Functionally modified mixed matrix membrane, preparation method and application in uranium-containing waste liquid treatment
By mixing the modified metal organic frame material with polymer to form a hybrid matrix membrane with high stability and selectivity, the problem of insufficient stability of existing membrane materials in acidic environments is solved, and the problem of low pH conditions is achieved Highly efficient separation and purification of uranyl.
Patent Information
- Application Number
- CN202411364408.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-11-26
AI Technical Summary
The existing membrane materials are inadequate in chemical stability, pollution resistance and separation efficiency when dealing with uranium-containing radioactive waste liquids, especially in acidic environments, which limits their application.
By mixing metal organic frame materials (MOFs) with polymers, modifying MOFs with alkylphosphonic acid, and co-crystallize with polyvinylidene fluoride and polyvinylpyrrolidone to form a hybrid matrix membrane with high stability and selectivity. Uranyl separation at low pH.
It realizes uranyl adsorption and capacity reduction in strong acid environments, improves the chemical stability and radiation resistance of membrane materials, maintains high separation performance, and is suitable for the treatment of uranium-containing wastewater in the nuclear fuel cycle.
Smart Images

Figure CN119015906A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the preparation of mixed matrix membranes, specifically to improving the stability of functional membrane materials by using metal-organic frameworks (MOFs) materials and their modified products, and applying them to reduce the volume of radioactive waste liquid in a low pH environment. Background Art
[0002] Nuclear energy is widely considered to be an ideal baseload energy source due to its low environmental pollution, high energy density and operational reliability. However, during the nuclear fuel cycle, a large amount of radioactive waste is generated, especially radioactive waste liquid with uranium as one of the main components. How to efficiently deal with the uranium element in the waste liquid has become a key issue in the sustainable use of nuclear energy.
[0003] Membrane processing has become one of the most promising technologies for treating uranium-containing radioactive waste liquid due to its environmental friendliness, simple preparation, high efficiency and good processing performance. However, uranium-containing waste liquid usually has the characteristics of high acidity, strong radioactivity and complex chemical composition, which limits the widespread application of membrane separation technology in this field. At the same time, metal-organic framework materials (MOFs), as a two-dimensional or three-dimensional porous crystal formed by self-assembly of metal sites or metal clusters and organic ligands, have the advantages of high crystallinity, strong modifiability and large porosity, and can effectively adsorb and separate uranium elements. However, most MOFs have poor chemical stability in acidic environments and are easily damaged.
[0004] Since both existing membrane materials and MOFs have significant deficiencies in treating uranium-containing radioactive waste liquid, how to effectively combine MOFs with membrane matrix to overcome the deficiencies in chemical stability, anti-pollution and separation efficiency of membrane materials, while improving the stability of MOFs under acidic conditions, has become a technical problem that needs to be solved urgently in this field. Summary of the invention
[0005] The purpose of the present invention is to provide a functionally modified mixed matrix membrane and a preparation method, in particular to provide a membrane material with high stability, high adsorption capacity and high selectivity for use in uranium radioactive waste liquid purification and volume reduction.
[0006] In the first aspect, the present invention provides a method for preparing a functionally modified mixed matrix membrane, comprising: dispersing the prepared first MOFs powder in an alkylphosphonic acid (APA) solution for chemical reaction to obtain a functionally modified second MOFs powder; respectively adding the second MOFs powder and the ionic liquid into a solvent for ultrasonic dispersion, then adding a polymer powder to the solvent for constant temperature stirring in an oil bath until the mixture is uniform to obtain a casting liquid; and degassing and film-forming the casting liquid, placing the formed membrane material in a constant temperature environment for phase inversion curing, and then immersing it in ultrapure water to obtain the target mixed matrix membrane.
[0007] According to the preferred embodiment of the first aspect, the preparation of the first MOFs powder includes: dissolving the organic ligand and the zirconium salt in formic acid and N,N-dimethylformamide (DMF) to obtain a MOFs mixed solution; and subjecting the MOFs mixed solution to a hydrothermal reaction and drying after multiple centrifugation and ethanol washing to obtain the first MOFs powder.
[0008] According to the preferred embodiment of the first aspect, the first MOFs powder is obtained by subjecting the MOFs mixed solution to a hydrothermal reaction at 120 to 160°C for 48 to 60 hours, and after the reaction, centrifuge separation and ethanol washing for 3 to 5 times, and then drying at 60 to 80°C for 10 to 12 hours, wherein each centrifugation time is 3 to 8 minutes.
[0009] Preferably, according to the first aspect, the second MOFs powder is obtained by ultrasonically dispersing the first MOFs powder in an APA solution, followed by a chemical reaction under stirring, and drying after multiple centrifugation and ethanol washing at the end of the reaction.
[0010] According to the preferred embodiment of the first aspect, the chemical reaction is carried out at 45°C for 12 to 24 hours, and the second MOFs powder is obtained after 3 to 5 times of centrifuge separation and ethanol washing after the chemical reaction, and then dried at 60 to 80°C for 10 to 12 hours, wherein each centrifugation time is 3 to 8 minutes.
[0011] According to the first aspect, the APA solution uses ethanol as a solvent, and the concentration of APA dissolved in ethanol is 0.4 to 0.9 mmol·L -1 .
[0012] According to the first aspect, the polymer powder includes polyvinylidene fluoride (PVDF) and polyvinyl pyrrolidone (PVP) powder.
