High-flux pollution-resistant polyamide reverse osmosis membrane as well as preparation method and application thereof

By interfacial polymerization on the surface of the polyamide reverse osmosis membrane, the dense functional layer and grafting high fluorination aliphatic fluorides are solved, and the existing membranes are achieved with high throughput and stain resistance. Improve and reduce usage costs.

CN119015909APending Publication Date: 2024-11-26CANGZHOU INSTITUTE OF TIANGONG UNIVERSITY +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411329860.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing polyamide reverse osmosis membranes are insufficient in the face of different charged small-molecular organic pollutants, resulting in increased flux attenuation and usage costs. The existing modification methods are low in grafting efficiency and limited in stain resistance. .

Method used

By using the interfacial polymerization method of polyamine and polyacid chloride on the surface of the polyamide reverse osmosis membrane, the dense functional layer is formed, and the high fluorination aliphatic fluoride is used as graft molecules to increase the amino group and acid chloride on the surface of the membrane through the amidation reaction. The grafting efficiency of the group reduces the free energy and potential of the film surface and improves the film's pollution resistance.

Benefits of technology

It significantly improves the water permeability and pollution resistance of the polyamide reverse osmosis membrane, reduces the free energy and potential of the membrane surface, enhances the pollution resistance of different types of pollutants, reduces the flux attenuation rate, reduces the maintenance frequency and Cost of use.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119015909A_ABST
    Figure CN119015909A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a polyamide reverse osmosis membrane with high flux and pollution resistance, the surface of the membrane is modified by fluorine-containing molecules with different fluorination degrees through a secondary interfacial polymerization process, and residual acyl chloride groups on the surface of the polyamide membrane are used as grafting sites to greatly improve the grafting efficiency; the polyamide membrane has an ultrahigh pure water permeability coefficient of more than 4 LMH / bar and a relatively low surface free energy of less than 51 mJ m <-2 >, and shows excellent pollution resistance to charge and neutral pollutants; the polyamide reverse osmosis membrane can remove and recover pollution sources or effective substances contained in pollutants such as dyeing wastewater, electrodeposition coating wastewater and the like which are causes of public nuisance, and contributes to the sealing of the wastewater. In addition, the present invention can be used for high-level treatments such as concentration of active ingredients in food applications and the like, removal of harmful ingredients in water purification applications, sewage applications and the like, and can be used for wastewater treatment in oil fields, shale gas fields and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of functional separation membrane materials, and in particular to a pollution-resistant polyamide composite membrane and a preparation method and application thereof, and specifically to a high-throughput pollution-resistant polyamide composite reverse osmosis membrane and a preparation method and application thereof. The composite reverse osmosis membrane is suitable for the production of ultrapure water, desalination of salt water or seawater, etc., and can remove and recover pollution sources or effective substances contained in pollutants such as dyeing wastewater, electrodeposition coating wastewater, etc. that are the causes of public hazards. Background Art

[0002] Thin-layer composite polyamide (PA) reverse osmosis (RO) membranes have the advantages of high permeability, high salt rejection, high chemical stability, simple preparation process and easy industrialization, and are widely used in seawater desalination, sewage treatment and other fields. However, in actual applications, membrane fouling seriously affects the separation efficiency and service life of RO membranes, greatly increases the operating cost of RO systems and restricts their application in complex water environments. Therefore, the development of reverse osmosis membranes with excellent pollution resistance is the current research focus in the membrane field.

[0003] Although existing studies have successfully improved the RO membrane's resistance to certain types of pollutants by surface grafting of hydrophilic materials and positively charged materials (CN112316752A and CN 111558300 A), it is difficult to simultaneously improve the resistance to small molecule organic pollutants of different charge types. Fluorine-containing materials are reported to be a type of pollution-resistant material with low surface energy, but there are few studies on the use of fluorine-containing materials to modify polyamide reverse osmosis membranes to improve the membrane's resistance to pollution. The patent CN 109569328 A has been published, using the residual amino groups on the surface of the nascent polyamide membrane as grafting sites to graft fluorine-containing molecules, which reduces the membrane's surface free energy to a certain extent, thereby improving the polyamide reverse osmosis membrane's resistance to pollution. However, the nascent polyamide membrane formed by interfacial polymerization has an excess of acyl chloride groups on its surface, and the proportion of residual amino groups is extremely low. Therefore, the above-mentioned disclosed patent adopts the method of reacting the acyl chloride groups on the grafted molecules with the residual amino groups on the surface of the nascent polyamide membrane, which results in an extremely low grafting efficiency of the fluorine-containing molecules. At the same time, the number of fluorine-containing groups in the selected modified molecules is relatively low (the number of fluorine atoms in a single molecule is less than 5). As a result, the pollution resistance of the prepared reverse osmosis membrane is limited (under 500ppm BSA conditions, the flux attenuation rate of the reverse osmosis membrane is greater than 30%), and frequent cleaning and maintenance are required, resulting in increased use costs. Therefore, it is of great value to use the residual acyl chloride on the surface of the nascent polyamide membrane as a grafting site to graft fluorine-containing molecules with a higher degree of fluorination to prepare a polyamide reverse osmosis membrane with excellent pollution resistance.

