Multifunctional hard tissue treating agent based on sulfydryl and sulfonic acid group structure compound and application
By forming a stable chemical combination with the dentin and bone surface, the problem of insufficient permeability and antibacteriality of the hard tissue bonding interface of the dentin is solved, and the early treatment of caries and root canal treatment is significantly improved and enhance the bonding strength of fracture fixation and intra-bone implants.
Patent Information
- Application Number
- CN202411096595.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-11-26
AI Technical Summary
The existing dental hard tissue repair materials are insufficiently penetrated during the bonding process, and the adhesive lacks stable bonding between the dentin matrix, resulting in the mixed layer being easily disintegrated, affecting the early treatment effect of caries and the success rate of root canal treatment. The bonding strength is insufficient during fracture fixation and intra-bone implant fixation.
Using a multifunctional hard tissue treatment agent based on the structure of thiol and sulfonic acid groups, a stable ionic bond is formed between thiol and hydroxyapatite through thiol-ethylenic bonding reaction, and a chemical bond with the bonding monomer is formed to promote the resin group. Material penetration forms a highly stable bonding interface with antibacterial and anti-enzymes.
Significantly improve the effects of tooth bonding, root canal treatment and fracture fixation, enhance the bonding strength, inhibit bacterial invasion and enzyme activity, improve the permeability and antibacteriality of repair materials, and prolong the stability of the mixed layer.
Smart Images

Figure HDA0004988108250000011 
Figure HDA0004988108250000012 
Figure HDA0004988108250000013
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of biological adhesive materials, and particularly relates to a multifunctional hard tissue treating agent based on a structural combination of thiol and sulfonic acid groups and its application. Technical Background
[0002] Dental caries is a chronic bacterial infection disease that affects the hard tissues of the teeth. It has a very high incidence rate and is characterized by progressive development. It is the main disease that causes tooth pain and loss of chewing function. The World Health Organization has listed dental caries, tumors, and cardiovascular diseases as the three major preventable diseases of humans. Due to the particularity of the hard tissues of the teeth, it is almost impossible to repair itself after damage. The repair of tooth defects mainly relies on alternative repairs with artificial materials such as resins. Therefore, the formation of a stable connection between the restorative material and the tooth tissue is the premise and prerequisite for successful repair.
[0003] The early manifestations of caries are white spots or brown spots. If no treatment measures are taken and it is allowed to develop, it will not only affect the appearance, but also caries cavities will soon form. At present, the most commonly used treatment for early enamel caries is infiltration resin, which is minimally invasive. Based on the low fluidity of infiltration resin, it enters the porous structure of demineralized enamel through capillary siphoning, blocks the channels for acidic substances and mineral ions to invade, enhances the acid resistance of the lesion, thereby blocking the progression of early caries and repairing defective tissues. However, this passive siphoning effect determines the inefficiency and limitation of infiltration, affecting the effect of treatment. How to promote the penetration of resin into the pore structure of enamel is the key to improving the treatment effect of early enamel caries.
[0004] If caries progresses further, it will affect the dentin. Dentin bonding forms a mixed layer, which is still the "short board" in the bonding joint. During the service of the composite, the mixed layer is prone to degradation and collapse, leading to restoration failure and a large number of secondary dental diseases. Insufficient penetration of the adhesive during the bonding process and the lack of stable bonding between the adhesive phase and the dentin matrix phase cause structural defects in the mixed layer. These structural defects lead to the disintegration of the mixed layer under chewing stress, endogenous enzyme action, and cariogenic bacteria attack. Therefore, solving the problem of dentin bonding durability requires simultaneously addressing the promotion of adhesive penetration, the formation of stable chemical bonding between the adhesive phase and the dentin matrix phase, and antibacterial and enzyme inhibition.
