Multifunctional hard tissue treating agent based on compound with sulfydryl and carboxylic acid group structures and application of multifunctional hard tissue treating agent

Through the multifunctional hard tissue treatment agent of thiol and carboxylic acid group structure compounds, the problem of insufficient permeability and bonding strength of the hard tissue repair materials in the dentin, root canal and bone surface treatment is achieved efficient adhesiveness in dentin, root canal and bone surface treatment The effect of conjugation and antibacterial enhances the effect of caries treatment and fracture fixation.

CN119015131APending Publication Date: 2024-11-26ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411096378.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing dental hard tissue repair materials are insufficient infiltration during the bonding process, and the lack of stable combination between the adhesive and the dentin matrix, resulting in poor caries treatment effect, insufficient sterilization ability of root canal flushing fluid and toxicity, and fracture fixation The problem of low bonding strength.

Method used

Using a multifunctional hard tissue treatment agent based on thiol and carboxylic acid group structure compounds, chemical bonds are formed with the bond monomer through thiol-ethylenically bond clicking reaction, promoting the penetration of resin-based materials and forming a stable bond interface, with antibacterial and enzyme inhibition Performance, suitable for dentin, root canal, and bone surface treatment, improving the effects of caries prevention, root canal treatment and fracture fixation.

Benefits of technology

Improve the permeability and bonding strength of the hard tissue repair material of the tooth, enhance the antibacterial and stability, improve the effect of caries treatment and the success rate of root canal treatment, improve the fracture fixation strength, and reduce the bonding process the effects of saliva and blood contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004988050030000011
    Figure HDA0004988050030000011
  • Figure HDA0004988050030000012
    Figure HDA0004988050030000012
  • Figure HDA0004988050030000013
    Figure HDA0004988050030000013
Patent Text Reader

Abstract

According to the multifunctional hard tissue treating agent based on the compound with the sulfydryl and carboxylic acid group structure and the application, the basic structural unit of the compound with the sulfydryl and carboxylic acid group structure is SHm-R-(COOH) n, the carboxylic acid group and calcium salt in a hard tissue form a stable ionic bond, and the sulfydryl at the other end has enzyme inhibition and antibacterial properties; through a sulfydryl-double bond click reaction, the polymer has the capability of chemically bonding with a bonding monomer. Different from an acidic monomer which takes double bonds as a polymeric group and can only have a polymerization reaction under the initiation of an initiator, the treating agent disclosed by the invention can spontaneously, quickly and efficiently react with a bonding monomer in a physiological environment so as to obtain a resin-based material with permeation driving force, enzyme inhibition and antibacterial surface and solve the problem of poor bonding effect of hard tissues; and adverse effects of saliva and blood pollution during clinical operation can be effectively eliminated. The treatment agent disclosed by the invention can be used for medical applications such as tooth bonding repair, caries prevention, root canal irrigation and bone surface treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of biological adhesive materials, and particularly relates to a multifunctional hard tissue treating agent based on thiol and carboxylic acid group structural compounds and its application. Technical Background

[0002] Dental caries is a chronic bacterial infection disease that affects the hard tissues of the teeth. It has a very high incidence rate and is characterized by progressive development. It is the main disease that causes tooth pain and loss of chewing function. The World Health Organization has listed dental caries, tumors, and cardiovascular diseases as the three major preventable diseases of humans. Due to the particularity of the hard tissues of the teeth, it is almost impossible to repair itself after damage. The repair of tooth defects mainly relies on alternative repairs with artificial materials such as resins. Therefore, the formation of a stable connection between the restorative material and the tooth tissue is the premise and prerequisite for successful repair.

[0003] The early manifestations of caries are white spots or brown spots. If no treatment measures are taken and it is allowed to develop, it will not only affect the appearance, but also caries cavities will soon form. At present, the most commonly used treatment for early enamel caries is infiltration resin, which is minimally invasive. Based on the low fluidity of infiltration resin, it enters the porous structure of demineralized enamel through capillary siphoning, blocks the channels for acidic substances and mineral ions to invade, enhances the acid resistance of the lesion, thereby blocking the progression of early caries and repairing defective tissues. However, this passive siphoning effect determines the inefficiency and limitation of infiltration, affecting the effect of treatment. How to promote the penetration of resin into the pore structure of enamel is the key to improving the treatment effect of early enamel caries.