[0004] This patent invents a method for preparing a polyamide reverse osmosis membrane with both high flux and pollution resistance. The fluorine-containing molecules are grafted onto the surface of the polyamide reverse osmosis membrane by the amidation reaction between the amino groups in the grafted molecules and the residual acyl chloride groups on the membrane surface. This not only significantly improves the water permeability of the reverse osmosis membrane (the water permeability coefficient of the polyamide membrane is greater than 4LMH / bar, which is better than the water permeability of most reverse osmosis membranes reported so far), but also significantly reduces the surface free energy of the reverse osmosis membrane (surface free energy <51mJ m -2 ), and at the same time, the surface potential of the reverse osmosis membrane is improved in a neutral water environment (when pH = 7, the membrane surface potential is between -10eV and -32eV). In summary, the polyamide reverse osmosis membrane has excellent anti-fouling properties. Compared with other patents reporting the use of fluorinated molecules for surface grafting to improve the anti-fouling properties of polyamide membranes, in this patent, a large number of residual acyl chloride groups on the surface of the nascent polyamide membrane are used as grafting sites, and amino-containing aliphatic fluorinated molecules are grafted to the surface of the polyamide membrane by layer-by-layer interfacial polymerization. On the one hand, the residual acyl chloride groups on the surface of the polyamide membrane provide sufficient grafting sites for grafting aliphatic fluorinated molecules, greatly improving the grafting efficiency; on the other hand, compared with the grafted molecules with low fluorinated groups selected in the above-mentioned disclosed patents, this patent uses a series of aliphatic molecules with higher fluorination as grafted molecules, which effectively improve the membrane surface properties (such as surface energy, charge, etc.) and improve the anti-fouling properties of the polyamide membrane. Summary of the invention

[0005] The purpose of the present invention is to provide a polyamide reverse osmosis membrane having both high flux and pollution resistance.

[0006] The object of the present invention is to provide a method for preparing the polyamide reverse osmosis membrane having both high flux and pollution resistance.

[0007] The purpose of the present invention is to provide the application of the polyamide reverse osmosis membrane having both high flux and pollution resistance.

[0008] To this end, the technical solution of the present invention is as follows:

[0009] A polyamide reverse osmosis membrane with both high flux and pollution resistance, characterized in that the polyamide reverse osmosis membrane comprises a porous ultrafiltration base membrane and a polyamide dense functional layer; wherein the polyamide dense functional layer is prepared on the surface of the porous ultrafiltration base membrane by interfacial polymerization of polyamine monomers and polyacyl chloride monomers; the surface free energy of the polyamide functional layer is less than 51mJ m -2 The surface charge at pH = 7 is -10eV to -32eV; the pure water permeability coefficient of the polyamide functional layer is >4L m -2 h -1 bar -1; The flux attenuation rate of the feed solution of 200ppm dodecylammonium bromide (DTAB) is <55%, the flux attenuation rate of the feed solution of 200ppm sodium dodecyl sulfate (SDS) is <30%, and the flux attenuation rate of the feed solution of 200ppm bovine serum albumin (BSA) is <20%.

[0010] The polyamine monomers used include but are not limited to at least one of m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, 1,3,5-triaminobenzene, 1,2,4-triaminobenzene, 3,5-diaminobenzoic acid, amphenol, 2,4-diaminotoluene, 2,6-diaminotoluene, N,N-dimethylm-phenylenediamine, 2,4-diaminoanisole, and phenylenediamine; the aliphatic polyamine monomers include but are not limited to at least one of ethylenediamine, propylenediamine, tris(2-aminoethyl)amine, and N-phenylethylenediamine; the alicyclic polyamine monomers include but are not limited to 1,3-diaminocyclohexane, 1,2-diaminocyclohexane, 1,4-diaminocyclohexane, etc. The above polyamine components can be selected from one or more and used in combination, preferably aromatic amino compounds such as m-phenylenediamine.