[0005] If caries progresses further, it will affect the dental pulp. Currently, the most commonly used treatment for pulpitis is root canal therapy. The sterilization of the root canal and the sealing of the root canal by filling materials are the keys to its success. The current root canal irrigants have relatively simple performances. Most of the irrigants only have irrigating and lubricating effects, and the bacterial microorganisms attached to the complex root canal system cannot be removed through root canal preparation, resulting in poor control of root canal system infection. Root canal irrigants with good bactericidal ability, tissue dissolving ability (dissolving the pulp), and the ability to remove bacterial biofilms have the disadvantages of high toxicity, corrosiveness, easy allergies, lack of sustained antibacterial and smear layer removal capabilities. Therefore, the development of antibacterial root canal irrigants with strong tissue dissolving ability, active binding properties to the root canal wall, and good biocompatibility is of great significance for improving the success rate of root canal treatment.
[0006] In fracture fixation and bone implant fixation, bone bonding with high bonding strength and without affecting bone healing is still a difficult problem. Improving bone bonding strength by treating the bone surface is of great significance to solving this problem. Summary of the invention
[0007] The object of the present invention is to provide a multifunctional hard tissue treating agent based on a thiol group and a sulfonic acid group structure compound, wherein the basic structural unit of the thiol group and the sulfonic acid group structure compound is (SH) m -R-(SO3) n , wherein SH is a thiol group, m represents the number of thiol groups (m≥1, and m is an integer); wherein SO3 is a sulfonate group, n represents the number of sulfonic acid groups (n≥1, and n is an integer); wherein R is an alkyl chain, which may contain an ester bond, an olefin bond, an amide group, an aromatic group, an imidazole group, an amino group, an amide group, a phosphoric acid group or a carboxylic acid group, and R may be an amide group, an aromatic group, an imidazole group, an amino group or an amide group. The compound includes a salt thereof.
[0008] The thiol and sulfonic acid structure compound contains at least one thiol group and one sulfonic acid group.
[0009] The thiol and sulfonic acid structure compound may have multiple thiol groups and / or multiple sulfonic acid groups.
[0010] The thiol group and sulfonic acid group of the thiol group and sulfonic acid structure compound may be located at both ends or in the middle of the compound chain.
[0011] The hard tissue treating agent is a solution containing mercapto, sulfonic acid structure compounds or their salts as essential components.
[0012] In the hard tissue treating agent, the concentration of the thiol group, sulfonic acid group structure compound and its salt is 0.001-1000 mg / mL.
[0013] The solvent of the hard tissue treating agent may be water, ethanol aqueous solution or acetone aqueous solution.
[0014] Another object of the present invention is to provide the use of the thiol and sulfonic acid group structure compounds and their salts in the preparation of hard tissue treatment agents for tooth bonding, bone bonding, improved restoration, caries prevention, root canal treatment, and irrigation and disinfection treatment, fracture fixation, and bone implant fixation. The multifunctional hard tissue treatment agent is a solution containing a thiol and sulfonic acid group structure compound or its salt as an essential component.
[0015] The hard tissue treating agent may contain fluoride ions or fluorine-containing nanoparticles as additives.
[0016] The hard tissue treating agent can be compounded with the existing dental acid etching agent to treat the tooth surface.
[0017] The hard tissue treatment agent must be used before the adhesive and must not be premixed with the adhesive.
[0018] When the hard tissue treating agent is used to treat the tooth surface, it can be coated on the tooth surface or the tooth surface after acid etching, the coating time is 3s-60s, and the number of coating times is 1 time-10 times.
[0019] When the hard tissue treating agent is used for root canal treatment, it can be rinsed by a flushing method, the flushing time is 3s-60s, and the number of flushing times is 1 time-10 times.
[0020] When the hard tissue treating agent is used to treat the bone surface, it can be applied or soaked, the treating time is 3s-60s, and the number of treating times is 1-10 times.
[0021] After use, the hard tissue treating agent can be rinsed with water, ethanol aqueous solution or pure ethanol, or the resin-based material, root canal filling material or bone adhesive can be used directly without rinsing.
