Sealing solution for anodized aluminum alloy films
By using thickened polysaccharides in the sealing treatment liquid of the aluminum alloy anodized film, the problems of free nickel salt, corrosion resistance and high sealing performance are solved, and excellent pollution resistance and dye fixation are achieved, avoiding The toxicity of nickel salts.
Patent Information
- Application Number
- CN201980068025.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2019-09-13
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2039-09-13
AI Technical Summary
In the prior art, it is difficult to achieve free nickel salt, corrosion resistance and high pore sealing properties during the sealing process, and there are problems of nickel allergies and toxicity of micro-powder nickel salts.
Using a sealing treatment solution containing thickened polysaccharides, select polysaccharides, beans, seaweeds, microbial fermentation products and other polysaccharides as main components, it forms excellent pollution resistance, dye fixability and dyeing appearance, and replaces traditional nickel. Salt sealing treatment.
The same sealing performance as the nickel salt sealing treatment solution is achieved, and the nickel salt-free treatment solution can provide excellent pollution resistance and dye fixation, avoiding the toxicity problem of nickel salt.
Smart Images

Figure BDA0003021630140000221
Abstract
Description
Technical Field
[0001] The invention relates to a sealing treatment liquid for anodized films of aluminum alloys. Background Art
[0002] For the anodic oxide film of aluminum alloy, a sealing treatment is usually performed in order to prevent pollution, improve corrosion resistance, etc. As the sealing treatment method, boiling water sealing, steam sealing, room temperature sealing, nickel acetate sealing using nickel acetate aqueous solution for sealing treatment, etc. are known.
[0003] Among them, nickel acetate sealing is particularly used because it is easier to obtain corrosion resistance of the film than boiling water sealing, has better operating efficiency than steam sealing, and is easier to manage liquids than normal temperature sealing. However, nickel allergy and the toxicity of fine powder nickel salts have become problems. Therefore, as a sealing treatment method that does not use nickel salts when manufacturing anodized films, it is necessary to exert the same degree of corrosion resistance, sealing degree and other sealing performance as nickel acetate sealing.
[0004] Patent Document 1 is a technology of the present applicant, which is a sealing treatment liquid for anodized film of aluminum alloy containing an alkali metal salt, a pH buffer and a surfactant. When the sealing treatment liquid is used, the anodized film of the aluminum alloy can be given the same degree of sealing performance as when a sealing treatment liquid containing a nickel salt is used, and can also be given excellent pollution resistance.
[0005] Patent Document 2 describes a method for sealing the pores of anodized aluminum surfaces using activated inorganic or organic substances or free and ionized coordination compounds by irradiating with light irradiation energy. 3 COO 2 and NiSO 4 The result when used as a sealing agent.
[0006] Patent Document 3 describes that a hydrophilic film (anodized film) can be formed on an aluminum substrate and then subjected to a pore sealing treatment. This technology describes only an example of using a sodium silicate aqueous solution as a pore sealing treatment using particles.
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: International Publication No. WO2017 / 170370A1
[0010] Patent Document 2: Japanese Patent Publication No. 61-027476 (Japanese Patent Publication No. 54-104463)
[0011] Patent Document 3: Japanese Patent Application Laid-Open No. 2003-034090 Summary of the invention
[0012] Technical problem to be solved by the invention
[0013] The present invention has been made in view of the above-mentioned problems of the prior art, and an object of the present invention is to provide a new sealing treatment liquid for anodized films of aluminum alloys.
[0014] An object of the present invention is to impart good sealing performance to an anodic oxide film of an aluminum alloy by adding a thickening polysaccharide to a sealing treatment liquid.
[0015] Technical solutions for solving technical problems
[0016] The inventors of the present invention have conducted intensive studies to achieve the above-mentioned object and have found that the above-mentioned object can be achieved by using a sealing treatment liquid for anodized film of aluminum alloy containing a thickening polysaccharide, thereby completing the present invention.
[0017] When the sealing treatment liquid of the present invention is used, even if it does not contain nickel salt, it can also impart the same degree of sealing performance as when using the sealing treatment liquid containing nickel salt. When the sealing treatment liquid of the present invention is used, the anodized film after the sealing treatment can show excellent stain resistance, dye fixation and excellent dyeing appearance.
[0018] That is, the present invention relates to the following sealing treatment liquid and sealing treatment method for an anodic oxide film of an aluminum alloy.