[0011] The polyacyl chlorides used include but are not limited to aromatic polyacyl chlorides, aliphatic polyacyl chlorides, and alicyclic polyacyl chlorides; wherein the aromatic polyacyl chlorides include but are not limited to at least one of trimesoyl chloride, terephthaloyl chloride, isophthaloyl chloride, biphenyl dicarboxylic acid chloride, naphthalene dicarboxylic acid chloride, benzene trisulfonyl chloride, benzene disulfonyl chloride, and chlorosulfonyl phthaloyl chloride; the aliphatic polyacyl chlorides include but are not limited to at least one of propanyl chloride, butanyl chloride, glutaryl chloride, propanyl tricarboxylic acid chloride, butanyl tricarboxylic acid chloride, glutaryl tricarboxylic acid chloride, and glutaryl chloride; the alicyclic polyacyl chlorides include but are not limited to cyclopropane tricarboxylic acid chloride, cyclobutane tetracarboxylic acid chloride, cyclopentane tricarboxylic acid chloride, cyclopentane tetracarboxylic acid chloride, cyclohexane tricarboxylic acid chloride, tetrahydrofuran tetracarboxylic acid chloride, cyclopentane dicarboxylic acid chloride, cyclobutane dicarboxylic acid chloride, cyclohexane dicarboxylic acid chloride, and tetrahydrofuran dicarboxylic acid chloride. The above-mentioned polyacyl chloride components can be selected and used alone or in combination of multiple types, and aromatic acyl chloride compounds such as 1,3,5-benzenetricarboxylic acid chloride are preferably used.

[0012] Preferably, the aliphatic fluoride is composed of an amino group and a fluorine group, and has the following chemical structure:

[0013]

[0014] Among them, 2 <n<8。

[0015] More preferably, the aliphatic fluoride includes but is not limited to at least one of pentafluoropropylamine, heptafluorobutylamine, nonafluoropentylamine, undecafluorohexylamine and perfluoroheptylamine.

[0016] A polyamide reverse osmosis membrane with both high flux and pollution resistance is formed by forming the aforementioned polyamide functional layer on the surface of a porous ultrafiltration base membrane; the porous ultrafiltration base membrane includes but is not limited to cellulose acetate membrane, polyethersulfone membrane, polyvinylidene fluoride membrane, polysulfone membrane, polyacrylonitrile membrane and other polymer ultrafiltration membranes with a pore size range of 10nm to 100nm or inorganic ultrafiltration membranes such as inorganic alumina. In the composite polyamide reverse osmosis membrane, the porous ultrafiltration base membrane as a base mainly plays the role of supporting the polyamide functional layer, that is, the mechanical strength of the membrane is increased by the formation of the composite, so as to increase the application range of the functional membrane.

[0017] A method for preparing a polyamide reverse osmosis membrane having both high flux and pollution resistance, characterized in that it comprises the following steps;

[0018] S1. Immerse one side of the porous ultrafiltration base membrane in the polyamine monomer for 0.5 min to 10 min, and use a rubber roller or an air knife to remove excess aqueous monomer solution on the surface of the ultrafiltration base membrane;

[0019] S2, uniformly applying the organic solution of polyacid chloride to the surface of the carrier coated with the aqueous monomer solution obtained in step S1 for 0.5 min to 10 min to form a thin layer of composite polyamide film;

[0020] S3, uniformly applying the modified solution containing fluorine molecules to the surface of the thin layer composite polyamide membrane obtained in step S2 for 0.5 min to 3 min to generate a modified thin layer composite polyamide membrane;

[0021] S4, placing the modified thin-layer composite polyamide membrane obtained in step S3 at 50° C. to 160° C. for thermal crosslinking for 3 min to 15 min, and finally obtaining a polyamide reverse osmosis membrane.

[0022] The preparation method is simple to operate, has a short reaction time, and has good stability, and has the advantages of stable industrial preparation and can be scaled up for industrial application.

[0023] Preferably, the method for preparing the aqueous monomer solution in step S1 is: preparing an aqueous solution of a polyamine monomer with a mass fraction of 0.1 wt.% to 3 wt.%.

[0024] Preferably, in step S1, the aqueous monomer solution is coated on the upper surface of the porous ultrafiltration base membrane, and after waiting for 0.5 min to 10 min, the excess aqueous monomer solution on the membrane is poured off, and then step S2 can be performed.