[0022] After the tooth surface is treated with the hard tissue treating agent, it is rinsed with water or ethanol aqueous solution or pure ethanol, or the resin-based material is directly used without rinsing.
[0023] The resin-based material includes resin-based adhesive, resin-based cement, flowing resin or infiltrating resin.
[0024] After the root canal is treated with the hard tissue treating agent, it is rinsed with water or ethanol aqueous solution or pure ethanol, or the root canal filling material is directly used without rinsing.
[0025] After the bone surface is treated with the hard tissue treating agent, it is rinsed with physiological saline, or the bone adhesive is directly used without rinsing.
[0026] The sulfonic acid group at one end of the compound of the present invention forms a stable ionic bond with hydroxyapatite in hard tissue, while the thiol group at the other end not only has enzyme inhibition and antibacterial properties, but also has the ability to chemically bond with bonding monomers through thiol-ene bond click reaction. Unlike the current reaction monomers with ene bonds as polymerization groups, which need to be initiated by an initiator to undergo polymerization reactions, this compound based on thiol and sulfonic acid group structures can react spontaneously, quickly and efficiently with ene bond bonding monomers in current dentin adhesives under physiological conditions to obtain a bonding surface with adhesive penetration driving force, promote the penetration of resin-based materials, and then form a multifunctional, highly stable bonding interface with integrated structural functions of enzyme inhibition, antibacterial, and hard tissue-adhesive chemical bonding, and can effectively eliminate the adverse effects of saliva and blood contamination on bonding during clinical operations, and improve the effects of tooth bonding repair, root canal treatment, fracture fixation, and intraosseous implant fixation.
[0027] The technical problem to be solved by the present invention is to optimize the structure and function of the hard tissue bonding interface and improve the problem of poor hard tissue bonding effect. The compound of the present invention can actively combine with the components in the hard tissue to promote the penetration of the resin-based material; it has the ability to react with the polymerized monomer to form a stable chemical bond; it also has antibacterial properties, kills residual bacteria and resists bacterial invasion; in addition, it also needs to have the performance of inhibiting the activity of metal matrix proteases that cause collagen degradation. Instruction Manual
[0028] Figure 1 .Scanning electron microscope image of Example 4.
[0029] Figure 2 .Scanning electron microscope images of Examples 5 and 6.
[0030] Figure 3 .Scanning electron microscope images of Examples 7 and 8.
[0031] Figure 4 .Scanning electron microscope images of Examples 10 and 11.
[0032] Figure 5 .Examples 12 and 13 Fourier transform infrared spectroscopy.
[0033] Figure 6 .Photoelectron energy spectra of Examples 12 and 13.
[0034] Figure 7 .Scanning electron microscopy images of cell morphology.
[0035] Figure 8 .CCK-8 assay for cell activity.
[0036] Fig. 9 . Antibacterial activity of the solution against Staphylococcus aureus.
[0037] Fig.10 .Antibacterial activity of the solution against Escherichia coli.
[0038] Fig.11 . Antibacterial activity of the solution against Streptococcus mutans.
[0039] Fig.12 .Antibacterial activity of treated tooth surfaces against Staphylococcus aureus.
[0040] Fig.13 .Antibacterial activity of treated tooth surfaces against Escherichia coli.
[0041] Fig.14 .Antibacterial activity of treated tooth surfaces against Streptococcus mutans.
[0042] Fig.15 .Enzyme inhibition properties for total acid etching bonding.
[0043] Fig.16 .Enzyme inhibition properties for self-etching bonding.
[0044] Fig.17 .Adhesion performance for total acid etch bonding.
[0045] Fig.18 .Adhesion performance when used for self-etching bonding.
[0046] Fig.19 .Adhesive properties for saliva contamination.
[0047] Fig. 20 .Adhesive properties when used for bone bonding.
[0048] Fig.21 . Adhesion properties for blood contamination (contamination occurs after treatment).
