off.

[0070] As a countermeasure, the number of Au bumps 50 may be increased, but the load required for flip-chip mounting increases in accordance with the increased number of Au bumps 50. Therefore, in the structure of the second embodiment, since vibration occurs between the electrode pads 30c on the surface of the insulating substrate 30 and the surface of the adsorption chuck, the electrode pads 30c may be deformed due to the increased load, and may come into contact with adjacent electrode pads 30c, causing a circuit short circuit and other problems. In addition, since dummy electrode pads 10b are required on the optical semiconductor element 10 in accordance with the increased number of Au bumps 50, the optical semiconductor element 10 is enlarged.

[0071] Therefore, in the present embodiment 2, as Figure 6 As shown, as a method for ensuring the reliability required for the product by uniformly dispersing the stress generated at the joint of the Au bump 50 while stably outputting combined light to multiple laser generating units on the optical semiconductor element 10 and miniaturizing the optical semiconductor element 10 without increasing the number of dummy pads, the Au bumps 50 are concentratedly arranged on the edges of the two ends of the insulating substrate 30.

[0072] Therefore, Figure 7 The case where the Au bumps 50 are uniformly arranged in the substrate as shown in (a), and Figure 7 Compared with the case where the Au bumps 50 are arranged along the periphery of the substrate as shown in (b), it is possible to suppress the increase in thermal stress generated at the bonding portion of the specific Au bumps 50 during cooling after flip-chip mounting. Figure 8 These are the results of stress analysis of the arrangement of bumps in the optical module according to the second embodiment and the arrangement of other bumps.

[0073] Regarding the number and arrangement of the Au bumps 50, when the electrode pads 10b are formed in one row in the case where a plurality of laser generating units are formed on the optical semiconductor element 10 as in the second embodiment, there is no problem even if the Au bumps 50 are arranged at other positions on the insulating substrate 30 as long as the Au bumps 50 are arranged in a manner opposed to each other at both ends of the insulating substrate 30. However, if the number of the Au bumps 50 increases, as described above, there is a possibility that a short circuit between the electrode pads 30c formed on the insulating substrate 30 during flip-chip mounting and the optical semiconductor element 10 may be enlarged. For this reason, it is preferable that the Au bumps 50 are arranged as dummy electrodes on the opposite sides in the same number as the number of electrode pads 10b arranged in one row according to the number of laser generating units formed on the optical semiconductor element 10.

[0074] Moreover, if Figure 1 As shown, the insulating substrate 30 mounted on the optical semiconductor element 10 is connected to the IC 110 or the like through the Au wire 60 from the electrode pad 30c formed on the surface thereof. At this time, in order to shorten the Au wire 60, the electrode pad 30c for bonding the Au wire 60 is preferably formed at the end of the insulating substrate 30. In addition, since the Au wire 60 is wire-bonded after the insulating substrate 30 is mounted on the optical semiconductor element 10, stress is generated at the joint portion of the Au bump 50 due to the pressure applied by the tool during the wire bonding. For this reason, by concentrating the Au bumps 50 on the sides at both ends of the insulating substrate 30 as in the second embodiment, it is possible to suppress the stress generated at the joint portion of a specific Au bump 50 when wire bonding is performed on the electrode pad 30c of the insulating substrate 30, thereby preventing the joint portion from peeling off.

[0075] As described above, according to the optical module 1001 involved in the second embodiment, since it includes the optical semiconductor element 10 having the electrode pad 10 b formed on the surface, the insulating substrate 30 having the electrode pads 30 c and 30 b formed on the surface and the back surface, and the Au bump 50 for bonding the electrode pad 30 b on the back surface of the insulating substrate 30 to the electrode pad 10 b of the semiconductor element 10, the back surface of the insulating substrate 30 is arranged to face the surface of the semiconductor element 10, and the electrode pad 30 b on the back surface of the insulating substrate 30 is bonded to the surface of the insulating substrate 30 via the through hole 30 d. The Au bump 50 is connected to the electrode pad 30c of the insulating substrate 30, and the Au bump 50 is arranged near one end of the insulating substrate 30 and near the other end opposite to the above-mentioned end. Therefore, compared with the case where the Au bump is evenly arranged in the surface of the insulating substrate and the case where the Au bump is arranged along the periphery of the board, the thermal stress generated during the cooling after the flip-chip installation and the stress generated during the wire bonding to the electrode pad of the insulating substrate after the flip-chip installation can be suppressed from increasing at the joint of the specific Au bump and causing the joint to peel off, thereby improving the yield and reliability of the optical module. In addition, since the Au bump can also be not arranged in the central part of the insulating substrate, the number of Au bumps required to ensure the reliability of the product is correspondingly reduced, so the load required for flip-chip installation can be reduced. As a result, the electrode pad on the surface of the insulating substrate can be suppressed from being deformed due to the friction between the end of the adsorption chuck caused by ultrasonic vibration, thereby contacting the adjacent electrode pad and causing the circuit to short-circuit. In addition, by reducing the number of required Au bumps, the number of dummy electrode pads used only for mechanically fixing the insulating substrate formed on the optical semiconductor element is also reduced, so that the optical semiconductor element can be miniaturized accordingly. Therefore, a more cost-effective and highly reliable optical module with improved yield can be obtained.