[0004] If caries progresses further, it will affect the dentin. Dentin bonding forms a mixed layer, which is still the "short board" in the bonding joint. During the service of the composite, the mixed layer is prone to degradation and collapse, leading to restoration failure and a large number of secondary dental diseases. Insufficient penetration of the adhesive during the bonding process and the lack of stable bonding between the adhesive phase and the dentin matrix phase cause structural defects in the mixed layer. These structural defects lead to the disintegration of the mixed layer under chewing stress, endogenous enzyme action, and cariogenic bacteria attack. Therefore, solving the problem of dentin bonding durability requires simultaneously addressing the promotion of adhesive penetration, the formation of stable chemical bonding between the adhesive phase and the dentin matrix phase, and antibacterial and enzyme inhibition.

[0005] If caries progresses further, it will affect the dental pulp. Currently, the most commonly used treatment for pulpitis is root canal therapy. The sterilization of the root canal and the sealing of the root canal by filling materials are the keys to its success. The current root canal irrigants have relatively simple performances. Most of the irrigants only have irrigating and lubricating effects, and the bacterial microorganisms attached to the complex root canal system cannot be removed through root canal preparation, resulting in poor control of root canal system infection. Root canal irrigants with good bactericidal ability, tissue dissolving ability (dissolving the pulp), and the ability to remove bacterial biofilms have the disadvantages of high toxicity, corrosiveness, easy allergies, lack of sustained antibacterial and smear layer removal capabilities. Therefore, the development of antibacterial root canal irrigants with strong tissue dissolving ability, active binding properties to the root canal wall, and good biocompatibility is of great significance for improving the success rate of root canal treatment.

[0006] In fracture fixation and bone implant fixation, bone bonding with high bonding strength and without affecting bone healing is still a difficult problem. Improving bone bonding strength by treating the bone surface is of great significance to solving this problem. Summary of the invention

[0007] The purpose of the present invention is to provide a multifunctional hard tissue treatment agent based on a thiol and carboxyl group structure compound, which is a solution with thiol and carboxyl structure compounds as essential components. The basic structural unit of the thiol and carboxyl group structure compound is SH m -R-(COOH) n ; Wherein SH is a thiol group, m represents the number of thiol groups, COOH is a carboxylic acid group, and n represents the number of carboxylic acid groups; the compound includes its salt. The compound having a thiol group and a carboxylic acid structure is specifically cysteine, glutathione, acetylcysteine, cysteine ​​methyl ester, cysteine ​​acetic acid, carboxymethylcysteine, 2-mercapto-L-histidine; mercaptoacetic acid, mercaptopropionic acid, mercaptobutyric acid, mercaptovaleric acid, mercaptohexanoic acid, mercaptooctanoic acid, mercaptoundecyl acid, mercaptododecyl acid, mercaptotetradecyl acid, mercaptohexadecyl acid, 2,3-dimercaptosuccinic acid, S-(2,3,4-trihydroxybutyl) mercapto acid, S-(4-fluorophenyl) mercapto acid, 4-mercaptobenzoic acid, mercapto-polyethylene glycol-carboxyl, mercapto-polyethylene glycol-propionic acid, or a mixture of two or more thereof.

[0008] The hard tissue bonding agent is an aqueous solution, an ethanol aqueous solution or an acetone aqueous solution.

[0008] The concentration of the mercapto group, carboxylic acid group structure compound and its salt in the hard tissue adhesive treatment agent is 0.001-1000 mg / mL.

[0009] Another object of the present invention is to provide the use of the thiol and carboxylic acid group structure compounds in the preparation of a multifunctional hard tissue treatment agent for treating dentin, enamel, root canals, and bone surfaces to improve the effects of bonding repair, caries prevention, root canal treatment, fracture fixation, or bone implant fixation.