[0013] According to the preferred embodiment of the first aspect, in the process of preparing the casting solution, the mass ratio of PVDF to PVP is 3:2, and the mass ratio of PVDF to MOFs is 1:0.7.
[0014] According to the first aspect, in the process of preparing the casting solution, the solvent is selected as N,N-dimethylacetamide (DMAc) or N,N-dimethylformamide (DMF), and the ionic liquid is selected as any one of the following: 1-hydroxyethyl-3-methylimidazolium hexafluorophosphate ([HEMIM]PF6), 1-ethyl-3-methylimidazolium tetrafluoroborate ([EMIM][BF4]), 1-butyl-3-methylimidazolium hexafluorophosphate ([BMIM][PF6]), 1-butyl-3-methylimidazolium chloride ([BMIM][Cl]), 1-ethyl-3-methylimidazolium bistrifluoromethanesulfonyl imide ([EMIM][NTf2]), and 1-ethyl-3-methylimidazolium acetate ([EMIM][OAc]).
[0015] According to the preference of the first aspect, the mixed matrix membrane is prepared by degassing the casting liquid for 12 to 24 hours, and then forming it by 3D printing or doctor blade coating process, and then placing the formed membrane material in a constant temperature oven at 55 to 65°C for phase inversion curing for 1 to 1.5 hours, and finally immersing the cured membrane material in ultrapure water for 2 to 6 hours to remove excess PVP and ionic liquid.
[0016] According to the preference of the first aspect, when the 3D printing forming preparation is adopted, the process parameters used include a needle with a diameter of 0.2 to 0.5 mm, a printing speed of 10 to 20 mm / s, a filling spacing of 0.8 to 1.2 mm, and a printing pressure of 0.3 to 0.5 MPa; when the scraping process is adopted for forming preparation, the process parameters used include a scraper advancement speed of 10 to 20 mm / s.
[0017] In a second aspect, the present invention provides a mixed matrix membrane obtained according to any method described in the first aspect.
[0018] In a third aspect, the present invention provides an application of the mixed matrix membrane according to the second aspect in separating and recovering uranyl from low-level uranium-containing wastewater during a nuclear fuel cycle.
[0019] Compared with the prior art, the preparation process of the mixed matrix membrane of the present invention has the following advantages: 1) the preparation process is simple and fast, all operations can be completed at room temperature, and the efficiency is high; 2) the functional modification of MOFs expands the application environment of the mixed matrix membrane and realizes uranyl adsorption and volume reduction in a strong acid environment; 3) it has a unique mass transfer channel, PVDF and PVP can co-crystallize to form spherulites, and the pores between the spherulites are interconnected to form a mass transfer channel; 4) the radiation resistance of the MOFs modified by APA is improved, and the prepared mixed matrix membrane still has a high separation performance after γ-ray irradiation with a total irradiation dose of 1000 kGy. This preparation process broadens the preparation method of MOFs mixed matrix membrane and its application prospects in the field of volume reduction and purification of uranium-containing radioactive waste liquid in the nuclear cycle.
[0020] It is to be understood that the foregoing general description and the following detailed description are exemplary only and are not restrictive of the invention. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The drawings described in this disclosure are for illustrative purposes only of selected embodiments and not all possible embodiments, and are not intended to limit the scope of the present disclosure.
[0022] Figure 1 A flow chart of the method for preparing the mixed matrix membrane of the present invention is shown;
[0023] Figure 2 The XRD patterns and water contact angles of HPA@MOF-808@PM in Example 1 and MOF-808@PM in Comparative Example 1 are shown;
[0024] Figure 3 Optical images of the mixed matrix membrane according to the present invention are shown, from left to right, MOF-808@PM of Comparative Example 1 and HPA@MOF-808@PM of Example 1; from top to bottom, samples before and after γ-ray irradiation;
[0025] Figure 4 The FTIR spectra of the samples of MOF-808 before and after functional modification of the present invention are shown, wherein (b) is a partial enlargement of (a);
[0026] Figure 5 and Figure 6 The SEM surface and cross-sectional morphologies of HPA@MOF-808@PM of Example 1 and MOF-808@PM of Comparative Example 1 are shown respectively, wherein: Figure 5 (j), (k), and (I) are the surface, local surface, and cross-sectional morphologies of HPA@MOF-808@PM, respectively; Figure 6 (g), (h), and (i) are the surface, local surface, and cross-sectional morphologies of MOF-808@PM, respectively;
[0027] Figure 7 The separation and removal rates of U(VI) in the solution by HPA@MOF-808@PM of Example 1 and MOF-808@PM of Comparative Example 1 during multiple cycles (a) and the loss of MOFS materials reflected by the Zr element content in the desorption solution (b) are shown;
[0028] Figure 8 The separation performance and separation selectivity of MOF-808@PM (a) of Comparative Example 1 and HPA@MOF-808@PM (b) of Example 1 before and after irradiation are shown. DETAILED DESCRIPTION
[0029] Embodiments of the present invention will be described in detail below in conjunction with examples. It will be appreciated by those skilled in the art that the following examples are only preferred embodiments of the present invention, so as to better understand the present invention, and thus should not be considered as limiting the scope of the present invention. For those skilled in the art, the present invention may have various changes and variations, and any modifications, equivalent replacements or improvements made within the spirit and principles of the present invention, etc., should all be included within the protection scope of the present invention.