[0019] Item 1. A sealing treatment liquid for an anodic oxide film of an aluminum alloy, characterized in that it contains a thickening polysaccharide.
[0020] Item 2. The sealing solution according to Item 1 above, wherein the thickening polysaccharide is at least one selected from the following components:
[0021] polysaccharides present in tree sap;
[0022] Polysaccharides present in the seeds of legumes;
[0023] Polysaccharides present in seaweed;
[0024] Polysaccharides present in fruits, leaves and underground stems;
[0025] fermentation products of microorganisms; and
[0026] An ingredient selected from the group consisting of oligoglucosamine, methylcellulose, carboxymethylcellulose, carboxymethylcellulose calcium, carboxymethylcellulose sodium, microfibrous cellulose, chitin, chitosan, glucosamine, sodium starch glycolate, gluten, gluten decomposition products and mannan.
[0027] Item 3. The sealing solution according to Item 1 above, wherein the thickening polysaccharide is a polysaccharide present in tree sap, and is at least one selected from the group consisting of gum arabic, arabinogalactan, gum karaya, gum ghatti, and gum tragacanth.
[0028] Item 4. The sealing treatment liquid according to Item 1 above, wherein the thickening polysaccharide is a polysaccharide present in the seeds of beans, and is at least one selected from flaxseed gum, cassia gum, carob gum (locust bean gum), guar gum, psyllium seed gum, wormwood seed gum, tamarind gum, tara gum, sesbania gum and soybean polysaccharides.
[0029] Item 5. The sealing treatment liquid according to Item 1 above, wherein the thickening polysaccharide is a polysaccharide present in seaweed, and is at least one selected from alginic acid, ammonium alginate, potassium alginate, calcium alginate, sodium alginate, propylene glycol alginate, carrageenan, agar, Colpomenia sinuosa extract, furcellan, seaweed cellulose and brown algae extract.
[0030] Item 6. The sealing treatment liquid according to Item 1 above, wherein the thickening polysaccharide is a polysaccharide present in fruits, leaves, and underground stems, and is at least one selected from Aloe vera extract, Aloe arborescens extract, pectin, okra extract, konjac extract, and sweet potato cellulose.
[0031] Item 7. The sealing treatment liquid according to Item 1 above, wherein the thickening polysaccharide is a fermentation product of microorganisms, and is at least one selected from Aeromonas gum, Agrobacterium succinoglycan, Brunei gum, curdlan gum, xanthan gum, gellan gum, sclerotium gum, dextran, pullulan, Macrophomopsis gum and rhamnan gum.
[0032] Item 8. The sealing treatment liquid according to Item 1 above, wherein the thickening polysaccharide is at least one selected from oligosaccharides, methylcellulose, carboxymethylcellulose, carboxymethylcellulose calcium, sodium carboxymethylcellulose, microfibrous cellulose, chitin, chitosan, glucosamine, sodium starch glycolate, gluten, gluten decomposition products and mannan.
[0033] Item 9. The sealing solution according to any one of Items 1 to 8, wherein the content of the thickening polysaccharide in the sealing solution is 0.1 g / L to 50 g / L.
[0034] Item 10. The sealing solution according to any one of Items 1 to 9, wherein the pH is 2.0 to 9.0.
[0035] Item 11. The sealing solution according to any one of Items 1 to 10, which contains no nickel compound.
[0036] Item 12. A sealing treatment method, which is a sealing treatment method for an anodized film of an aluminum alloy, characterized in that it has a process of using the sealing treatment liquid described in any one of Items 1 to 11 to immerse an article having an anodized film of an aluminum alloy in the sealing treatment liquid for the anodized film of the aluminum alloy.
[0037] Item 13. The sealing method according to Item 12 above, wherein the sealing solution has a temperature of 80°C to 98°C.
[0038] Item 14. An article which has been sealed by the sealing method according to Item 12 or 13.
[0039] Item 15. A dye fixing treatment liquid, which is a dye fixing treatment liquid for an anodic oxide film of an aluminum alloy, characterized in that the anodic oxide film of the aluminum alloy is a film that has been subjected to a dyeing treatment, and the dye fixing treatment liquid contains a thickening polysaccharide.