[0008] The carboxylic acid group at one end forms a stable ionic bond with hydroxyapatite in the hard tissue, while the thiol group at the other end not only has enzyme inhibition and antibacterial properties, but also has the ability to chemically bond with bonding monomers through thiol-ene bond click reactions. Unlike the current reaction monomers with ene bonds as polymerization groups, which require initiators to initiate polymerization reactions, this compound can react spontaneously, quickly, and efficiently with ene bond bonding monomers in current dentin adhesives under physiological conditions to obtain a bonding surface with adhesive penetration driving force, promote the penetration of resin-based materials, and then form a multifunctional, highly stable bonding interface with integrated structural functions of enzyme inhibition, antibacterial, and hard tissue-adhesive chemical bonding. It can also effectively eliminate the adverse effects of saliva and blood contamination on bonding during clinical operations, and improve the effects of tooth bonding, repair, root canal treatment, fracture fixation, and intraosseous implant fixation.

[0010] The hard tissue treating agent may contain fluoride releasing substances as additives, including sodium fluoride and fluoride nanoparticles.

[0011] The hard tissue treating agent can be used for treating fracture ends or bone surfaces to improve the fixation effect of fractures or intraosseous implants.

[0012] When the hard tissue treating agent is used to treat the tooth surface, the treating agent can be mixed with the existing tooth acid etching agent, or the tooth surface can be treated with the acid etching agent first and then with the treating agent, or the treating agent can be used alone.

[0013] The hard tissue treatment agent is used before the adhesive and must not be premixed with the adhesive.

[0014] When the hard tissue treating agent is used to treat tooth surface or bone surface, it can be applied by coating or soaking, with the coating time ranging from 3s to 60s and the coating times ranging from 1 to 10 times.

[0015] When the hard tissue treating agent is used for root canal treatment, the method of flushing can be adopted, and the flushing time is 3s-60s, and the flushing can be performed multiple times as needed.

[0016] After the tooth surface or root canal is treated with the hard tissue treating agent, it can be rinsed with water or ethanol aqueous solution or pure ethanol, or the resin-based material or root canal filling material can be directly used without rinsing.

[0017] The resin-based material includes resin-based adhesive, resin-based cement, flowing resin or infiltrating resin.

[0018] After the hard tissue treating agent is applied to the bone surface, it can be rinsed with physiological saline, or bone adhesives such as bone cement can be directly used without rinsing.

[0019] The hard tissue treatment agent of the present invention contains an aqueous solution, an ethanol aqueous solution or an acetone aqueous solution of 0.001-1000mg / mL of a thiol group, a carboxylic acid group structural compound or a mixture thereof. The treatment agent is used to treat tooth surface, bone surface, root canal wall or tooth surface after acid etching, and the carboxylic acid group at one end forms a stable ionic bond with hydroxyapatite in the hard tissue, while the thiol group at the other end not only has enzyme inhibition and antibacterial properties, but also has the ability to chemically bond with bonding monomers through thiol-double bond click reaction. Different from the acidic monomers with double bonds as polymerizing groups that need to be initiated by an initiator to undergo polymerization reaction, this structural compound can react spontaneously, quickly and efficiently with bonding monomers under a physiological environment to obtain an enzyme inhibition and antibacterial bonding surface with an adhesive penetration driving force, and can effectively eliminate the adverse effects of saliva and blood contamination on bonding during clinical operation, and improve the fixation effect of tooth bonding repair, root canal treatment, fracture fixation and bone implants.

[0020] The technical problem solved by the present invention is to optimize the structure and function of the hard tissue bonding interface and improve the problem of poor hard tissue bonding effect. The compound of the present invention can actively combine with the components in the hard tissue to promote the penetration of the resin-based material; it has the ability to react with the polymerized monomer to form a stable chemical bond; it also has antibacterial properties, kills residual bacteria and resists bacterial invasion; in addition, it also needs to have the performance of inhibiting the activity of metal matrix proteases that cause collagen degradation. Instruction Manual

[0021] Figure 1 .Scanning electron microscope image of Example 4.

[0022] Figure 2 .Scanning electron microscope images of Examples 5 and 6.

[0023] Figure 3 .Scanning electron microscope images of Examples 7 and 8.

[0024] Figure 4 .Scanning electron microscope images of Examples 9 and 10.

[0025] Figure 5 .Examples 12 and 13 Fourier transform infrared spectroscopy.

[0026] Figure 6 .Photoelectron energy spectra of Examples 12 and 13.

[0027] Figure 7 .Scanning electron microscopy images of cell morphology.

[0028] Figure 8 .CCK-8 assay for cell activity.