[0030] The present invention generally relates to preparing membrane materials by mixing metal organic framework materials (MOFs) and their modified products with polymers to obtain mixed matrix membranes for separation and recovery of uranyl in low-level uranium-containing wastewater in the nuclear fuel cycle process. Figure 1 The flow chart of the preparation method of the mixed matrix membrane of the present invention is shown. Figure 1 As shown, a general example of the method for preparing the mixed matrix membrane is shown below.
[0031] (1) Preparation of the first MOFs powder
[0032] The invention comprises the steps of dissolving an organic ligand and a zirconium salt in a mixed solution of formic acid and N,N-dimethylformamide (DMF) to obtain a MOFs mixed solution, subjecting the MOFs mixed solution to a hydrothermal reaction, and drying the solution after multiple centrifugation and ethanol washing to obtain a first MOFs powder.
[0033] In this step, an organic ligand (e.g., trimesic acid) and a zirconium salt (e.g., zirconium oxychloride octahydrate) are first dissolved in formic acid and DMF to form a uniform MOFs mixed solution, and the solution is placed in a high-temperature reactor at 120 to 160°C for hydrothermal reaction. The hydrothermal reaction time is 48 to 60 hours to promote the growth of MOFs crystals, so that the zirconium salt and the organic ligand can be orderly self-assembled in the solution to form a three-dimensional porous structure. After the hydrothermal reaction is completed, the reaction product is centrifuged for multiple times, the centrifugation time is 3 to 8 minutes, and the speed is set to 10,000 rpm. After each centrifugation, the product needs to be rinsed with ethanol to remove the by-products and unreacted substances generated during the reaction. The centrifugation and ethanol rinsing process are usually performed alternately 3 to 5 times to ensure the purity and structural integrity of the MOFs powder. Finally, the product after centrifugal rinsing is placed in an oven at 60 to 80°C for drying, and the drying time is 10 to 12 hours until a pure first MOFs powder is obtained. The dried MOFs crystals are the first MOFs powder required by the present invention, which has good pore structure and chemical stability and is suitable for subsequent functional modification and membrane material preparation.
[0034] In the present invention, the types of MOFs used include but are not limited to MOF-808, MOF-801 and MOF-545, etc. These MOFs can show excellent performance in the subsequent modification and membrane material preparation process due to their unique porous structure and good chemical stability.
[0035] (2) Preparation of the second MOFs powder
[0036] The present invention also relates to functional modification of the first MOFs powder to prepare a functionalized second MOFs powder, by dispersing the first MOFs powder obtained in step (1) in an alkylphosphonic acid (APA) solution, and subjecting the first MOFs powder to a chemical reaction so that a modification reaction occurs on its surface, thereby obtaining a second MOFs powder having specific functional properties.
[0037] In this step, a certain amount of APA solution is first prepared. Ethanol is selected as the solvent to ensure that APA is completely dissolved in ethanol to form a uniform solution. The concentration of APA in ethanol is controlled to be between 0.4 and 0.9 mmol·L -1 In the range (preferably 0.5-0.7 mmol·L -1 ) to optimize the effect of the modification reaction and ensure that the surface of MOFs can fully contact and react with APA.
[0038] Next, the first MOFs powder obtained in step (1) is added to the APA solution. To ensure that the MOFs powder can be evenly dispersed in the solution, it is first subjected to ultrasonic dispersion to effectively break up the powder aggregates, increase its specific surface area, and thereby promote the reaction between MOFs and APA. After ultrasonic treatment, the mixture is placed in a stirrer for constant temperature stirring reaction. The reaction temperature is controlled at 45°C and the reaction time is 12 to 24 hours. This temperature and time range enables APA to fully contact the MOFs surface and undergo a chemical reaction, thereby introducing functional groups on the surface of the MOFs powder.
[0039] After the chemical reaction is completed, the product is still in a suspended state and needs to be separated and rinsed by centrifuge multiple times. First, the reaction system is centrifuged 3 to 5 times, with the time of each centrifugation controlled at 3 to 8 minutes and the centrifugal speed set to 10,000 rpm. The centrifugation process can effectively separate the modified MOFs powder and remove the residual solution and unreacted chemicals that may remain during the reaction process. In order to further purify the powder, the centrifuged MOFs powder needs to be rinsed with ethanol to remove residual reaction solvents and impurities. The rinsing process is alternated with the centrifugation operation.
[0040] Finally, the MOFs powder after centrifugation and washing is placed in a drying device and dried at a temperature of 60 to 80°C for 10 to 12 hours. The drying process can effectively remove the residual solvent in the MOFs powder, making it a completely dry functionalized MOFs powder. After this series of operations, the second MOFs powder obtained has the characteristics of functional modification and is suitable for the subsequent preparation of mixed matrix membranes.
[0041] (3) Preparation of casting solution
[0042] The present invention also has the steps of respectively adding the second MOFs powder (i.e. the modified first MOFs powder) and the ionic liquid into a solvent for ultrasonic dispersion, and then adding the polymer powder into the solvent for constant temperature stirring in an oil bath until the mixture is uniform to obtain a casting solution.
[0043] In this step, first, the second MOFs powder and the ionic liquid need to be added to an appropriate amount of solvent and ultrasonically dispersed (ultrasonic time is, for example, 30 to 50 minutes) to uniformly disperse the powder and liquid in the solvent to avoid the formation of agglomerates. The selected solvent is, for example, N,N-dimethylacetamide (DMAc) or N,N-dimethylformamide (DMF). These two solvents can dissolve polymers well and are compatible with MOFs and ionic liquids.