[0049] Fig. 22 . Adhesive properties for blood contamination (contamination occurs before treatment). DETAILED DESCRIPTION
[0050] The present invention is described in more detail below with reference to the embodiments and the accompanying drawings, but the present invention is not limited to these embodiments.
[0051] Embodiment 1 The present invention provides a multifunctional hard tissue adhesive treatment agent based on a thiol group and a sulfonic acid group structural compound, wherein the basic structural unit of the thiol group and the sulfonic acid group structural compound is (SH) m -R-(SO3) n, wherein SH is a thiol group, m represents the number of thiol groups (m≥1, and m is an integer); wherein SO3 is a sulfonate group, n represents the number of sulfonic acid groups (n≥1, and n is an integer); wherein R is an alkyl chain, which may contain ester bonds, olefin bonds, amide groups, aromatic groups, imidazole groups, amino groups, amide groups, phosphoric acid, carboxylic acid groups, etc., and R may be amide groups, aromatic groups, imidazole groups, amino groups, amide groups, etc. The compounds include salts thereof.
[0052] The thiol and sulfonic acid structure compound contains at least one thiol group and one sulfonic acid group.
[0053] The thiol and sulfonic acid structure compound may have multiple thiol groups and / or multiple sulfonic acid groups.
[0054] The thiol group and sulfonic acid group of the thiol group and sulfonic acid structure compound may be located at both ends or in the middle of the compound chain.
[0055] Embodiment 2 A 1 mg / mL 2-mercaptoethanesulfonic acid (CAS No.: 3375-50-6) ethanol / water solution was prepared as a treating agent.
[0056] Embodiment 3 Dentin or enamel slices were prepared using a slow-speed cutter and rinsed with deionized water.
[0057] Embodiment 4 The treatment agent of Example 2 was applied to the dentin surface of Example 3 for 20 seconds and then blown dry.
[0058] Embodiment 5 The dentin surface of Example 3 was treated with 37% phosphoric acid solution for 15 seconds and then rinsed with a large amount of deionized water.
[0059] Embodiment 6 The treatment agent of Example 2 was applied to the dentin surface obtained in Example 5 for 20 seconds and then rinsed with a large amount of deionized water.
[0060] Embodiment 7 Treat the enamel surface with 37% phosphoric acid solution for 30 seconds and rinse with plenty of deionized water.
[0061] Embodiment 8 The treatment agent of Example 2 was applied to the enamel surface obtained in Example 7 for 20 seconds, and then rinsed with a large amount of deionized water.
[0062] Embodiment 9 Treat the enamel surface with 37% phosphoric acid solution for 15 seconds and rinse with plenty of deionized water.
[0063] Embodiment 10 The treatment agent of Example 2 was applied to the surface of the tooth enamel obtained in Example 9 for 20 seconds and then blown dry.
[0064] Embodiment 11 The samples obtained in Examples 3-10 were dehydrated with gradient ethanol and observed under a field emission scanning electron microscope. It can be seen that the treatment agent in Example 2 can dissolve the stain layer and expose the dentin organic matrix network (Example 4, Figure 1 ); Compared with the dentin surface treated with 37% phosphoric acid (Example 5), the further treatment with the treatment agent of Example 2 (Example 6) had no obvious morphological changes ( Figure 2 ); Compared with the enamel surface treated with 37% for 30s (Example 7), the further treatment with the treatment agent of Example 2 (Example 8) showed no obvious morphological changes ( Figure 3 ); Compared with the enamel surface treated with 37% phosphoric acid for 15s (Example 9), the further treatment with the treatment agent of Example 2 (Example 10) makes the enamel pillars more fully exposed ( Figure 4 ).
[0065] Embodiment 12 The hydroxyapatite sheets were rinsed with deionized water and freeze-dried.
[0066] Embodiment 13 The treating agent obtained in Example 2 was coated on the surface of hydroxyapatite for 20 seconds, rinsed with a large amount of deionized water, and freeze-dried.