[0025] Preferably, in step S2, the mass fraction of the polyacyl chloride in the organic mixed solution is 0.01wt.% to 5wt.%; the organic solvent used to prepare the organic mixed solution includes but is not limited to n-hexane, isoparaffin, n-nonane, and n-decane.

[0026] Preferably, in step S2, the surface of the carrier coated with the aqueous monomer solution is immersed in an organic mixed solution prepared with polyacyl chlorides for 0.5 min to 10 min, the membrane is taken out and left to stand for 1 min, and the organic solvent is allowed to evaporate before step S3 is performed.

[0027] Preferably, in step S3, the fluorine-containing molecule solution is uniformly coated on the surface of the nascent polyamide membrane obtained in step S2, and after waiting for 0.5 min to 3 min, the membrane is taken out and allowed to stand for 1 min, and then step S4 can be performed.

[0028] The invention discloses an application of a polyamide reverse osmosis membrane having both high flux and pollution resistance, specifically: using the polyamide reverse osmosis membrane as a reverse osmosis membrane in the fields of seawater desalination, sewage treatment, etc.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) The high-throughput and pollution-resistant polyamide reverse osmosis membrane prepared in the present application solves the problems of decreased membrane flux caused by typical small-molecule organic pollutants and the secondary pollution caused by them, and the inability to simultaneously improve the pollution resistance to different types of pollutants: wherein ① the amino groups in the fluorine-containing molecular structure react with the large number of acyl chloride groups remaining on the surface of the primary ecological membrane by the secondary interfacial polymerization method, which greatly improves the grafting rate of the modified molecules and effectively improves the surface properties of the membrane; ② the introduction of long-chain fluorine-containing molecules is conducive to reducing the free energy of the membrane surface and weakening the interaction between pollutants and the membrane surface, thereby facilitating the improvement of the pollution resistance of the polyamide reverse osmosis membrane; in summary, the polyamide separation membrane has excellent pollution resistance;

[0031] (2) The preparation method of the polyamide reverse osmosis membrane of the present application is a simple interfacial polymerization method and a secondary interfacial polymerization method, which simultaneously achieves the improvement of the comprehensive performance of the polyamide separation membrane and has good industrial production application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 A comparison diagram of the surface Zeta potential curves and surface free energy of the polyamide reverse osmosis membrane prepared in Example 1 of the present invention and Comparative Example 1;

[0033] Figure 2 This is a comparison chart of the selective permeability of the polyamide reverse osmosis membrane prepared in Example 1 of the present invention and Comparative Example 1;

[0034] Figure 3 This is a comparison chart of the pollution resistance of the polyamide reverse osmosis membrane prepared in Example 1 of the present invention and Comparative Example 1 to model charged small molecule pollutants. DETAILED DESCRIPTION

[0035] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments, but the following embodiments are by no means intended to limit the present invention in any way.

[0036] Example 1

[0037] A polyamide reverse osmosis membrane with both high flux and excellent pollution resistance is prepared by the following steps:

[0038] S1, dissolving m-phenylenediamine in water to prepare a 2 wt.% m-phenylenediamine aqueous solution to obtain an aqueous monomer solution; immersing one side of a porous ultrafiltration base membrane in the polyamine monomer solution for 2 minutes, and removing excess aqueous monomer solution on the surface of the ultrafiltration base membrane using a rubber roller or an air knife;

[0039] S2, dissolving trimesoyl chloride in n-hexane to prepare a 0.1wt.% trimesoyl chloride organic solution, stirring and mixing to obtain an oil phase monomer solution; applying the oil phase monomer solution evenly to the surface of the carrier coated with the aqueous phase monomer solution obtained in step S1 for 1 minute to form a thin layer of composite polyamide film;

[0040] S3, dissolving heptaflubutylamine in water to prepare a 2 wt.% heptaflubutylamine aqueous solution; then, evenly applying the obtained aqueous solution to the surface of the thin layer composite polyamide membrane obtained in step S2 for 2 minutes to generate a modified thin layer composite polyamide membrane;

[0041] S4, placing the modified thin layer composite polyamide membrane obtained in step S3 at 60° C. for 10 minutes for thermal crosslinking, and finally obtaining a polyamide reverse osmosis membrane.

[0042] Example 2

[0043] A polyamide reverse osmosis membrane having both high flux and excellent anti-fouling performance, which is different from Example 1 in that 2 wt. % of heptafluorobutylamine is replaced by 1 wt. % of heptafluorobutylamine.