[0044] During the ultrasonic dispersion process, MOFs powder and ionic liquid are co-dispersed, and the resulting solution has excellent uniformity, providing a basis for the subsequent mixing step. The ionic liquid can be selected from different types of ionic liquids such as 1-hydroxyethyl-3-methylimidazolium hexafluorophosphate ([HEMIM]PF6), 1-ethyl-3-methylimidazolium tetrafluoroborate ([EMIM][BF4]), 1-butyl-3-methylimidazolium hexafluorophosphate ([BMIM][PF6]), 1-butyl-3-methylimidazolium chloride ([BMIM][Cl]), 1-ethyl-3-methylimidazolium bistrifluoromethanesulfonyl imide salt ([EMIM][NTf2]), 1-ethyl-3-methylimidazolium acetate ([EMIM][OAc]), preferably 1-hydroxyethyl-3-methylimidazolium hexafluorophosphate ([HEMIM]PF6). The presence of ionic liquid can not only effectively improve the performance of the membrane, but also have a positive effect on the viscosity and dispersibility of the casting solution. In some embodiments, based on the mass of 1 g of PVDF solid powder, 0.1 to 0.7 g of 1-hydroxyethyl-3-methylimidazolium hexafluorophosphate is required, and the preferred amount is 0.7 g, to ensure the ideal performance of the casting solution.
[0045] Subsequently, after the ultrasonic dispersion is completed, polyvinylidene fluoride (PVDF) and polyvinyl pyrrolidone (PVP) powders are added to the dispersed mixed solution of MOFs and ionic liquids in proportion. In some embodiments, the mass ratio of PVDF to PVP is set to 3:2. In addition, the mass ratio of PVDF to MOFs is 1:0.7 to ensure the reasonable distribution of MOFs powder in the membrane, so that the adsorption performance of the membrane in the uranyl separation and recovery process is optimized.
[0046] After adding the polymer powder, the entire solution is placed in a constant temperature oil bath for stirring. The oil bath temperature is constant and can be controlled within the range of 40 to 60°C (preferably 60°C). Under constant temperature stirring conditions, the polymer powder in the solution gradually dissolves to form a uniform casting solution. The stirring time of this process can be adjusted according to the specific situation, for example, it can be controlled within 5 to 8 hours to ensure that the solution is evenly mixed.
[0047] (4) Defoaming
[0048] After obtaining the casting solution in step (3), in order to ensure the uniformity and quality of the membrane material, it is necessary to degas the casting solution. Specifically, the degassing process is to transfer the casting solution from the stirring vessel to the barrel, and then stand for 12 to 24 hours to eliminate the bubbles introduced by the casting solution during ultrasonic dispersion and stirring. It should be understood that the presence of bubbles will affect the structure and performance of the final film, resulting in pores or defects in the film, thereby affecting the mechanical strength, separation efficiency and stability of the film. During the standing process, the barrel should remain stable and avoid vibration to avoid reintroducing bubbles during the degassing process.
[0049] (5) Film Forming
[0050] After obtaining the degassed casting solution, film forming can be carried out.
[0051] In some embodiments, a DIW (direct ink writing) 3D printing process can be used to prepare the film material. This process can accurately control the deposition path and thickness of the casting liquid to form a film material with a desired structure. The specific DIW 3D printing process parameters are as follows: a needle with a diameter of 0.2 to 0.5 mm is used as an extrusion print head, a printing speed of 10 to 20 mm / s, a filling spacing of 0.8 to 1.2 mm, and a printing pressure of 0.3 to 0.5 MPa. The specific implementation process of the DIW 3D printing is shown below.
[0052] a) Equipment preparation: Select a needle with a diameter of 0.2 to 0.5 mm and install it on the extrusion print head (i.e. barrel) of the 3D printer. Then load the barrel of the degassed casting liquid into the 3D printer. When filling, make sure that the liquid is well sealed to prevent bubbles from entering the material during the printing process.
[0053] b) Printing parameter settings: Set the printing speed to 10 to 20 mm / s to ensure uniform deposition of the material. Adjust the fill spacing to 0.8 to 1.2 mm to ensure that the distance between adjacent printing paths is appropriate to form a continuous film material. According to the viscosity and fluidity of the casting solution, adjust the printing pressure to 0.3 to 0.5 MPa to ensure stable and smooth extrusion of the material.
[0054] c) Printing process: Start the 3D printer and print the film material layer by layer according to the preset path, ensuring that the distance between the needle and the substrate surface is consistent to maintain uniform film thickness. Control the overlap rate of the printing path to ensure that the film layers are tightly combined to avoid structural breaks or discontinuities.
[0055] In some embodiments, the casting liquid can also be scraped using a conventional scraping method to obtain a film material. The specific implementation process of the scraping treatment is: first prepare the degassed casting liquid to ensure that the solution is bubble-free and has moderate viscosity. Then pour the casting liquid evenly on one end of the substrate, gently contact the polymer solution with a scraper, and push the scraper evenly at a speed of 10 to 20 mm / s. When pushing the scraper, maintain a certain angle to ensure that the solution is evenly coated on the surface of the substrate to form a uniform film layer. If the film thickness needs to be controlled, the distance between the scraper and the substrate can be adjusted as needed. If the required film thickness is not achieved in one scraping, multiple scrapings can be performed after the initial scraping film layer is cured, and each operation maintains a consistent advancement speed and angle. However, care should be taken to avoid repeated scraping on an undried film layer to prevent damage or unevenness to the film layer.