[0076] Implementation 3

[0077] In the third embodiment, a method for manufacturing the optical semiconductor element 10 , the submount 20 , and the insulating substrate 30 of the optical module 1001 according to the first embodiment will be described.

[0078] Fig. 9 2 is a cross-sectional view showing a method for manufacturing an optical module according to Embodiment 3. Fig. 9Only the manufacturing method of the optical semiconductor element 10, the submount 20 and the insulating substrate 30 in the optical module 1001 of embodiment 3 is shown, and other assembly processes of the optical module 1001 other than those shown in the figure, such as the process of fixing the thermal module 40 to the housing 100, the process of mounting the assembled optical semiconductor element 10, the submount 20 and the insulating substrate 30 on the thermal module 40 fixed to the housing 100, the process of wire bonding from the electrode pad 30c of the insulating substrate 30 mounted on the thermal module 40 to the IC 110, and the process of installing the lens 120 and the combiner 130 between the laser generating part formed in the optical semiconductor element 10 and the emitting part of the housing 100, are omitted from the illustration because they are the same as those of the existing optical modules.

[0079] First, if Fig. 9 As shown in (a), the submount 20 is placed on a hot plate 200 heated to a temperature above 280°C, which is the melting point of the AuSn solder 70, so that the AuSn solder 70 pre-coated on the electrode pad 20b of the submount 20 is melted, thereby soldering the submount 20 to the optical semiconductor element 10.

[0080] At this time, the optical semiconductor element 10 can be placed on the submount 20 after the melting of the AuSn solder 70 is confirmed, or before the melting of the AuSn solder 70 is confirmed. However, in order to miniaturize the submount 20, the size of the pre-coated AuSn solder 70 is preferably set to the same level as the optical semiconductor element 10. Therefore, if the size of the pre-coated AuSn solder 70 is not larger than the optical semiconductor element 10, it is preferred to place the optical semiconductor element 10 after the melting of the AuSn solder 70 is confirmed. In addition, in the third embodiment, the heating temperature of the hot plate 200 is set to 340°C.

[0081] Next, if Fig. 9 As shown in (b), the submount 20 to which the optical semiconductor element 10 is die-bonded is placed on the workbench 300 of the ultrasonic mounter. At this time, in order to improve the bonding property of the Au bump 50, the workbench 300 of the ultrasonic mounter is preheated at a temperature lower than the melting point of the AuSn solder 70, that is, 200°C. In addition, the submount 20 placed on the workbench 300 is evacuated and adsorbed on the workbench 300, and the side surfaces of the submount 20 on both sides of the direction in which the ultrasonic vibration is applied are mechanically clamped and fixed using clamps 300a and 300b to prevent the submount 20 from moving in the vibration direction of the ultrasonic wave.

[0082] Further, if Fig. 9As shown in (c), Au bumps 50 are formed in advance on the electrode pads 30b of the insulating substrate 30 at positions corresponding to the electrode pads 10b on the optical semiconductor element 10, and the surface of the insulating substrate 30 on which the electrode pads 30c are formed is adsorbed by the adsorption chuck 400 of the ultrasonic mounting machine, and the insulating substrate 30 is conveyed to a predetermined position on the optical semiconductor element 10 preheated to 200°C. The insulating substrate 30 is placed on the optical semiconductor element 10 at a position where the electrode pads 30b on the insulating substrate 30 and the electrode pads 10b of the optical semiconductor element 10 corresponding to the electrode pads 30b are opposed to each other. In the third embodiment, the Au bumps 50 are formed on the electrode pads 30b, but the position where the Au bumps 50 are formed in advance may be the electrode pads 10b of the optical semiconductor element 10.