[0044] Example 3

[0045] A polyamide reverse osmosis membrane having both high flux and excellent anti-fouling performance, which is different from Example 1 in that 2 wt. % of heptafluorobutylamine is replaced by 5 wt. % of heptafluorobutylamine.

[0046] Example 4

[0047] A polyamide reverse osmosis membrane having both high flux and excellent anti-fouling performance, which is different from Example 1 in that heptafluorobutylamine is replaced by pentafluoropropylamine molecules.

[0048] Example 5

[0049] A polyamide reverse osmosis membrane having both high flux and excellent pollution resistance, which is different from Example 1 in that the heptafluorobutylamine molecule is replaced by nonafluoropentylamine.

[0050] Example 6

[0051] A polyamide reverse osmosis membrane having both high flux and excellent pollution resistance, which is different from Example 1 in that the heptafluorobutylamine molecule is replaced by undecafluorohexylamine.

[0052] Example 7

[0053] A polyamide reverse osmosis membrane having both high flux and excellent pollution resistance, which is different from Example 1 in that the heptafluorobutylamine molecule is replaced by perfluoroheptylamine.

[0054] Example 8

[0055] A polyamide reverse osmosis membrane having both high flux and excellent anti-fouling performance, which is different from Example 1 in that the thermal crosslinking condition is changed to 80° C. thermal crosslinking for 5 minutes.

[0056] Example 9

[0057] A polyamide reverse osmosis membrane having both high flux and excellent pollution resistance, which is different from Example 1 in that the solvent n-hexane in the organic solution for preparing trimesoyl chloride is replaced by isoparaffin Isopar G.

[0058] Example 10

[0059] A polyamide reverse osmosis membrane having both high flux and excellent anti-fouling performance, which is different from Example 1 in that the polysulfone bottom membrane as the porous ultrafiltration base membrane is replaced by a polyvinylidene fluoride membrane.

[0060] Comparative Example 1

[0061] A polyamide reverse osmosis membrane with both high flux and excellent pollution resistance is prepared by the following steps:

[0062] S1, dissolving m-phenylenediamine in water to prepare a 2 wt.% m-phenylenediamine aqueous solution to obtain an aqueous monomer solution; immersing one side of a porous ultrafiltration base membrane in the polyamine monomer solution for 2 minutes, and removing excess aqueous monomer solution on the surface of the ultrafiltration base membrane using a rubber roller or an air knife;

[0063] S2, dissolving trimesoyl chloride in n-hexane to prepare a 0.1wt.% trimesoyl chloride organic solution, stirring and mixing to obtain an oil phase monomer solution; applying the oil phase monomer solution evenly to the surface of the carrier coated with the aqueous phase monomer solution obtained in step S1 for 1 minute to form a thin layer of composite polyamide film;

[0064] S3, placing the thin layer composite polyamide membrane obtained in step S2 in a forced air drying oven at 60° C. for thermal crosslinking for 10 minutes, and finally obtaining a polyamide reverse osmosis membrane.

[0065] Evaluation and measurement methods

[0066] Determination of modification rate

[0067] The modification rate of the modified polyamide film is defined as: the number of acyl chlorides reacted with the nitrogen-containing compound relative to the number of all acyl chlorides remaining after the cross-linking reaction of MPD and TMC. Specifically, the modification rate of heptafluorobutylamine of the modified polyamide film is calculated by the following formula based on the photoelectron spectrum obtained by X-ray photoelectron spectroscopy (XPS). The results are shown in Table 1.

[0068] Based on the modification of heptaflubutamine, the modification rate (%) is calculated as follows:

[0069]

[0070] Wherein, a represents the peak area of ​​C*-F; b represents the peak area of ​​O=C*; c represents the peak area of ​​CO*-H; d represents the peak area of ​​C=O*.

[0071] As shown in Table 1, the modification rate of the RO membrane by molecules with different degrees of fluorination is 27.3-40.4%. As the degree of fluorination in the grafted molecular structure increases, the modification rate of the grafted molecule on the RO membrane shows an overall decreasing trend. At the same time, as the degree of fluorination in the grafted molecular structure increases, the reduction of the surface free energy of the RO membrane shows a decreasing trend. In summary, while maintaining a high modification rate, selecting grafted molecules with a higher degree of fluorination is conducive to further improving the anti-fouling performance of the RO membrane.