[0040] Effects of the Invention
[0041] The sealing treatment liquid of the present invention contains a thickening polysaccharide, and when the sealing treatment liquid is used, a good sealing performance can be imparted to the anodic oxide film of the aluminum alloy.
[0042] The sealing treatment liquid of the present invention can provide sealing performance equivalent to that of a case where a sealing treatment liquid containing a nickel salt is used.
[0043] The sealing treatment liquid of the present invention can impart excellent stain resistance, dye fixation and excellent dyed appearance to the anodic oxidation film of the aluminum alloy. DETAILED DESCRIPTION
[0044] Hereinafter, the present invention will be described in detail.
[0045] 1. Sealing liquid
[0046] The sealing solution of the present invention is a sealing solution for an anodic oxide film of an aluminum alloy (hereinafter also referred to as "sealing solution"), and is characterized by containing a thickening polysaccharide.
[0047] When the sealing treatment liquid of the present invention is used, even if it does not contain nickel salt, it can also give the anodized film of the aluminum alloy the same degree of sealing performance as when using the sealing treatment liquid containing nickel salt. The sealing treatment liquid of the present invention can give the anodized film of the aluminum alloy excellent stain resistance, dye fixation and excellent dyeing appearance.
[0048] (1) Thickening polysaccharides
[0049] The sealing solution of the present invention is characterized by containing a thickening polysaccharide.
[0050] In the sealing treatment liquid of the present invention, the thickening polysaccharide is preferably at least one selected from the following components:
[0051] polysaccharides present in tree sap;
[0052] Polysaccharides present in the seeds of legumes;
[0053] Polysaccharides present in seaweed;
[0054] Polysaccharides present in fruits, leaves and underground stems;
[0055] fermentation products of microorganisms; and
[0056] An ingredient selected from the group consisting of oligoglucosamine, methylcellulose, carboxymethylcellulose, carboxymethylcellulose calcium, carboxymethylcellulose sodium, microfibrous cellulose, chitin, chitosan, glucosamine, sodium starch glycolate, gluten, gluten decomposition products and mannan.
[0057] In the sealing solution of the present invention, the thickening polysaccharide is preferably a polysaccharide present in tree sap, and is at least one selected from the group consisting of gum arabic, arabinogalactan, karaya gum, ghatti gum, and tragacanth gum.
[0058] In the sealing treatment liquid of the present invention, the above-mentioned thickening polysaccharide is preferably a polysaccharide present in the seeds of beans, and is at least one selected from linseed gum, cassia gum, carob gum (locust bean gum), guar gum, psyllium seed gum, artemisia seed gum, tamarind gum, tara gum, sesbania gum and soybean polysaccharides.
[0059] In the sealing treatment liquid of the present invention, the above-mentioned thickening polysaccharide is preferably a polysaccharide present in seaweed, which is at least one selected from alginic acid, ammonium alginate, potassium alginate, calcium alginate, sodium alginate, propylene glycol alginate, carrageenan, agar, cystine extract, red seaweed gel, seaweed cellulose and brown seaweed extract.
[0060] In the sealing treatment liquid of the present invention, the above-mentioned thickening polysaccharide is preferably a polysaccharide present in fruits, leaves, and underground stems, and is at least one selected from Aloe vera extract, Aloe arborescens extract, pectin, okra extract, konjac extract and sweet potato cellulose.
[0061] In the sealing treatment liquid of the present invention, the above-mentioned thickening polysaccharide is preferably a fermentation product of microorganisms, and is at least one selected from Aeromonas gum, Agrobacterium succinoglycan, Brunei gum, curdlan gum, xanthan gum, gellan gum, sclerotium gum, dextran, pullulan, Macrostella gum and rhamnan gum.
[0062] In the sealing treatment liquid of the present invention, the above-mentioned thickening polysaccharide is preferably at least one selected from oligosaccharides, methylcellulose, carboxymethylcellulose, carboxymethylcellulose calcium, sodium carboxymethylcellulose, microfibrous cellulose, chitin, chitosan, glucosamine, sodium starch glycolate, gluten, gluten decomposition products and mannan.
[0063] In the sealing solution of the present invention, the thickening polysaccharide may be used alone or in combination of two or more.
[0064] In the sealing solution of the present invention, the content of the thickening polysaccharide in the sealing solution is preferably 0.1 g / L to 50 g / L. In the sealing solution of the present invention, the content of the thickening polysaccharide in the sealing solution is more preferably about 0.5 g / L to 25 g / L, and further preferably about 1 g / L to 10 g / L.