[0029] Fig. 9 . Antibacterial activity of the solution against Staphylococcus aureus.

[0030] Fig.10 .Antibacterial activity of the solution against Escherichia coli.

[0031] Fig.11 . Antibacterial activity of the solution against Streptococcus mutans.

[0032] Fig.12 .Antibacterial activity of treated tooth surfaces against Staphylococcus aureus.

[0033] Fig.13 .Antibacterial activity of treated tooth surfaces against Escherichia coli.

[0034] Fig.14 .Antibacterial activity of treated tooth surfaces against Streptococcus mutans.

[0035] Fig.15 .Enzyme inhibition properties for total acid etch bonding.

[0036] Fig.16 .Enzyme inhibition properties for self-etching bonding.

[0037] Fig.17 .Adhesion performance for total acid etching bonding.

[0038] Fig.18 .Adhesion performance when used for self-etching bonding.

[0039] Fig.19 .Adhesive properties for saliva contamination.

[0040] Fig. 20 .Adhesion properties when used for bone bonding.

[0041] Fig.21 . Adhesion properties for blood contamination (contamination occurs after treatment).

[0042] Fig. 22 . Adhesive properties for blood contamination (contamination occurs before treatment). DETAILED DESCRIPTION

[0043] The present invention is described in more detail below with reference to the embodiments and the accompanying drawings, but the present invention is not limited to these embodiments.

[0044] Embodiment 1 A multifunctional hard tissue adhesive treatment agent based on a thiol and carboxyl group structure compound, which is a solution with thiol and carboxyl structure compounds as essential components. The basic structural unit of the thiol and carboxyl group structure compound is SH m -R-(COOH) n; Wherein SH is a thiol group, m represents the number of thiol groups, COOH is a carboxylic acid group, and n represents the number of carboxylic acid groups; the compound includes its salt. The compound having a thiol group and a carboxylic acid structure is specifically cysteine, glutathione, acetylcysteine, cysteine ​​methyl ester, cysteine ​​acetic acid, carboxymethylcysteine, 2-mercapto-L-histidine; mercaptoacetic acid, mercaptopropionic acid, mercaptobutyric acid, mercaptovaleric acid, mercaptohexanoic acid, mercaptooctanoic acid, mercaptoundecyl acid, mercaptododecyl acid, mercaptotetradecyl acid, mercaptohexadecyl acid, 2,3-dimercaptosuccinic acid, S-(2,3,4-trihydroxybutyl) mercapto acid, S-(4-fluorophenyl) mercapto acid, 4-mercaptobenzoic acid, mercapto-polyethylene glycol-carboxyl, mercapto-polyethylene glycol-propionic acid, or a mixture of two or more thereof.

[0045] Embodiment 2 A 100 mg / mL 3-mercaptopropionic acid (CAS No.: 107-96-0) aqueous solution was prepared as a treating agent.

[0046] Embodiment 3 Dentin slices were prepared using a slow cutter and rinsed with deionized water.

[0047] Embodiment 4 The treatment agent of Example 2 was applied to the dentin surface of Example 2 for 20 seconds and then blown dry.

[0048] Embodiment 5 The dentin surface of Example 3 was treated with 37% phosphoric acid solution for 15 seconds and then rinsed with a large amount of deionized water.

[0049] Embodiment 6 The treatment agent of Example 2 was applied to the dentin surface obtained in Example 4 for 20 seconds and then rinsed with a large amount of deionized water.

[0050] Embodiment 7 Treat the enamel surface with 37% phosphoric acid solution for 30 seconds and rinse with plenty of deionized water.

[0051] Embodiment 8 The treatment agent of Example 2 was applied to the enamel surface obtained in Example 7 for 20 seconds, and then rinsed with a large amount of deionized water.

[0052] Embodiment 9 Treat the enamel surface with 37% phosphoric acid solution for 15 seconds and rinse with plenty of deionized water.

[0053] Embodiment 10 The treatment agent of Example 2 was applied to the surface of the tooth enamel obtained in Example 9 for 20 seconds and then blown dry.