[0072] Table 1: Modification rate of fluorinated molecules on the surface of polyamide reverse osmosis membrane

[0073] name Modification rate (%) Example 1 38.9 Example 2 27.3 Example 3 41.6 Example 4 40.4 Example 5 35.5 Example 6 32.8 Example 7 30.1 Example 8 35.0 Example 9 39.0 Example 10 31.2

[0074] Membrane surface properties:

[0075] The solid surface zeta potential analyzer was used to characterize the potential change on the surface of the polyamide reverse osmosis membrane. According to the test, the polyamide reverse osmosis membrane prepared in Examples 1 to 10 maintained a surface zeta potential of -31 mV to 15 mV during the pH change from 3 to 10, showing a weak electronegativity.

[0076] like Figure 1Part a is a comparison of the surface Zeta potential curves of the polyamide reverse osmosis membranes prepared in Example 1 of the present invention and Comparative Example 1; it can be seen from the figure that the surface potential of the polyamide reverse osmosis membrane of Example 1 changes from -30.8mV to 14.7mV during the pH change from 3 to 10, while the surface Zeta potential of the traditional polyamide membrane prepared in Comparative Example 1 changes from -48.4mV to 6.9mV during the pH change from 3 to 10. It can be concluded that compared with Comparative Example 1, the surface electronegativity of the RO membrane obtained in Example 1 is greatly weakened, which is conducive to the improvement of the pollution resistance of the RO membrane to positively charged pollutants.

[0077] A water contact angle meter was used to characterize the surface free energy change of the polyamide reverse osmosis membrane. After testing, the surface free energy of the polyamide reverse osmosis membrane prepared in Examples 1 to 10 was 33 mJ·m -2 ~51mJ·m -2 between them, showing lower free energy.

[0078] like Figure 1 Part b shows a comparison of the surface free energy of the polyamide reverse osmosis membranes prepared in Example 1 of the present invention and in Comparative Example 1; it can be clearly seen from the figure that the surface free energy of the conventional polyamide reverse osmosis membrane is 61 mJ·m -2 The surface free energy of the polyamide reverse osmosis membrane prepared in Example 1 is 50 mJ·m -2 Compared with Comparative Example 1, Example 1 regulates the membrane surface properties by introducing molecules containing fluorine-based chains. The fluorine-based chains in the fluorine-containing molecules grafted to the surface of the polyamide membrane can effectively reduce the free energy of the membrane surface, thereby reducing the accumulation of pollutants on the membrane surface, and making it easier for pollutants to desorb from the membrane surface, thereby improving the pollution resistance of the polyamide reverse osmosis membrane.

[0079] In summary, the polyamide reverse osmosis membrane prepared in the present application achieves an increase in the Zeta potential of the membrane surface and a significant reduction in the free energy of the membrane surface, thereby improving the pollution resistance of the polyamide reverse osmosis membrane to charged pollutants.

[0080] Membrane separation performance test:

[0081] For the composite reverse osmosis membrane, a reverse osmosis cross-flow test system (effective membrane surface area: 28.26 cm 2), measure the permeate flux (Flux) and salt retention rate (Rej). Initially, operate at a pressure of 20 bar for 2 hours to stabilize the permeability of the composite reverse osmosis membrane. Next, use a supply aqueous solution containing NaCl at a concentration of 2000 mg / L, operate at a pressure of 15 bar for 1 hour, and then measure the permeate flux of the composite reverse osmosis membrane (collect the permeate for 30 minutes). The permeate flux is calculated using the following formula (1). In addition, a conductivity meter (Thermo, Eutech CON2700, USA) is used to measure the concentrations of the supply solution and the permeate. The salt retention rate is calculated using the following formula (2). Repeat the test 3 times and take the average data as the final result. The results are shown in Table 2.

[0082]

[0083] J: Permeate flux (LMH / bar)

[0084] V: Volume of permeate (L)

[0085] A: Effective membrane area of ​​composite reverse osmosis membrane (28.26cm 2 )

[0086] Δt: penetration time (h)

[0087] ΔP: Osmotic pressure (bar)

[0088]

[0089] R: Salt retention rate (%)

[0090] C f :Concentration of supply solution (mg / L)

[0091] C p :Permeate concentration (mg / L)

[0092] Table 2: Selective permeability performance of polyamide reverse osmosis membrane

[0093]

[0094] From the test results in Table 2, we can see that:

[0095] Compared with the polyamide reverse osmosis membrane prepared in Comparative Example 1, the polyamide reverse osmosis membranes prepared in Examples 1 to 10 are used as reverse osmosis membranes. Under the premise of maintaining a high salt rejection rate, the water permeability coefficient is greatly improved. Specifically, compared with the water permeability coefficient of 2.3LMH / bar in Comparative Example 1, the water permeability coefficients of Examples 1 to 10 are increased to 4.0LMH / bar to 4.8LMH / bar.