[0083] Afterwards, if Fig. 9 As shown in (d), the insulating substrate 30 adsorbed by the adsorption chuck 400 is pressurized while being placed on the optical semiconductor element 10. At this time, it is a common process to impart ultrasonic vibration immediately after pressurization to bond the optical semiconductor element 10 to the Au bump 50. In contrast, in the third embodiment, the adsorption chuck 400 is preheated in advance, or the insulating substrate 30 is continuously pressurized toward the optical semiconductor element 10 via the Au bump 50, and the Au bump 50 is also heated to 200°C, which is the same as the optical semiconductor element 10.

[0084] Finally, if Fig. 9 As shown in (e), while the Au bump 50 is heated to about 200° C. in the same manner as the optical semiconductor element 10, an ultrasonic mounting machine is used to impart ultrasonic vibration to the direction (C direction) of the sub-mount 20 mechanically fixed using the clamps 300a and 300b, thereby ultrasonically bonding the optical semiconductor element 10 to the Au bump 50.

[0085] In this way, by heating the Au bump 50 to the same temperature as the optical semiconductor element 10 and performing ultrasonic bonding, good bonding can be obtained even with a lower load, lower amplitude, and shorter time than bonding at room temperature, so that the optical semiconductor element 10 can be prevented from being damaged by the ultrasonic waves applied during bonding. In addition, the thermal stress generated at the bonding portion of the Au bump 50 when the assembled optical semiconductor element 10, the submount 20, and the insulating substrate 30 are removed from the workbench 300 of the ultrasonic mounting machine for cooling can be reduced compared to the case where the Au bump 50 is not heated but bonded at room temperature, so that the bonding portion of the Au bump 50 can be prevented from peeling off due to heating and cooling applied after flip-chip mounting, thereby preventing the optical module 1001 from being damaged. In addition, by performing chip bonding between the optical semiconductor element 10 and the submount 20 in the pre-flip-chip mounting process, it is not necessary to directly mechanically fix the optical semiconductor element 10 during flip-chip mounting, so that the element can be prevented from being damaged by contact with a fixing jig or the like during flip-chip mounting.

[0086] In the third embodiment, the optical semiconductor element 10 is placed on the workbench of the ultrasonic mounting machine after die bonding with the submount 20, and the insulating substrate 30 is flip-chip mounted while the submount 20 is fixed. However, the order of assembling the optical semiconductor element 10, the submount 20, and the insulating substrate 30 is not limited to this. For example, the optical semiconductor element 10 may be placed on the workbench of the ultrasonic mounting machine to directly fix the optical semiconductor element 10, and the insulating substrate 30 may be flip-chip mounted, and then the optical semiconductor element 10 with the insulating substrate 30 flip-chip mounted may be die-bonded with the submount 20. However, when a clamp or the like is used to mechanically fix the side surface of the optical semiconductor element 10, in order to prevent the laser generating portion of the optical semiconductor element 10 from being damaged by the ultrasonic vibration applied during flip-chip mounting, it is necessary to set the direction of the ultrasonic vibration and the fixing by the clamp so that the clamp does not contact the laser generating portion of the optical semiconductor element 10. For example, in a case where the laser generating portion is formed on the side surface of the short side of the optical semiconductor element 10, it is necessary to perform flip-chip mounting by vibrating the insulating substrate 30 relative to the long side of the optical semiconductor element 10 fixed by the clamp while the two side surfaces of the long side of the optical semiconductor element 10 are fixed by the clamp.

[0087] When the insulating substrate 30 is flip-chip mounted before the optical semiconductor element 10 is die-bonded with the submount 20, the bonding portion of the Au bump 50 is subjected to thermal stress caused by heating and cooling during die bonding with the submount 20. However, when the insulating substrate 30 is flip-chip mounted before the optical semiconductor element 10 is die-bonded with the submount 20, the influence of the optical semiconductor element 10 being tilted due to the difference in thickness of the AuSn solder 70 pre-coated on the submount 20 and being bent due to thermal stress during die bonding can be eliminated. Thus, it is possible to suppress the situation in which the insulating substrate 30 is rotated during flip-chip mounting due to the application of ultrasonic waves in a state in which only specific Au bumps 50 are in contact with the optical semiconductor element 10, and the specific Au bumps 50 are excessively flattened after flip-chip mounting, thereby damaging the optical semiconductor element 10.