[0065] The sealing treatment liquid of the present invention contains a thickening polysaccharide, and when the sealing treatment liquid is used, it can impart good sealing performance to the anodic oxidation film of the aluminum alloy. The sealing treatment liquid of the present invention can impart good sealing performance to the same degree as when a sealing treatment liquid containing a nickel salt is used. The sealing treatment liquid of the present invention can impart excellent stain resistance, dye fixation and excellent dyeing appearance to the anodic oxidation film of the aluminum alloy.
[0066] (2) pH adjuster
[0067] The sealing treatment liquid of the present invention may contain a pH adjuster as needed in order to improve the sealing performance and anti-fouling property and to improve the usability of the liquid.
[0068] In the sealing treatment liquid of the present invention, the pH adjuster is not particularly limited, and a conventionally known pH adjuster can be used.
[0069] In the sealing treatment liquid of the present invention, as a pH adjuster for adjusting the sealing treatment liquid to the acidic side, acetic acid, aminosulfonic acid, sulfuric acid, nitric acid, organic sulfonic acid, etc., or diluted aqueous solutions thereof are preferably used. Among them, acetic acid or diluted aqueous solutions thereof are preferably used in view of excellent sealing performance.
[0070] In the sealing treatment liquid of the present invention, as a pH adjuster for adjusting the sealing treatment liquid to the alkaline side, preferably used is ammonia water, sodium hydroxide aqueous solution, potassium hydroxide aqueous solution, etc. Among them, sodium hydroxide aqueous solution is preferably used in view of excellent sealing performance.
[0071] In the sealing solution of the present invention, the pH adjuster may be used alone or in combination of two or more.
[0072] In the sealing treatment liquid of the present invention, the concentration of the pH adjuster in the sealing treatment liquid can be any concentration as long as it can adjust the pH of the liquid, and is preferably about 0.1g / L to 20g / L, more preferably about 0.2g / L to 10g / L, and further preferably about 0.3g / L to 5g / L.
[0073] The sealing solution of the present invention contains a pH adjuster, so that the sealing solution can exhibit sufficient sealing performance and can suppress a decrease in the sealing degree of the anodized film sealed with the sealing solution.
[0074] (3) Other ingredients
[0075] The sealing treatment liquid of the present invention may contain additives as needed in order to improve the sealing performance and anti-fouling property and to improve the usability of the liquid.
[0076] Examples of additives include antifungal agents such as benzoic acid and benzoate salts, complexing agents such as citric acid and citric acid salts, etc. As the antifungal agent, a commercially available antifungal agent such as "TAC KABIKORON" (manufactured by Okuno Pharmaceutical Co., Ltd.) can be added.
[0077] The sealing liquid of the present invention may contain a pH buffer, a metal salt, etc., as required, in order to improve the sealing performance and contamination resistance and to improve the usability of the liquid.
[0078] (4) pH of the sealing solution
[0079] The pH of the sealing treatment liquid of the present invention is preferably 2.0 to 9.0, more preferably about 3.0 to 7.0, and even more preferably about 4.5 to 6.5.
[0080] The sealing treatment liquid of the present invention has a pH value of 2.0 to 9.0, and exhibits sufficient sealing performance. The anodized film of the aluminum alloy sealed with the sealing treatment liquid fully exhibits pollution resistance, dye fixation and excellent dyeing appearance, and can suppress the poor appearance (floating powder, fogging) of powdery attachments attached to the surface of the treated object.
[0081] (5) Ingredients that are not included
[0082] The sealing solution of the present invention preferably does not contain a nickel-based metal salt, or substantially does not contain a nickel-based metal salt. Examples of metal salts such as nickel-based metal salts include metal salts of Ni, Co, and the like.
[0083] In recent years, nickel allergy and the toxicity of fine powder nickel salts have become problems. Therefore, for the sealing treatment liquid, it is expected to use a sealing treatment method that does not use nickel-based metal salts to produce an anodized film with the same degree of corrosion resistance, sealing degree and other sealing properties as nickel acetate sealing.