[0067] Embodiment 14 The hydroxyapatite sheets obtained in Examples 12 and 13 were used for Fourier transform infrared spectroscopy detection. -1 The peak is attributed to the PO stretching band of the phosphate group. After modification, the phosphate group reacts with hydrogen ions and the peak blue-shifts to 880 cm -1 . At 1560cm -1 The new peak at is COO - The stretching vibration of COOH and Ca 2+ On the surface of hydroxyapatite, ionic bonds are formed ( Figure 5 ).
[0068] Embodiment 15 The hydroxyapatite sheets obtained in Examples 12 and 13 were used for photoelectron spectroscopy analysis. The peaks at the positions with binding energies of 163 eV and 226 eV corresponded to the peaks of S(2p) and S(2s), indicating that the thiol groups were adsorbed on the hydroxyapatite ( Figure 6 ).
[0069] Embodiment 16 L929 cells were cultured on the surface of the dentin slices obtained in Examples 3 and 4 for 24 hours, fixed, dehydrated, and the cell morphology was observed under a scanning electron microscope. It can be seen that the cells in Example 4 spread into a spindle shape, and there is no significant difference in morphology between the cells in Example 4 and the control ( Figure 7 ).
[0070] Embodiment 17 After L929 cells were cultured on the surface of the dentin slices obtained in Examples 3 and 4 for 24 hours, the cell activity was detected using a CCK8 kit. There was no significant difference in the cell activity of Example 4 compared with the control ( Figure 8 ).
[0071] Embodiment 18 Different concentrations of 2-mercaptoethanesulfonic acid aqueous solutions were prepared to test their antibacterial activity against Staphylococcus aureus. When the concentration was 1.25%, it showed obvious antibacterial activity, and the antibacterial rate was close to 100% ( Fig. 9 ).
[0072] Embodiment 19 Different concentrations of 2-mercaptoethanesulfonic acid aqueous solutions were prepared to test their antibacterial activity against Escherichia coli. When the concentration was 1.25%, it showed obvious antibacterial activity, and the antibacterial rate was close to 100% ( Fig.10 ).
[0073] Embodiment 20 Different concentrations of 2-mercaptoethanesulfonic acid aqueous solutions were prepared to test their antibacterial activity against Streptococcus mutans. When the concentration was 5%, it showed obvious antibacterial activity, and the antibacterial rate was close to 100% ( Fig.11 ).
[0074] Embodiment 21 Staphylococcus aureus was cultured on the surface of the dentin slices obtained in Examples 3 and 4. After 24 hours of culture, the dead and live bacteria detection kit was used for staining. Laser confocal microscopy was used for observation and it was found that the number of dead bacteria increased significantly ( Fig.12 ).
[0075] Embodiment 22 Escherichia coli was cultured on the surface of the dentin slices obtained in Examples 3 and 4, and stained with a dead and live bacteria detection kit after 24 hours of culture. Laser confocal microscopy revealed that the number of dead bacteria in Example 4 increased significantly ( Fig.13 ).
[0076] Embodiment 23 Mutans Streptococcus was cultured on the surface of the dentin slices obtained in Examples 3 and 4, and stained with a dead and live bacteria detection kit after 24 hours of culture. Laser confocal microscopy was used to observe and found that a large number of dead bacteria ( Fig.14 ).
[0077] Embodiment 24 The dentin surface obtained in Examples 5 and 6 was coated with the total acid etching adhesive Spectrum bond, applied for 20 seconds, blown gently for 15 seconds, and illuminated with a light curing lamp for 20 seconds, and the resin was layered to a resin layer of 1 mm thickness. After 24 hours in a 37°C water bath, a dentin-resin sheet with a thickness of 100 μm was prepared using a slow cutter. The enzyme activity in the demineralized dentin matrix was determined using the EnzChek gelatin activity kit (E-12055, Molecular Probes, Eugene, OR, USA). The diluted gelatin matrix was dropped onto the dentin slice, covered with a coverslip, and incubated at 37°C in a humid environment with a relative humidity of 100% under light-proof conditions. The demineralized layer was scanned layer by layer by CLSM, with an emission light of 530 nm and an excitation light of 488 nm, and the fluorescence intensity of the mixed layer was observed. Unlike the strong fluorescence of the mixed layer in Example 5, the mixed layer in Example 6 had almost no fluorescence ( Fig.15 ).