[0056] In addition to 3D printing and doctor blade coating, other molding processes such as electrospinning can also be used to prepare membrane materials. The appropriate membrane making process is selected according to specific needs to ensure that the performance and structure of the membrane material meet the application requirements.
[0057] (6) Curing and shaping
[0058] The present invention also has the steps of placing the formed membrane material in a constant temperature environment for phase inversion solidification, and then soaking it in ultrapure water to obtain the target mixed matrix membrane.
[0059] In this step, the formed membrane material is first placed in a constant temperature oven at 55 to 65°C for phase inversion curing for 1 to 1.5 hours. The purpose of phase inversion curing is to promote the molecular rearrangement of the polymer in the membrane material by controlling the temperature and time, so that it gradually changes from liquid to solid, thereby forming a more stable and dense membrane structure. This process can not only improve the mechanical strength of the membrane material, but also effectively enhance its durability, so that it has higher compressive and tensile strength in subsequent use.
[0060] After the curing is completed, the membrane material is taken out of the oven and soaked in ultrapure water for 2 to 6 hours to remove the residual PVP and ionic liquid in the membrane material. PVDF, as a hydrophobic material, is retained as the main component of the membrane material during this process. This selective retention property gives the membrane material excellent chemical stability and mechanical properties. Through the curing and soaking treatment, the resulting mixed matrix membrane can show excellent pore size control and filtration capabilities, which is particularly suitable for achieving efficient separation and recovery of uranyl in the treatment of nuclear fuel cycle wastewater.
[0061] The preparation process of the mixed matrix membrane of the present invention has the following advantages: 1) the preparation process is simple and fast, all operations can be completed at room temperature, and the efficiency is high; 2) the functional modification of MOFs expands the application environment of the mixed matrix membrane and realizes uranyl adsorption and volume reduction in a strong acid environment; 3) it has a unique mass transfer channel, PVDF and PVP can co-crystallize to form spherulites, and the pores between the spherulites are interconnected to form a mass transfer channel; 4) the radiation resistance of the MOFs modified by APA is improved, and the prepared mixed matrix membrane still has a high separation performance after γ-ray irradiation with a total irradiation dose of 1000 kGy. This preparation process broadens the preparation method of MOFs mixed matrix membrane and its application prospects in the field of volume reduction and purification of uranium-containing radioactive waste liquid in the nuclear cycle.
[0062] In order to better understand the present invention, the implementation process of the present invention is further described below based on detailed examples, but it should be understood that the present invention is not limited to the following examples.
[0063] Example 1
[0064] The APA solution used in this embodiment is specifically an n-hexyl phosphoric acid (HPA) solution. It should be understood that APA is a general term for a class of organic substances. HPA, as a specific APA, has a molecular structure composed of a six-carbon alkyl chain and a phosphate group. APA is an important class of organophosphorus compounds composed of an alkyl group and a phosphate group, with the general formula R-PO(OH)2. It has acidity and good coordination ability, and can form stable complexes with metal ions. HPA has good solubility in organic solvents, exhibits moderate acidity and high thermal stability (boiling point exceeds 200°C).
[0065] The specific implementation process of this embodiment is shown below.
[0066] (1) Weigh 0.3023 g zirconium oxychloride octahydrate and add it into a 100 mL reactor. Weigh 0.1965 g trimesic acid and add 30 mL DMF and 30 mL formic acid into the reactor, respectively. After sonication for 30 min to dissolve, keep the reactor at 130 °C for 48 h to carry out hydrothermal reaction. After cooling to room temperature, centrifuge for 4 times (5 min each time at 10,000 rpm) and wash with anhydrous ethanol. Then, dry the product in an oven at 70 °C for 12 h to obtain MOF-808 white powder, which is the first MOFs powder mentioned above.
[0067] (2) Add the MOF-808 powder obtained in step (1) into the HPA solution (the solvent is ethanol, and the concentration of APA in ethanol is 0.6 mmol·L -1 ), and then subjected to ultrasonic dispersion for 30 minutes, and then placed in a constant temperature stirrer at 45°C for stirring reaction for 24 hours, and then centrifuged 4 times (5 minutes each time, the speed was 10000 rpm) and washed with anhydrous ethanol, and then the product after centrifugation and washing was placed in an oven at 70°C for 12 hours to obtain HPA@MOF-808 white powder, which is the second MOFs powder mentioned above.
[0068] (3) Weigh 2.1 g of functionalized HPA@MOF-808 and 2.1 g of 1-hydroxyethyl-3-methylimidazolium hexafluorophosphate into a flask, use a measuring cylinder to measure 24.3 mL of DMAc and add them to the flask. Ultrasonic dispersion is carried out for 30 min. Then, 3 g of PVDF and 2 g of PVP are weighed and added to the flask. Stir for 12 h in a constant temperature oil bath at 60 °C to form a uniform casting solution.
[0069] (4) The casting solution obtained in step (3) is transferred from the stirring container to a barrel and allowed to stand for 12 h to eliminate bubbles introduced into the casting solution during ultrasonic dispersion and stirring.