[0054] Embodiment 11 The samples obtained in Examples 3-10 were dehydrated with gradient ethanol and observed under a field emission scanning electron microscope. It can be seen that the treatment agent in Example 2 can dissolve the stain layer and expose the dentin organic matrix network (Example 4, Figure 1 ); Compared with the dentin surface treated with 37% phosphoric acid (Example 5), the further treatment with the treatment agent of Example 2 (Example 6) showed no obvious morphological changes ( Figure 2 ); Compared with the enamel surface treated with 37% for 30s (Example 7), the further treatment with the treatment agent of Example 2 (Example 8) showed no obvious morphological changes ( Figure 3 ); Compared with the enamel surface treated with 37% phosphoric acid for 15s (Example 9), the further treatment with the treatment agent of Example 2 (Example 10) makes the enamel pillars more fully exposed ( Figure 4 ).

[0055] Embodiment 12 The hydroxyapatite sheets were rinsed with deionized water and freeze-dried.

[0056] Embodiment 13 The treating agent obtained in Example 2 was coated on the surface of hydroxyapatite for 20 seconds, rinsed with a large amount of deionized water, and freeze-dried.

[0057] Embodiment 14 The hydroxyapatite sheets obtained in Examples 12 and 13 were used for Fourier transform infrared spectroscopy detection. -1 The peak is attributed to the PO stretching band of the phosphate group. After modification, the phosphate group reacts with hydrogen ions and the peak blue-shifts to 880 cm -1 . At 1560cm -1 The new peak at is COO - The stretching vibration of COOH and Ca 2+ On the surface of hydroxyapatite, ionic bonds are formed ( Figure 5 ).

[0058] Embodiment 15 The hydroxyapatite sheets obtained in Examples 12 and 13 were used for photoelectron spectroscopy analysis. The peaks at the positions with binding energies of 163 eV and 226 eV corresponded to the peaks of S(2p) and S(2s), indicating that the thiol groups were adsorbed on the hydroxyapatite ( Figure 6 ).

[0059] Embodiment 16 L929 cells were cultured on the surface of the dentin slices obtained in Examples 3 and 4 for 24 hours, fixed, dehydrated, and the cell morphology was observed under a scanning electron microscope. It was found that the cells spread into a spindle shape, and there was no significant difference in morphology from the control ( Figure 7 ).

[0060] Embodiment 17 After L929 cells were cultured on the surface of the dentin slices obtained in Examples 3 and 4 for 24 hours, the cell activity was detected using a CCK8 kit. There was no significant difference in cell activity compared with the control ( Figure 8 ).

[0061] Embodiment 18 Different concentrations of 3-mercaptopropionic acid aqueous solutions were prepared to test their antibacterial activity against Staphylococcus aureus. When the concentration was 1.25%, it showed obvious antibacterial activity, and the antibacterial rate was close to 100% ( Fig. 9 ).

[0062] Embodiment 19 Different concentrations of 3-mercaptopropionic acid aqueous solutions were prepared to test their antibacterial activity against Escherichia coli. When the concentration was 1.25%, it showed obvious antibacterial activity, and the antibacterial rate was close to 100% ( Fig.10 ).

[0063] Embodiment 20 Different concentrations of 3-mercaptopropionic acid aqueous solutions were prepared to test their antibacterial activity against Streptococcus mutans. When the concentration was 5%, it showed obvious antibacterial activity, and the antibacterial rate was close to 100% ( Fig.11 ).

[0064] Embodiment 21 Staphylococcus aureus was cultured on the surface of the dentin slices obtained in Examples 3 and 4. After 24 hours of culture, the dead and live bacteria detection kit was used for staining. Laser confocal microscopy was used for observation and it was found that the number of dead bacteria increased significantly ( Fig.12 ).

[0065] Embodiment 22 Escherichia coli was cultured on the surface of the dentin slices obtained in Examples 3 and 4. After 24 hours of culture, the dead and live bacteria detection kit was used for staining. Laser confocal microscopy was used for observation and it was found that the number of dead bacteria increased significantly ( Fig.13 ).

[0066] Embodiment 23 Mutans Streptococcus was cultured on the surface of the dentin slices obtained in Examples 3 and 4. After 24 hours of culture, the dead and live bacteria detection kit was used for staining. Laser confocal microscopy was used to observe and found that a large number of dead bacteria ( Fig.14 ).