[0088] As described above, according to the manufacturing method of the optical module 1001 involved in the present embodiment 3, since it includes the steps of providing the Au bump 50 on the surface of the electrode pad 10b formed on the surface of the optical semiconductor element 10 or the surface of the electrode pad 30b formed on the back surface of the insulating substrate 30, and placing the insulating substrate 30 on the optical semiconductor element 10 at a position where the electrode pad 10b of the optical semiconductor element 10 and the electrode pad 30b of the insulating substrate 30 are opposite to each other, the step of heating the Au bump 50 while the insulating substrate 30 is placed on the optical semiconductor element 10, and the step of ultrasonically bonding while pressurizing the electrode pad 30b of the insulating substrate 30 or the electrode pad 10b of the optical semiconductor element 10 and the Au bump 50, it is possible to obtain a good bonding state under a low load, low amplitude, and short time compared with bonding at room temperature, and it is possible to suppress the optical semiconductor element from being damaged by the load and amplitude applied during ultrasonic bonding. Furthermore, the stress generated at the joint of the Au bump when the assembled optical semiconductor element, submount, and insulating substrate are removed from the workbench of the ultrasonic mounting machine for cooling can be reduced compared to the case where the optical semiconductor element and the Au bump are joined in a state where there is a temperature difference, thereby preventing the Au bump joint from peeling off due to heating and cooling after flip-chip mounting, thereby preventing the optical module from being damaged. Therefore, a highly reliable optical module with a further improved yield can be obtained.

[0089] Implementation 4

[0090] In the fourth embodiment, a method for manufacturing the optical semiconductor element 10 , the submount 20 , and the insulating substrate 30 of the optical module 1001 according to the second embodiment will be described.

[0091] Fig.101 is a top view showing a method for manufacturing an optical module according to Embodiment 4. The basic manufacturing process of the optical module 1001 of Embodiment 4 is the same as the manufacturing method of the optical module 1001 of Embodiment 3, except that Fig.10 The flip-chip mounting process of the insulating substrate 30 shown in the figure is different. Therefore, here, the differences are mainly described, and the description of the same manufacturing process is omitted. Fig.10 Only a method of flip-chip mounting the insulating substrate 30 and the optical semiconductor element 10 die-bonded to the sub-mount 20 of the optical module 1001 by an ultrasonic mounter is shown, and other assembly steps are omitted from illustration and description.

[0092] In the third embodiment, since the Au bumps 50 are uniformly arranged in the surface of the insulating substrate 30, there is no problem in which direction the ultrasonic vibration is applied when the Au bumps 50 are flip-chip mounted. In contrast, in the fourth embodiment, since the Au bumps 50 are arranged in a row on the sides at both ends of the insulating substrate 30, ultrasonic vibration is applied in a direction perpendicular to the row of the Au bumps 50, which is different from the third embodiment.

[0093] The optical module 1001 of the fourth embodiment has Au bumps 50 arranged in a row on the sides of the insulating substrate 30 at both ends. Therefore, it is conceivable that when ultrasonic waves are applied in the same direction as the row of Au bumps 50, the Au bumps 50 arranged at both ends of the row are first bonded, so that the vibration caused by the ultrasonic waves is suppressed, and the bondability of the Au bumps 50 arranged inside the row is reduced. Therefore, when stress is generated in the bonding portion of the Au bumps 50, the optical module 1001 may be damaged due to the peeling of the bonding portion of the Au bumps 50 arranged in the center of the row where the bondability is lower than that of the two ends of the row.

[0094] Therefore, in the present embodiment 4, Fig.10 As shown, as a method of ensuring the reliability required for the product in a state where the optical semiconductor element 10 is miniaturized by uniformly improving the bonding properties of the Au bumps 50 arranged in a row on the sides of the two ends of the insulating substrate 30, ultrasonic waves are applied in a direction (D direction) perpendicular to the row of the arranged Au bumps 50. In this way, since the arranged Au bumps 50 are all located at the two ends relative to the vibration direction of the ultrasonic wave, it is possible to suppress the bonding properties of other Au bumps 50 from being reduced due to the first bonding of a specific Au bump 50, and compared with the case where ultrasonic waves are applied in the same direction as the row of the Au bumps 50, it is possible to suppress the separation of the bonding portion of the Au bump 50 and the damage to the optical module 1001, thereby improving the reliability of the product.