[0070] (5) The feed barrel is equipped with a needle with a diameter of 0.35 mm, which is installed on the DIW 3D printer so that it moves along the x and y axes at a speed of 15 mm / s on the substrate, with a filling spacing of 1 mm and a printing air pressure of 0.4 MPa. For the embodiment using the traditional scraping method, the scraper is pushed at the same speed of 15 mm / s to form a uniform film material.
[0071] (6) The formed membrane material was placed in a constant temperature oven at 60 °C for 1.5 h to undergo phase inversion curing treatment and finally immersed in ultrapure water for 4 h to remove the ionic liquid and excess PVP and to separate the film from the stainless steel substrate (substrate), thereby obtaining a mixed matrix membrane, which was denoted as HPA@MOF-808@PM.
[0072] Comparative Example 1
[0073] The main difference between Comparative Example 1 and Example 1 is that the MOF-808 used is not functionally modified, and the other steps are the same. That is, compared with Example 1, Comparative Example 1 lacks step (2), and 2.1 g of MOF-808 is weighed in step (3). The mixed matrix membrane finally obtained according to Comparative Example 1 is recorded as MOF-808@PM.
[0074] Morphology characterization and performance testing
[0075] The morphological characterization and performance test of the present invention aims to analyze the performance of MOFs in mixed matrix membranes before and after functional modification, mainly through scanning electron microscopy (SEM), X-ray diffraction (XRD), water contact angle measurement, Fourier transform infrared spectroscopy (FTIR) and liquid immersion method, and combined with water flux test for performance evaluation. The following electron microscope images are obtained using a FEI Quanta 250F field emission environmental scanning electron microscope (Quant 250FEG); the X-ray diffraction pattern is provided by a powder X-ray diffractometer (Bruker-AXS D8 Advance).
[0076] Figure 2The XRD patterns and water contact angles of HPA@MOF-808@PM in Example 1 and MOF-808@PM in Comparative Example 1 are shown. It can be seen from the XRD pattern that the crystal structure of HPA@MOF-808 is basically consistent with the original MOF-808, indicating that the functional modification has not significantly changed the crystal phase structure of MOF. However, due to the introduction of HPA, the water contact angle of HPA@MOF-808 increased significantly, indicating that the introduced HPA molecules improve the hydrophobicity of the membrane, and the hexaalkyl chain in HPA gives the membrane better drainage ability, thereby weakening the adsorption of water on the membrane surface.
[0077] Figure 3 Optical images of the mixed matrix membrane according to the present invention are shown, from left to right, MOF-808@PM of Comparative Example 1 and HPA@MOF-808@PM of Example 1; from top to bottom, they are samples before and after γ-ray irradiation. It can be seen from the figure that the functionally modified membrane material is somewhat different from the unmodified membrane material in appearance, which is manifested in that the surface of the HPA@MOF-808@PM membrane is smoother and more uniform, and the overall light transmittance of the membrane material is slightly improved. The figure shows the samples before and after irradiation from top to bottom. After γ-ray irradiation, the appearance of the membrane material has not changed significantly, indicating that the chemical stability of MOFs is improved after functional modification, and it can effectively resist the radiation environment.
[0078] Figure 4 shows the FTIR spectra of the MOF-808 samples before and after functionalization modification, where (b) is a partial enlargement of (a). It can be seen from the figure that the functionalized HPA@MOF-808 has a new absorption peak in the band range of 500-1600 cm⁻¹, indicating that the HPA molecules have been successfully grafted onto MOF-808.
[0079] Figure 5 and Figure 6 The SEM surface and cross-sectional morphologies of HPA@MOF-808@PM of Example 1 and MOF-808@PM of Comparative Example 1 are shown respectively, wherein: Figure 5 (j), (k), and (I) are the surface, local surface, and cross-sectional morphologies of HPA@MOF-808@PM, respectively; Figure 6 (g), (h), and (i) are the surface, local surface, and cross-sectional morphologies of MOF-808@PM, respectively. SEM observations show that the surface of HPA@MOF-808@PM is more uniform and dense, and the local surface morphology shows that the smoothness of the material surface increases after functionalization. The cross-sectional morphology also shows that the density of the membrane has been improved. In contrast, the surface of MOF-808@PM has more microscopic defects and its cross-sectional structure is relatively rough, which is consistent with its lower water flux performance.
[0080] The porosity of the membrane was tested by a liquid immersion method, and the results are shown in Table 1. The porosity of the HPA@MOF-808@PM membrane of Example 1 was 37.06%, while the porosity of the MOF-808@PM membrane of Comparative Example 1 was 36.14%, and the porosities of the two were relatively close.
[0081]
[0082] Table 1 Specifically, the porosity is calculated using the following formula:
[0083]
[0084] Among them, W2 is the mass of wet membrane, W1 is the mass of dry membrane, ρ is the liquid density, A is the area of membrane, and d is the thickness of membrane. The porosity of membrane material is calculated by this formula, and the results show that functional modification has little effect on the porosity of membrane material, and the thickness and porosity of the two are similar.
[0085] In general, the mixed matrix membrane of Example 1 of the present invention has a thickness of 0.15 to 0.3 mm, a porosity of 35% to 40%, and a water flux of 20 to 50 L·m -2 ·h -1 MPa -1 .
[0086] Uranyl separation and recovery performance
[0087] The present invention evaluates the performance difference of HPA@MOF-808@PM and MOF-808@PM mixed matrix membranes in separating uranyl ions U(VI) through multiple recycling tests and uranyl separation tests in different acidic environments, with special attention paid to their separation performance, selectivity, stability and tolerance to radiation.