[0078] Embodiment 25 The dentin surface obtained in Examples 3 and 4 was coated with the self-etching adhesive Single bond universal, applied for 20 seconds, gently blown for 15 seconds, and illuminated with a light-curing lamp for 20 seconds, and the resin was layered to a thickness of 1 mm. A slow cutter was used to prepare a dentin-resin sheet with a thickness of 100 μm. The enzyme activity in the demineralized dentin matrix was determined using the EnzChek gelatin activity kit (E-12055, Molecular Probes, Eugene, OR, USA). The diluted gelatin matrix was dropped onto the dentin slice, covered with a coverslip, and incubated at 37°C in a humid environment with a relative humidity of 100% under light-proof conditions. The demineralized layer was scanned layer by layer by CLSM, with an emission light of 530 nm and an excitation light of 488 nm, and the fluorescence intensity of the mixed layer was observed ( Fig.16 ).
[0079] Embodiment 26 The dentin obtained in Examples 5 and 6 and the enamel obtained in Examples 9 and 10 were coated with Spectrum bond for 20 seconds, blown gently for 15 seconds, and illuminated with a light curing lamp for 20 seconds. The resin was layered to a 3 mm thick resin layer. After 24 hours in a 37°C water bath, a 1 mm × 1 mm tooth strip was prepared with a slow cutter. The micro tensile fracture strength of the sample was tested with a micro tensile instrument, and the cross-sectional dimensions were recorded. The micro tensile strength ( Fig.17 ).
[0080] Embodiment 27 The Bond component of Clearfil SEBond was applied to the dentin obtained in Example 4 and the enamel obtained in Example 10, respectively. Apply for 20 seconds, blow gently for 15 seconds, and lightly cure for 20 seconds, and then build up the resin layer in layers to a thickness of 3 mm. After 24 hours in a 37°C water bath, a slow cutter was used to prepare a 1mm×1mm tooth strip with a bonding surface. The micro-tensile tester was used to test the micro-tensile fracture strength, and the cross-sectional dimensions were recorded to calculate the micro-tensile strength. The controls were the dentin obtained in Example 3 and the enamel obtained in Example 9, which were bonded according to the instructions of Clearfil SE Bond. ( Fig.18 ).
[0081] Embodiment 28 The dentin surface obtained in Examples 5 and 6 was soaked in human saliva for 20 seconds, and then dried with a small cotton swab until the surface was slightly moist. The Spectrum bond was applied for 20 seconds, and then blown for 15 seconds. The light-curing light was used for 20 seconds, and the resin was layered to a resin layer with a thickness of 3 mm. After 24 hours in a 37°C water bath, a 1mm×1mm tooth strip was prepared by a slow cutting machine. The micro-tensile fracture strength of the sample was tested by a micro-tensile instrument, and the cross-sectional dimensions were recorded. The micro-tensile strength ( Fig.19 ).
[0082] Embodiment 29 A slow-speed cutter and polisher were used to prepare a smooth surface of porcine cortical bone.
[0083] Embodiment 30 The treatment agent of Example 2 was applied to the surface of the cortical bone of Example 28 for 20 seconds and then blown dry.
[0084] Embodiment 31 The surface of the cortical bone obtained in Examples 28 and 29 was directly filled with a self-curing base resin whose main component was a methacrylate copolymer. After solidification at room temperature for 30 minutes, a bone strip with a bonding surface of 2 mm×2 mm was prepared using a slow cutting machine. The micro-tensile fracture strength of the sample was tested using a micro-tensile tester, and the cross-sectional dimensions were recorded. The micro-tensile strength ( Fig. 20 ).