[0067] Embodiment 24 The dentin surface obtained in Examples 5 and 6 was coated with the total acid etching adhesive Spectrum bond, applied for 20 seconds, blown gently for 15 seconds, and illuminated with a light curing lamp for 20 seconds, and the resin was layered to a resin layer of 1 mm thickness. After 24 hours in a 37°C water bath, a dentin-resin sheet with a thickness of 100 μm was prepared using a slow cutter. The enzyme activity in the demineralized dentin matrix was determined using the EnzChek gelatin activity kit (E-12055, Molecular Probes, Eugene, OR, USA). The diluted gelatin matrix was dropped onto the dentin slice, covered with a coverslip, and incubated at 37°C in a humid environment with a relative humidity of 100% under light-proof conditions. The demineralized layer was scanned layer by layer by CLSM, with an emission light of 530 nm and an excitation light of 488 nm, and the fluorescence intensity of the mixed layer was observed. Unlike the strong fluorescence of the mixed layer in Example 5, the mixed layer in Example 6 had almost no fluorescence ( Fig.15 ).

[0068] Embodiment 25 The dentin surface obtained in Examples 3 and 4 was coated with the self-etching adhesive Single bond universal, applied for 20 seconds, gently blown for 15 seconds, and illuminated with a light-curing lamp for 20 seconds, and the resin was layered to a thickness of 1 mm. A slow cutter was used to prepare a dentin-resin sheet with a thickness of 100 μm. The enzyme activity in the demineralized dentin matrix was determined using the EnzChek gelatin activity kit (E-12055, Molecular Probes, Eugene, OR, USA). The diluted gelatin matrix was dropped onto the dentin slice, covered with a coverslip, and incubated at 37°C in a humid environment with a relative humidity of 100% under light-proof conditions. The demineralized layer was scanned layer by layer by CLSM, with an emission light of 530 nm and an excitation light of 488 nm, and the fluorescence intensity of the mixed layer was observed ( Fig.16 ).

[0069] Embodiment 26 The dentin obtained in Examples 5 and 6 and the enamel obtained in Examples 7 and 8 were coated with Spectrum bond for 20 seconds, blown gently for 15 seconds, and illuminated with a light curing lamp for 20 seconds. The resin was layered to a resin layer with a thickness of 3 mm. After 24 hours in a 37°C water bath, a 1mm×1mm tooth strip was prepared with a slow cutting machine. The micro-tensile fracture strength of the sample was tested with a micro-tensile instrument, and the cross-sectional dimensions were recorded. The micro-tensile strength ( Fig.17 ).

[0070] Embodiment 27 The Bond component of Clearfil SEBond was applied to the dentin obtained in Example 4 and the enamel obtained in Example 10, respectively. Apply for 20 seconds, blow gently for 15 seconds, and lightly cure for 20 seconds, and then build up the resin layer in layers to a thickness of 3 mm. After 24 hours in a 37°C water bath, a slow cutter was used to prepare a 1mm×1mm tooth strip with a bonding surface. The micro-tensile tester was used to test the micro-tensile fracture strength, and the cross-sectional dimensions were recorded to calculate the micro-tensile strength. The controls were the dentin obtained in Example 3 and the enamel obtained in Example 9, which were bonded according to the instructions of Clearfil SE Bond. ( Fig.18 ).

[0071] Embodiment 28 The dentin surface obtained in Examples 5 and 6 was soaked in human saliva for 20 seconds, and then dried with a small cotton swab until the surface was slightly moist. The Spectrum bond was applied for 20 seconds, and then blown for 15 seconds. The light-curing light was used for 20 seconds, and the resin was layered to a resin layer with a thickness of 3 mm. After 24 hours in a 37°C water bath, a 1mm×1mm tooth strip was prepared by a slow cutting machine. The micro-tensile fracture strength of the sample was tested by a micro-tensile instrument, and the cross-sectional dimensions were recorded. The micro-tensile strength ( Fig.19 ).

[0072] Embodiment 29 A slow-speed cutter and polisher were used to prepare a smooth surface of porcine cortical bone.

[0010] Embodiment 30 The treatment agent of Example 2 was applied to the surface of the cortical bone of Example 28 for 20 seconds and then blown dry.