[0088] Figure 7 The separation and removal rates of U(VI) in the solution by HPA@MOF-808@PM of Example 1 and MOF-808@PM of Comparative Example 1 during multiple cycles (a) and the loss of MOFS material reflected by the Zr element content in the desorption solution (b) are shown.
[0089] The separation performance of the mixed matrix membrane for uranyl under different pH conditions was evaluated by the SDI measuring device. The pH of the test solution was 4.5, 1 and 1 M HNO3, respectively, and the results are shown in Table 2. The experiment shows that both HPA@MOF-808@PM and MOF-808@PM can achieve a high U(VI) removal rate under pH=4.5. However, when the pH value of the solution is reduced to 1 or lower 1M HNO3, the HPA@MOF-808@PM of Example 1 still maintains a high removal rate, while the removal rate of MOF-808@PM of Comparative Example 1 is significantly reduced. This difference shows that the functionalized HPA@MOF-808@PM exhibits better separation performance under strong acidic conditions, mainly due to the introduction of HPA, which enhances the chemical stability of MOFS materials, so that it can still maintain good structure and function under low pH conditions. However, MOF-808@PM that has not been functionalized has poor stability under acidic conditions and is prone to decomposition or structural collapse, resulting in a decrease in its separation performance.
[0090]
[0091] Table 2 The experiment shows that after 5 cycles of "adsorption-desorption-reduction", the separation and removal rate of HPA@MOF-808@PM is significantly higher than that of MOF-808@PM. This shows that the functionally modified MOFs material has better cycle stability in the process of adsorbing uranyl, and the introduction of HPA enhances the chemical stability of the material, thereby improving its reusability. In contrast, the separation and removal rate of the MOF-808@PM membrane of Comparative Example 1 decreased significantly after multiple cycles of use, which may be due to the gradual degradation and inactivation of MOF-808, which has not been functionally modified, during the cycle, resulting in the decline of its adsorption performance. The functional modification of HPA enhances the chemical stability of MOFS materials, enabling them to maintain a high separation performance in multiple cycles. In addition, the results also show that the HPA@MOF-808@PM of Example 1 has almost no loss of Zr elements during multiple cycles, while the MOF-808@PM of Comparative Example 1 has obvious Zr element dissolution, indicating that its structure is damaged during the cycle and part of the MOFS material dissolves into the desorption solution. This difference in material loss further verifies that the functional modification of HPA can effectively enhance the structural stability of MOF and reduce the loss of MOF in acidic and multiple adsorption-desorption processes. Therefore, HPA@MOF-808@PM not only maintains a high separation performance, but also exhibits excellent stability during cyclic use.
[0092] Figure 8The separation performance and separation selectivity of MOF-808@PM (a) of Comparative Example 1 and HPA@MOF-808@PM (b) of Example 1 before and after irradiation are shown. The test shows that after irradiation with a total irradiation dose of 1000 kGy of gamma rays, the separation performance of Example 1 remains almost unchanged, and the separation selectivity does not decrease significantly, indicating that HPA@MOF-808@PM has good radiation resistance. In contrast, the performance of MOF-808@PM decreased significantly after irradiation. MOF-808 without functional modification has poor tolerance to radiation, and some structural damage occurs during the irradiation process, resulting in decreased separation performance and selectivity. In addition, the polymer matrix of the membrane showed a slight yellowing phenomenon on a macroscopic scale after irradiation, indicating that the irradiation had a certain effect on the mechanical properties of the material.
[0093] It can be seen that the present invention significantly improves the chemical stability of MOF by functionalizing MOFs materials with HPA. Before functionalization, MOFs are prone to degradation or structural collapse in strong acidic or complex chemical environments, resulting in decreased adsorption performance. Through the introduction of HPA, the pore structure of MOFs is strengthened, and the interaction between HPA molecules and MOF skeletons enhances the durability of the material under extreme conditions, allowing it to maintain structural integrity and functional activity in a strong acidic environment of pH ≤ 1.
[0094] The functionalized MOFs were blended with PVDF-PVP matrix to prepare mixed matrix membranes. PVDF and PVP as matrix materials provide good membrane formability and mechanical strength. In particular, the excellent chemical stability and hydrophobicity of PVDF enable the membrane to provide a stable mass transfer channel in a complex solution environment. The introduction of PVP improves the hydrophilicity of the membrane and optimizes the water flux of the membrane. However, these polymers themselves do not contain reactive functional groups, so they do not directly participate in the adsorption and separation process of uranyl, but rely on the MOFs materials mixed in the matrix to achieve efficient separation of U(VI). The porous structure of MOFs and their excellent adsorption capacity for metal ions play a key role in the membrane.
[0095] After functional modification, the chemical stability of MOFs materials has been significantly improved, which is reflected in the greatly enhanced adsorption capacity of uranyl ions U(VI) in strong acidic solutions. Especially in extremely acidic environments with a pH of ≤ 1, the HPA@MOF-808@PM mixed matrix membrane exhibits excellent separation effects. This is because the functionally modified MOFs can effectively resist the erosion of acidic media, maintain the integrity of their structure, and ensure that the adsorption and separation efficiency of U(VI) will not decrease significantly with the increase in acidity.