[0085] Embodiment 32 The treatment agent obtained in Example 1 is used for root canal treatment to flush the root canal during root canal dredging and preparation.
[0086] Embodiment 33 A 2 mg / mL 2-mercaptoethanesulfonic acid ethanol / water solution (50 / 50) was prepared as a treatment agent. After the tooth surface was etched with phosphoric acid, the treatment agent was applied for 20 seconds and then adhesive restoration was performed.
[0087] Embodiment 34 Prepare 0.001 mg / mL 2-mercaptoethanesulfonic acid aqueous solution treatment agent, apply the treatment agent on the tooth surface for 20 seconds, rinse with plenty of water, and perform bonding restoration.
[0088] Embodiment 35 A 1mg / mg 4-mercaptobutanesulfonic acid (CAS No.: 24687-42-1) ethanol-water solution (50 / 50) was prepared as the treatment agent. After the tooth surface was acid-etched, the treatment agent was applied for 20 seconds, and then rinsed with a large amount of ethanol-water solution and repaired with bonding.
[0089] Embodiment 36 A 10 mg / mL 4-mercaptobenzenesulfonic acid (Cas No.: 7134-41-0) ethanol aqueous solution (60 / 40) was prepared as the treatment agent. After the tooth surface was acid-etched, the treatment agent was applied for 20 seconds and then repaired with bonding.
[0090] Embodiment 37 A 1 mg / mL 3-mercaptopropanesulfonic acid (Cas No.: 17636-10-1) ethanol aqueous solution (50 / 50) was prepared as the treatment agent. After the tooth surface was acid-etched, the treatment agent was applied for 30 seconds and then repaired with bonding.
[0091] Embodiment 38 A 5 mg / mL methyl tetrazolium mercaptosulfonate (Cas No.: 66242-82-8) ethanol aqueous solution (50 / 50) was prepared as the treatment agent. After the tooth surface was acid-etched, the treatment agent was applied for 30 seconds and then repaired with bonding.
[0092] Embodiment 39 A 10 mg / mL 4-mercaptobenzoic acid (Cas No.: 1074-36-8) ethanol aqueous solution (50 / 50) was prepared as the treatment agent. After the tooth surface was acid-etched, the treatment agent was applied for 20 seconds and then repaired with bonding.
[0093] Embodiment 40 A 5 mg / mL 2,3-dimercaptopropanesulfonic acid (Cas No.: 4076-02-2) ethanol aqueous solution (50 / 50) was prepared as the treatment agent. After the tooth surface was acid-etched, the treatment agent was applied for 20 seconds and then repaired with bonding.
[0094] Embodiment 41 2-Amino-1,4-benzenedisulfonic acid (Cas No.: 98-44-2) was modified by thiol group, and a 20 mg / mL product solution in ethanol-water solution (50 / 50) was prepared as a treatment agent. The tooth surface was coated with the treatment agent for 20 seconds after acid etching, and then repaired with bonding.
[0095] Embodiment 42 The dentin surface obtained in Examples 5 and 6 was contaminated with blood for 20 seconds, and then dried with a small cotton swab until the surface was slightly moist. Apply the total acid etching adhesive Spectrum bond, apply for 20 seconds, blow gently for 15 seconds, and light-curing light for 20 seconds, and layer the resin to a resin layer of 3 mm thickness. After 24 hours in a 37°C water bath, a slow cutter was used to prepare a 1mm×1mm tooth strip with a bonding surface. The sample micro-tensile instrument was used to test the micro-tensile fracture strength, and the cross-sectional dimensions were recorded. The micro-tensile strength ( Fig.21 ).
[0096] Embodiment 43 The dentin surface of Example 3 was contaminated with blood for 20 seconds, and then treated by Example 5 (acid etching) or Example 6 (acid etching + treatment agent treatment), and dried with a small cotton swab until the surface was slightly moist. Apply the total acid etching adhesive Spectrumbond, apply for 20 seconds, blow gently for 15 seconds, lightly cure for 20 seconds, and layer the resin to a 3mm thick resin layer. After 24 hours in a 37°C water bath, a slow cutter was used to prepare a 1mm×1mm tooth strip with a bonding surface. The sample micro-tensile instrument was used to test the micro-tensile fracture strength, and the cross-sectional dimensions were recorded. The micro-tensile strength ( Fig. 22 ).