[0073] Embodiment 31 The surface of the cortical bone obtained in Examples 29 and 30 was directly filled with a self-curing base resin whose main component was a methacrylate copolymer. After solidification at room temperature for 30 minutes, a bone strip with a bonding surface of 2 mm×2 mm was prepared using a slow cutting machine. The micro-tensile fracture strength of the sample was tested using a micro-tensile tester, and the cross-sectional dimensions were recorded. The micro-tensile strength ( Fig. 20 ).

[0074] Embodiment 32 The treatment agent obtained in Example 2 is used for root canal treatment to flush the root canal during root canal dredging and preparation.

[0075] Embodiment 33 Prepare a 1 mg / mL 3-mercaptopropionic acid aqueous solution treatment agent, apply the treatment agent for 20 seconds after phosphoric acid etching on the tooth surface, and then perform bonding restoration.

[0076] Embodiment 34 Prepare 250mg / mL 3-mercaptopropionic acid aqueous solution treatment agent, apply the treatment agent on the tooth surface for 20s, rinse with plenty of water, and perform bonding restoration.

[0077] Embodiment 35 Prepare 100 mg / mL sodium 3-mercapto-1-propanesulfonate (CAS No. 107-96-0) aqueous solution as the treatment agent. Mix the treatment agent and the acid etchant at a ratio of 1:9 and treat the tooth surface for 15 seconds. Rinse with plenty of water and then perform bonding repair.

[0078] Embodiment 36 Prepare 150mg / mg 4-mercaptobenzoic acid (CAS No.: 1074-36-8) ethanol aqueous solution (50 / 50) as the treatment agent. After the tooth surface is acid-etched, apply the treatment agent for 20s, rinse with a large amount of ethanol aqueous solution, and then repair with bonding.

[0079] Embodiment 37 A 100 mg / mL 6-mercaptohexanoic acid (Cas No.: 17689-17-7) ethanol aqueous solution (60 / 40) was prepared as the treatment agent. After the tooth surface was acid-etched, the treatment agent was applied for 20 seconds and then repaired with bonding.

[0080] Embodiment 38 A 50 mg / mL 11-mercaptoundecanoic acid (Cas No.: 71310-21-9) ethanol aqueous solution (70 / 30) was prepared as a treatment agent. After the tooth surface was acid-etched, the treatment agent was applied for 30 seconds and then repaired with bonding.

[0081] Embodiment 39 A 150 mg / mL 12-mercaptododecylphosphonic acid (Cas No.: 159239-33-5) ethanol aqueous solution (50 / 50) was prepared as the treatment agent. After the tooth surface was acid-etched, the treatment agent was applied for 30 seconds and then repaired with bonding.

[0082] Embodiment 40 A 10 mg / mL succimer (Cas No.: 304-55-2) ethanol aqueous solution (50 / 50) was prepared as the treatment agent. After the tooth surface was acid-etched, the treatment agent was applied for 20 seconds and then repaired with bonding.

[0083] Embodiment 41 A 20 mg / mL mercaptosuccinic acid (Cas No.: 70-49-5) ethanol aqueous solution (50 / 50) was prepared as the treatment agent. After the tooth surface was acid-etched, the treatment agent was applied for 20 seconds and then repaired with bonding.

[0084] Embodiment 42 A 100 mg / mL 6,8-dimercaptooctanoic acid (Ca No.: 462-20-4) ethanol aqueous solution (50 / 50) was prepared as the treatment agent. After the tooth surface was acid-etched, the treatment agent was applied for 20 seconds and then repaired with bonding.

[0085] Embodiment 43 Aspartic acid (Cas number: 56-84-8) was thiol-modified, and a 20 mg / mL product solution in ethanol-water solution (50 / 50) was prepared as a treatment agent. The tooth surface was acid-etched and coated with the treatment agent for 20 seconds, followed by bonding and repair.

[0086] Embodiment 44 The dentin surface obtained in Examples 5 and 6 was contaminated with blood for 20 seconds, and then dried with a small cotton swab until the surface was slightly moist. Apply the total acid etching adhesive Spectrum bond, apply for 20 seconds, blow gently for 15 seconds, and light-curing light for 20 seconds, and layer the resin to a resin layer of 3 mm thickness. After 24 hours in a 37°C water bath, a slow cutter was used to prepare a 1mm×1mm tooth strip with a bonding surface. The sample micro-tensile instrument was used to test the micro-tensile fracture strength, and the cross-sectional dimensions were recorded. The micro-tensile strength ( Fig.21 ).