[0095] In the third embodiment, the order of assembling the optical semiconductor element 10, the submount 20, and the insulating substrate 30 may be such that, after flip-chip mounting the insulating substrate 30 on the optical semiconductor element 10, the optical semiconductor element 10 on which the insulating substrate 30 is flip-chip mounted is die-bonded to the submount 20. However, in the fourth embodiment, the order of assembling the optical semiconductor element 10, the submount 20, and the insulating substrate 30 is preferably such that, after die-bonding the optical semiconductor element 10 to the submount 20, the optical semiconductor element 10 is placed on a workbench of an ultrasonic mounting machine, and the insulating substrate 30 is flip-chip mounted with the submount 20 fixed.

[0096] This is because, for example, when a clamp or the like is used to mechanically fix the side surface of the optical semiconductor element 10, it is necessary to mechanically clamp the side surfaces on both sides of the direction in which the ultrasonic vibration is applied to prevent the optical semiconductor element 10 from moving in the ultrasonic vibration direction. Moreover, in the direction in which the optical semiconductor element 10 is mechanically fixed, in the present embodiment 4, ultrasonic vibration is applied in a direction perpendicular to the row in which the Au bumps 50 are arranged, and the optical semiconductor element 10 and the Au bumps 50 are ultrasonically bonded. At this time, as shown in the embodiment 2, the optical semiconductor element 10 having a plurality of laser generating parts formed therein is preferably arranged in a row with respect to the electrode pads 10b formed on the optical semiconductor element 10 of the laser generating parts, and one side of the row of the Au bumps 50 arranged on the insulating substrate 30 is arranged at a place that can be bonded with the electrode pads 10b. Therefore, the plurality of laser generating parts are preferably formed on the side surface in a direction perpendicular to the row in which the electrode pads 10b of the optical semiconductor element 10, i.e., the Au bumps 50 are arranged.

[0097] Therefore, when the insulating substrate 30 is flip-chip mounted before the optical semiconductor element 10 and the sub-mount 20 are chip-bonded, the optical module manufacturing method involved in the present embodiment 4 must clamp the side of the optical semiconductor element 10 on which the laser generating portion is formed to fix it by a clamp or the like during the flip-chip mounting, and there is a possibility that the laser generating portion of the optical semiconductor element 10 is damaged due to the ultrasonic vibration applied during the flip-chip mounting.

[0098] Based on the above reasons, in the present embodiment 4, it is preferred to place the optical semiconductor element 10 on the workbench of the ultrasonic mounting machine after chip bonding with the sub-mount 20, and in a state where the side surface of the sub-mount 20 in the direction of the laser generating portion of the optical semiconductor element 10 is mechanically fixed by a clamp, ultrasonic vibration is applied to the direction of the mechanically fixed mount 20, and the optical semiconductor element 10 is ultrasonically bonded to the Au bump 50 to perform flip-chip mounting of the insulating substrate 30.

[0099] As described above, according to the manufacturing method of the optical module 1001 involved in the present fourth embodiment, the Au bumps 50 are provided on the surface of the electrode pads 10 b formed on the surface of the optical semiconductor element 10 or on the surface of the electrode pads 30 b formed on the back surface of the insulating substrate 30, and the insulating substrate 30 is placed on the optical semiconductor element 10 at a position where the electrode pads 10 b of the optical semiconductor element 10 and the electrode pads 30 b of the insulating substrate 30 are opposed to each other, the step of heating the Au bumps 50 while the insulating substrate 30 is placed on the optical semiconductor element 10, and the step of heating the Au bumps 50 while heating the electrode pads 30 b of the insulating substrate 30 or the optical semiconductor element 10. The electrode pad 10b of the insulating substrate 30 and the Au bump 50 are pressed while performing the ultrasonic bonding process, and the Au bump 50 is arranged near one end of the insulating substrate and near the other end opposite to the one end. When the ultrasonic bonding is performed, ultrasonic vibration is applied in a direction perpendicular to one end of the insulating substrate 30, so compared with the bonding at room temperature, the load is low, the amplitude is low, and the time is short, so that it is possible to prevent a specific Au bump from being bonded first and causing the bonding of other Au bumps to decrease, and obtain a good bonding state for all the arranged Au bumps, and it is possible to prevent the optical semiconductor element from being damaged by the load and amplitude applied during the ultrasonic bonding. In addition, since the thermal stress generated at the bonding portion of the Au bump due to the heating and cooling of the optical module described in the third embodiment can be reduced compared to the case where the bonding is performed in a state where there is a temperature difference between the optical semiconductor element and the Au bump, it is possible to obtain an effect of preventing the bonding portion of the Au bump from peeling off after flip-chip mounting and causing damage to the optical module. Furthermore, since the number of Au bumps required to ensure the reliability of the product described in the second embodiment is reduced, the following effect can be obtained, that is, the electrode pads on the surface of the insulating substrate can be prevented from deforming due to friction between the electrode pads and the end of the suction chuck caused by ultrasonic vibration, thereby contacting the adjacent electrode pads and causing a circuit short circuit, and the number of dummy electrode pads of the insulating substrate formed on the optical semiconductor element by only mechanically fixing can be reduced, and the optical semiconductor element can be miniaturized accordingly. Therefore, a more inexpensive and highly reliable optical module with improved yield can be obtained.