Claims
1. A multifunctional hard tissue treating agent based on a thiol and sulfonic acid group structure compound, characterized in that: The basic structural unit of the thiol group, sulfonic acid group structure compound and its salt is (SH) m -R-(SO3) n , wherein SH is a thiol group, m represents the number of thiol groups, m≥1, and m is an integer, wherein SO3 is a sulfonate group, n represents the number of sulfonic acid groups, n≥1, and n is an integer, wherein R is an alkyl chain or an ester bond, an olefin bond, an amide group, an aromatic group, an imidazole group, an amino group, an amide group, the compound includes a salt thereof, and the concentration of the thiol group, sulfonic acid group structure compound and its salt is 0.001-1000 mg / mL.
2. The hard tissue treating agent according to claim 1, characterized in that: The alkyl chain may contain an ester bond, an olefin bond, an amide group, an aromatic group, an imidazole group, an amino group, an amide group, a phosphoric acid group or a carboxylic acid group.
3. The hard tissue treating agent according to claim 1, characterized in that: The solvent of the hard tissue pretreatment agent is water, ethanol aqueous solution or acetone aqueous solution.
4. The hard tissue treating agent according to claim 1, characterized in that: The thiol and sulfonic acid structure compound contains at least one thiol group and one sulfonic acid group.
5. The hard tissue treating agent according to claim 1, characterized in that: R is an amide group, an aromatic group, an imidazole group, an amino group or an amide group.
6. The hard tissue treating agent according to claim 1, characterized in that: The thiol and sulfonic acid structure compound has multiple thiol groups and / or multiple sulfonic acid groups.
7. The hard tissue treating agent according to claim 1, characterized in that: The thiol groups and sulfonic acid groups of the thiol and sulfonic acid structure compounds are at both ends or in the middle of the compound chain.
8. Use of the thiol-sulfonic acid group structure compound and its salt according to claim 1 in the preparation of a hard tissue treating agent for tooth bonding, root canal washing, bone bonding, improved restoration, caries prevention, washing and disinfection in root canal treatment, and fracture fixation and intraosseous implant fixation.
9. The use according to claim 8, characterized in that: The hard tissue treatment agent must be used before the adhesive and must not be premixed with the adhesive.
10. The use according to claim 8, characterized in that: When the treatment agent is used to treat tooth surface or bone surface, it can be applied or immersed, the treatment time is 3s-60s, and the number of treatments is 1 time-10 times.
11. The use according to claim 8, characterized in that: When the treatment agent is used to treat tooth surface, it can be compounded with existing dental acid etching agent to treat tooth surface, or firstly treated with acid etching agent and then treated with the treatment agent, or treated with the treatment agent alone.
12. The use according to claim 8, characterized in that: When the hard tissue treating agent is used for root canal treatment, a flushing method is used, the flushing time is 3s-60s, and the flushing times are 1 time-10 times.
13. The use according to claim 8, characterized in that: When the hard tissue treating agent is used to treat tooth surface or root canal, fluoride ions or fluorine-containing nanoparticles are added as additives.
14. The use according to claim 8, characterized in that: After the tooth surface or root canal is treated with the hard tissue treating agent, it is rinsed with an aqueous solution or an ethanol aqueous solution or pure ethanol, or the resin-based material is directly used without rinsing.
15. The use according to claim 8, characterized in that: After the bone surface is treated with the hard tissue treating agent, it is rinsed with physiological saline, or bone adhesives such as bone cement are directly used without rinsing.
16. The use according to claim 14, characterized in that The resin-based material is selected from resin-based adhesives, resin-based cements, flowing resins or penetrating resins.