[0087] Embodiment 45 The dentin surface of Example 3 was contaminated with blood for 20 seconds, and then treated by Example 5 (acid etching) or Example 6 (acid etching + treatment agent treatment), and dried with a small cotton swab until the surface was slightly moist. Apply the total acid etching adhesive Spectrumbond, apply for 20 seconds, blow gently for 15 seconds, lightly cure for 20 seconds, and layer the resin to a 3mm thick resin layer. After 24 hours in a 37°C water bath, a slow cutter was used to prepare a 1mm×1mm tooth strip with a bonding surface. The sample micro-tensile instrument was used to test the micro-tensile fracture strength, and the cross-sectional dimensions were recorded. The micro-tensile strength ( Fig. 22 ).

Claims

1. A multifunctional hard tissue treatment agent based on the structural combination of thiol and carboxyl groups, It is characterized in that The basic structural unit of the thiol and carboxylic acid group structural compound is SH m -R-(COOH) n , wherein SH is a thiol group, m represents the number of thiol groups, COOH is a carboxylic acid group, n represents the number of carboxylic acid groups, and the compound includes its salt, wherein the compound with thiol and carboxylic acid structure is cysteine, glutathione, acetylcysteine, cysteine ​​methyl ester, cysteine ​​acetic acid, carboxymethylcysteine, 2-mercapto-L-histidine; mercaptoacetic acid, mercaptopropionic acid, mercaptobutyric acid, mercaptovaleric acid, mercaptohexanoic acid, mercaptooctanoic acid, mercaptoundecyl acid, mercaptododecyl acid, mercaptotetradecyl acid, mercaptohexadecyl acid, 2,3-dimercaptosuccinic acid, S-(2,3,4-trihydroxybutyl) mercapto acid, S-(4-fluorophenyl) mercapto acid, 4-mercaptobenzoic acid, mercapto-polyethylene glycol-carboxyl or mercapto-polyethylene glycol-propionic acid, or a mixture of two or more thereof.

2. The hard tissue treating agent according to claim 1, It is characterized in that The treating agent is an aqueous solution, an ethanol aqueous solution or an acetone aqueous solution.

3. The hard tissue treating agent according to claim 1, It is characterized in that The concentration of the mercapto group, carboxylic acid group structure compound and its salt in the treating agent is 0.001-1000 mg / mL.

4. The thiol and carboxylic acid group structure compound according to claim 1 is used in the preparation of a multifunctional hard tissue treating agent for treating dentin, enamel, root canal, bone surface, improving bonding repair, caries prevention, root canal treatment, fracture fixation or bone implant fixation effect.

5. The use according to claim 4, It is characterized in that When the hard tissue treating agent is used for treating dentin, enamel and root canal, fluoride releasing substances are added as additives, including sodium fluoride and fluoride nanoparticles.

6. The use according to claim 4, It is characterized in that When the hard tissue treating agent is used to treat dentin and enamel, the treating agent is mixed with the existing acid etching agent, or the acid etching agent is used first and then the treating agent is used, or the treating agent is used alone for treatment.

7. The use according to claim 4, It is characterized in that The hard tissue treatment agent is used before the adhesive and must not be premixed with the adhesive.

8. The use according to claim 4, It is characterized in that When the hard tissue treating agent is used to treat dentin, enamel and bone surface, the method of coating or soaking is adopted, the treating time is 3s-60s, and the treating times are 1-10 times.

9. The use according to claim 4, It is characterized in that When the hard tissue treating agent is used for root canal treatment, the method of rinsing is adopted, and the rinsing time is 3s-60s, or the rinsing is performed multiple times as required.

10. The use according to claim 4, It is characterized in that After the hard tissue treating agent treats the dentin, enamel or root canal, it is rinsed with water or ethanol aqueous solution or pure ethanol, or the resin-based material or root canal filling material is directly used without rinsing.

11. The use according to claim 10, It is characterized in that The resin-based material is selected from resin-based adhesives, resin-based cements, flowing resins or penetrating resins.

12. The use according to claim 4, It is characterized in that After the hard tissue treating agent is applied to the bone surface, it can be rinsed with physiological saline, or bone cement bone adhesive can be used directly without rinsing.