[0096] Membrane anti-fouling performance test:

[0097] As model pollutants, DTAB (dodecyl trimethyl ammonium bromide), SDS (sodium dodecyl sulfate) and BSA (bovine serum albumin) are used. DTAB is used as an example of a surfactant with a positive charge, i.e., a small molecule pollutant. SDS is used as an example of a surfactant with a negative charge. BSA is used as an example of a macromolecular organic pollutant with a negative charge, and these are typical representative examples of common organic pollutants in water systems.

[0098] The anti-fouling performance was evaluated by the Flux maintenance rate (%). The Flux maintenance rate was measured in the following four stages.

[0099] In stage 1, the RO system was operated at 15 bar and a cross flow velocity of 14 cm / s for 30 minutes using a feed aqueous solution containing 2000 mg / L NaCl to determine baseline permeate flux and salt retention.

[0100] In the second stage, 200 ppm of the model pollutant was added to the feed aqueous solution, and the RO system was operated for 6 hours under the same conditions as in the first stage.

[0101] In the third stage, the composite reverse osmosis membrane was cleaned with deionized water at a circulation flow rate of 3 L / min for 30 minutes.

[0102] In the fourth stage, the permeate flux was measured using a feed aqueous solution containing 2000 mg / L NaCl.

[0103] Then, the Flux maintenance rate was calculated by the following formula. The results are shown in Table 3.

[0104] Flux maintenance rate (%) = (permeation flux of the fourth stage / permeation flux of the first stage) × 100% Table 3: Anti-fouling performance of polyamide reverse osmosis membrane

[0105]

[0106] From the test results in Table 3, it can be seen that the permeation flux and the selective permeation performance before and after the pollution resistance test of the polyamide reverse osmosis membrane prepared in the examples of the present application are better than those of the polyamide reverse osmosis membrane of the comparative example. It can be seen that the polyamide reverse osmosis modified by aliphatic fluoride exhibits excellent pollution resistance to both positively charged and negatively charged organic pollutants.

[0107] Industrially available lines

[0108] The polyamide reverse osmosis membrane of the present invention is suitable for the manufacture of ultrapure water, desalination of salt water or seawater, etc., and can remove and recover the pollution sources or effective substances contained in the pollutants such as dyeing wastewater and electrodeposition coating wastewater as the cause of public pollution, and contribute to the sealing of wastewater. In addition, it can be used for high-level treatment such as concentration of effective ingredients in food applications, removal of harmful ingredients in water purification and sewage applications, etc. In addition, it can be used for wastewater treatment in oil fields, shale gas fields, etc.

Claims

1. A polyamide reverse osmosis membrane having both high flux and pollution resistance, characterized in that: The polyamide reverse osmosis membrane comprises a porous ultrafiltration base membrane and a polyamide dense functional layer; wherein the polyamide dense functional layer is prepared on the surface of the porous ultrafiltration base membrane by interfacial polymerization of polyamine monomers and polyacyl chloride monomers; the surface free energy of the polyamide functional layer is less than 51 mJ m -2 The surface charge at pH = 7 is -10eV to -32eV; the pure water permeability coefficient of the polyamide functional layer is >4L m -2 h -1 bar -1 The flux attenuation rate of the feed solution of 200ppm dodecylammonium bromide is <55%, the flux attenuation rate of the feed solution of 200ppm sodium dodecyl sulfate is <30%, and the flux attenuation rate of the feed solution of 200ppm bovine serum albumin is <20%.

2. The polyamide reverse osmosis membrane having both high flux and pollution resistance as claimed in claim 1, characterized in that: The porous ultrafiltration base membrane includes but is not limited to polymer ultrafiltration membrane and inorganic ultrafiltration membrane with a pore size range of 10nm to 100nm; the polymer ultrafiltration membrane is cellulose acetate membrane, polyethersulfone membrane, polyvinylidene fluoride membrane, polysulfone membrane or polyacrylonitrile membrane; the inorganic ultrafiltration membrane is inorganic alumina.

3. The polyamide reverse osmosis membrane having both high flux and pollution resistance according to claim 1, characterized in that: The polyamine monomers used include but are not limited to at least one of m-phenylenediamine, p-phenylenediamine, o-phenylenediamine, 1,3,5-triaminobenzene, 1,2,4-triaminobenzene, 3,5-diaminobenzoic acid, 2,4-diaminotoluene, 2,6-diaminotoluene, N,N-dimethylm-phenylenediamine, 2,4-diaminoanisole, and phenylenediamine; the aliphatic polyamine monomers include but are not limited to at least one of ethylenediamine, propylenediamine, tris(2-aminoethyl)amine, and N-phenylethylenediamine; the alicyclic polyamine monomers include but are not limited to at least one of 1,3-diaminocyclohexane, 1,2-diaminocyclohexane, and 1,4-diaminocyclohexane.