[0100] Although the present application records various illustrative embodiments and examples, the various features, methods and functions recorded in one or more embodiments are not limited to the application of specific embodiments, and can be applied to the embodiments alone or in various combinations. Therefore, countless unillustrated variations can be imagined within the technical scope disclosed in the present application specification. For example, it includes the case where at least one constituent element is deformed, added, or omitted, and the case where at least one constituent element is extracted and combined with constituent elements of other embodiments.

[0101] Description of reference numerals:

[0102] 10 ... optical semiconductor element; 10b ... electrode pad; 30 ... insulating substrate; 30b, 30c ... electrode pads; 30d ... through hole; 50 ... Au bump; 1001 ... optical module.

Claims

1. An optical module, characterized in that: The invention comprises: a semiconductor element having an electrode pad formed on the surface; an insulating substrate having electrode pads formed on the surface and the back surface; and a bump for bonding the electrode pad on the back surface of the insulating substrate to the electrode pad of the semiconductor element. The back surface of the insulating substrate is arranged to face the front surface of the semiconductor element, and The electrode pads on the back surface of the insulating substrate are connected to the electrode pads on the front surface of the insulating substrate via the through holes.

2. The optical module according to claim 1, characterized in that: The area of ​​the surface of the insulating substrate on which the electrode pad is formed is smaller than the area of ​​the surface of the semiconductor element on which the electrode pad is formed.

3. The optical module according to claim 1 or 2, characterized in that: The bumps are evenly arranged in the surface of the insulating substrate.

4. The optical module according to claim 1 or 2, characterized in that: The bump is disposed near one end of the insulating substrate and near another end opposite to the one end.

5. The optical module according to claim 4, characterized in that: The bump disposed near the other end is dummy.

6. The optical module according to claim 4 or 5, characterized in that: The semiconductor element includes a laser generating unit. The laser generating section is provided on a side surface of the semiconductor element in a direction perpendicular to one end of the insulating substrate.

7. A method for manufacturing an optical module, characterized in that: Including the following processes: Providing bumps on the surface of an electrode pad formed on the surface of a semiconductor element or on the surface of an electrode pad formed on the back surface of an insulating substrate, and placing the insulating substrate on the semiconductor element at a position where the electrode pad of the semiconductor element and the electrode pad of the insulating substrate face each other; heating the bump while the insulating substrate is placed on the semiconductor element; as well as Ultrasonic bonding is performed while applying pressure to the electrode pads of the insulating substrate or the electrode pads of the semiconductor element and the bumps.

8. The method for manufacturing an optical module according to claim 7, characterized in that: The back surface of the insulating substrate is arranged to face the front surface of the semiconductor element, and The electrode pads on the back surface of the insulating substrate are connected to the electrode pads on the front surface of the insulating substrate via the through holes.

9. The method for manufacturing an optical module according to claim 7 or 8, characterized in that: The area of ​​the surface of the insulating substrate on which the electrode pad is formed is smaller than the area of ​​the surface of the semiconductor element on which the electrode pad is formed.

10. The method for manufacturing an optical module according to any one of claims 7 to 9, characterized in that: The bumps are evenly arranged in the surface of the insulating substrate.

11. The method for manufacturing an optical module according to any one of claims 7 to 9, characterized in that: The bump is disposed near one end of the insulating substrate and near another end opposite to the one end.

12. The method for manufacturing an optical module according to claim 11, characterized in that: The bump disposed near the other end is dummy.

13. The method for manufacturing an optical module according to claim 11 or 12, characterized in that: When performing the ultrasonic bonding, the ultrasonic vibration is applied in a direction perpendicular to one end of the insulating substrate.

14. The method for manufacturing an optical module according to any one of claims 11 to 13, characterized in that: The semiconductor element includes a laser generating unit. The laser generating section is provided on a side surface of the semiconductor element in a direction perpendicular to one end of the insulating substrate.