[0096] In addition, the radiation resistance of the mixed matrix membrane has also been significantly improved. After irradiation with a total irradiation dose of 1000 kGy of gamma rays, the functionally modified HPA@MOF-808@PM mixed matrix membrane still maintained good separation performance and selectivity, while the unmodified MOF-808@PM membrane showed a certain performance degradation after irradiation. This shows that the introduction of HPA not only enhances the chemical stability of MOFs, but also gives them stronger structural tolerance in irradiation environments, avoiding the degradation of material properties caused by irradiation. Therefore, the mixed matrix membrane of the present invention can stably achieve efficient separation of U(VI) in complex acidic and irradiated environments, showing good application prospects, and is particularly suitable for nuclear waste treatment and purification of radioactive waste liquid.
[0097] The applicant declares that the present invention illustrates the detailed features and detailed methods of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed features and detailed methods, that is, it does not mean that the present invention must rely on the above-mentioned detailed features and detailed methods to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., and other changes made within the knowledge scope of ordinary technicians in the field without departing from the purpose of the present invention, all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a functionalized modified mixed matrix membrane, comprising: The prepared first MOFs powder is dispersed in an alkylphosphonic acid (APA) solution to carry out a chemical reaction to obtain a functionally modified second MOFs powder; The second MOFs powder and the ionic liquid are added to a solvent for ultrasonic dispersion, and then the polymer powder is added to the solvent for constant temperature stirring in an oil bath until the mixture is uniform to obtain a casting solution; and The casting solution is degassed and film-formed, and the formed membrane material is placed in a constant temperature environment for phase inversion solidification, and then immersed in ultrapure water to obtain the target mixed matrix membrane.
2. The method according to claim 1, wherein the preparation of the first MOFs powder comprises: The organic ligand and the zirconium salt are co-dissolved in formic acid and N,N-dimethylformamide (DMF) to obtain a MOFs mixed solution; as well as The MOFs mixed solution is subjected to a hydrothermal reaction and after the reaction is completed, it is centrifuged and washed with ethanol for multiple times and then dried to obtain the first MOFs powder.
3. The method according to claim 2, wherein the first MOFs powder is obtained by subjecting the MOFs mixed solution to a hydrothermal reaction at 120 to 160°C for 48 to 60 hours, and after the reaction is completed, centrifuge separation and ethanol washing are performed 3 to 5 times, and then drying at 60 to 80°C for 10 to 12 hours, wherein each centrifugation time is 3 to 8 minutes.
4. The method according to claim 1, wherein the second MOFs powder is obtained by ultrasonically dispersing the first MOFs powder in an APA solution, then performing a chemical reaction under stirring conditions, and drying after multiple centrifugation and ethanol washing at the end of the reaction.
5. The method according to claim 4, wherein the chemical reaction is carried out at 45°C for 12 to 24 hours, and the second MOFs powder is obtained after 3 to 5 times of centrifuge separation and ethanol washing after the chemical reaction, and then dried at 60 to 80°C for 10 to 12 hours, wherein each centrifugation time is 3 to 8 minutes.
6. The method according to claim 4 or 5, wherein the APA solution uses ethanol as a solvent, and the concentration of APA dissolved in ethanol is 0.4 to 0.9 mmol·L -1 .
7. The method of claim 1, wherein the polymer powder comprises polyvinylidene fluoride (PVDF) and polyvinyl pyrrolidone (PVP) powders.
8. The method according to claim 7, in the process of preparing the casting solution, the mass ratio of PVDF to PVP is 3:2, and the mass ratio of PVDF to MOFs is 1:0.
7.
9. The method according to claim 1, in the process of preparing the casting solution, the solvent is selected from N, N-dimethylacetamide (DMAc) or N, N-dimethylformamide (DMF), and the ionic liquid is selected from any one of the following: 1-Hydroxyethyl-3-methylimidazolium hexafluorophosphate ([HEMIM]PF6), 1-Ethyl-3-methylimidazolium tetrafluoroborate ([EMIM][BF4]), 1-Butyl-3-methylimidazolium hexafluorophosphate ([BMIM][PF6]), 1-Butyl-3-methylimidazolium chloride ([BMIM][Cl]), 1-Ethyl-3-methylimidazolium bis(trifluoromethanesulfonyl)imide salt ([EMIM][NTf2]), 1-Ethyl-3-methylimidazolium acetate ([EMIM][OAc]).
10. The method according to claim 7, wherein the mixed matrix membrane is prepared by degassing the casting solution for 12 to 24 hours, and then forming it by 3D printing or doctor blade coating process, and then placing the formed membrane material in a constant temperature oven at 55 to 65° C. for 1 to 1.5 hours of phase inversion curing, and finally immersing the cured membrane material in ultrapure water for 2 to 6 hours to remove excess PVP and ionic liquid.
11. The method according to claim 10, wherein when the 3D printing forming process is adopted, the process parameters used include a needle with a diameter of 0.2 to 0.5 mm, a printing speed of 10 to 20 mm / s, a filling spacing of 0.8 to 1.2 mm, and a printing pressure of 0.3 to 0.5 MPa; when the scraping process is adopted, the process parameters used include a scraper advancement speed of 10 to 20 mm / s.
12. A mixed matrix membrane obtained according to the method of any one of claims 1 to 11.
13. Use of the mixed matrix membrane according to claim 12 for separation and recovery of uranyl from low-level uranium-containing wastewater in a nuclear fuel cycle.