4. The polyamide reverse osmosis membrane having both high flux and pollution resistance according to claim 1, characterized in that: The polyacyl chlorides used include but are not limited to aromatic polyacyl chlorides, aliphatic polyacyl chlorides, and alicyclic polyacyl chlorides; wherein the aromatic polyacyl chlorides include but are not limited to at least one of trimesoyl chloride, terephthaloyl chloride, isophthaloyl chloride, biphenyl dicarboxylic acid chloride, naphthalene dicarboxylic acid chloride, benzene trisulfonyl chloride, benzene disulfonyl chloride, and chlorosulfonyl phthaloyl chloride; the aliphatic polyacyl chlorides include but are not limited to at least one of propanyl chloride, butanyl chloride, glutaryl chloride, propanyl tricarboxylic acid chloride, butanyl tricarboxylic acid chloride, glutaryl tricarboxylic acid chloride, and glutaryl chloride; the alicyclic polyacyl chlorides include but are not limited to at least one of cyclopropane tricarboxylic acid chloride, cyclobutane tetracarboxylic acid chloride, cyclopentane tricarboxylic acid chloride, cyclopentane tetracarboxylic acid chloride, cyclohexane tricarboxylic acid chloride, tetrahydrofuran tetracarboxylic acid chloride, cyclopentane dicarboxylic acid chloride, cyclobutane dicarboxylic acid chloride, cyclohexane dicarboxylic acid chloride, and tetrahydrofuran dicarboxylic acid chloride.

5. A method for preparing a polyamide reverse osmosis membrane having both high flux and pollution resistance as claimed in any one of claims 1 to 4, characterized in that: The steps include: S1. Immerse one side of the porous ultrafiltration base membrane in the polyamine monomer for 0.5 min to 10 min, and use a rubber roller or an air knife to remove excess aqueous monomer solution on the surface of the ultrafiltration base membrane; S2, uniformly applying the organic solution of polyacid chloride to the surface of the carrier coated with the aqueous monomer solution obtained in step S1 for 0.5 min to 10 min to form a thin layer of composite polyamide film; S3, uniformly applying the modified solution containing fluorine molecules to the surface of the thin layer composite polyamide membrane obtained in step S2 for 0.5 min to 3 min to generate a modified thin layer composite polyamide membrane; S4, placing the modified thin-layer composite polyamide membrane obtained in step S3 at 50° C. to 160° C. for thermal crosslinking for 3 min to 15 min, and finally obtaining a polyamide reverse osmosis membrane.

6. The method for preparing a polyamide reverse osmosis membrane having both high flux and pollution resistance according to claim 5, characterized in that: Aliphatic fluorides are composed of amino and fluorine groups and have the following chemical structure: Among them, 2 <n<8。 7. A method for preparing a polyamide reverse osmosis membrane having both high flux and pollution resistance according to claim 6, characterized in that: The aliphatic fluoride includes but is not limited to at least one of pentafluoropropylamine, heptafluorobutylamine, nonafluoropentylamine, undecafluorohexylamine and perfluoroheptylamine.

8. The method for preparing a polyamide reverse osmosis membrane with high flux and pollution resistance according to claim 6 is characterized in that the aqueous monomer solution used in step S1 is 0.1wt.% to 10wt.% of a polyamine monomer; the polyacyl chloride organic solution used in step S2 is 0.01wt.% to 5wt.% of a polyacyl chloride organic solution, and the organic solvent includes but is not limited to at least one of n-hexane, isoalkane, n-nonane, and n-decane; the modified solution of fluorine-containing molecules used in step S3 is 0.2wt.% to 10wt.% of a modified solution.

9. An application of a polyamide reverse osmosis membrane having both high flux and anti-fouling properties as claimed in any one of claims 1 to 4, characterized in that: Polyamide reverse osmosis membrane is used as reverse osmosis membrane in seawater desalination and sewage treatment.

Citation Information

Cited By

  • Preparation method of boron-removed seawater desalination reverse osmosis membrane and reverse osmosis membrane prepared by same

    CN120771733A

  • A polyolefin-based reverse osmosis membrane and a method for preparing the same

    CN122999004A