[0084] The sealing treatment liquid of the present invention preferably does not contain fluorine compounds or fluorine ions, or substantially does not contain them. As ion sources of fluorine ions, fluorine compounds such as hydrogen fluoride, ammonium fluoride, acidic ammonium fluoride, potassium fluoride, acidic potassium fluoride, sodium fluoride, acidic sodium fluoride, cobalt fluoride, ammonium fluorozirconate, and boron fluoride can be cited.
[0085] Since excessive dissolution of aluminum alloy and anodized film caused by fluorine leads to a decrease in dye fixation or dyeing appearance, it is expected to produce anodized films with sealing properties such as corrosion resistance and sealing degree by a sealing treatment method that does not use fluorine compounds or fluoride ions.
[0086] The sealing solution of the present invention preferably contains no heavy metal or substantially no heavy metal. Examples of the heavy metal include heavy metals such as chromium and manganese.
[0087] When the sealing treatment liquid contains heavy metals, the surface of the article treated with the sealing treatment liquid may be attached with heavy metals, such as chromium, which may be harmful to the human body. In addition, in recent years, environmental restrictions on wastewater from treatment liquids have been promoted, and there are concerns about increased manufacturing costs or reduced operability. Therefore, it is expected that an anodic oxide film with sealing properties such as corrosion resistance and sealing degree can be manufactured by a sealing treatment method that does not use heavy metals.
[0088] 2. Sealing treatment method
[0089] The sealing treatment method of the present invention is a sealing treatment method for an anodic oxide film of an aluminum alloy, characterized in that it has a step of using the above-mentioned sealing treatment liquid containing the above-mentioned thickening polysaccharide and immersing an article having an anodic oxide film of an aluminum alloy in the sealing treatment liquid.
[0090] The impregnation method is not particularly limited, and the impregnation may be carried out by a conventionally known method.
[0091] The sealing treatment liquid of the present invention contains a thickening polysaccharide. When the sealing treatment liquid is used to seal the anodic oxide film of the aluminum alloy, the anodic oxide film of the aluminum alloy can be given good sealing performance. The sealing treatment method of the present invention can well give the same degree of sealing performance as when using a sealing treatment liquid containing a nickel salt. The sealing treatment method of the present invention can give the anodic oxide film of the aluminum alloy excellent stain resistance, dye fixation and excellent dyeing appearance.
[0092] In the sealing method of the present invention, the pH of the sealing solution is preferably 2.0 to 9.0. In the sealing method of the present invention, the liquid temperature (bath temperature) of the sealing solution is preferably 80°C to 98°C.
[0093] (1) Liquid temperature of sealing treatment liquid
[0094] In the sealing method of the present invention, in the immersion step, the sealing solution temperature (bath temperature) is preferably about 80 to 98° C., more preferably about 92 to 98° C., and even more preferably about 95 to 98° C.
[0095] In the sealing treatment method, sufficient sealing performance can be exhibited by adjusting the temperature of the sealing treatment liquid.
[0096] (2) pH of the sealing solution
[0097] In the sealing method of the present invention, the pH of the sealing solution is preferably 2.0 to 9.0. In the sealing method of the present invention, the pH of the sealing solution is more preferably about 3.0 to 7.0, and even more preferably about 4.5 to 6.5.
[0098] In the sealing method, by adjusting the pH of the sealing solution, the sealing solution can exhibit sufficient sealing performance and can suppress appearance defects (floating powder, fogging) caused by powdery deposits on the surface of the treated object.
[0099] (3) Sealing time
[0100] The sealing treatment time can be generally determined according to the film thickness of the anodized film to be treated. The sealing treatment time is generally preferably adjusted within a time range of about 3 minutes to 1 hour.
[0101] For example, it is preferred that the value (μm) representing the film thickness of the anodic oxide film to be treated be multiplied by 0.1 to 10 to obtain the sealing treatment time (minutes). It is further preferred that the value (μm) representing the film thickness be multiplied by 0.2 to 5 to obtain the sealing treatment time (minutes), and it is further preferred that the value (μm) representing the film thickness be multiplied by 0.5 to 4 to obtain the sealing treatment time (minutes).
[0102] For example, if the thickness of the anodized film is 10 μm, the immersion time is preferably 10 times 0.2 to 5, that is, about 2 to 50 minutes.
[0103] In the sealing treatment method, by adjusting the sealing treatment time, the sealing treatment liquid can exhibit sufficient sealing performance, and the anodized film of the aluminum alloy sealed with the sealing treatment liquid can fully exhibit pollution resistance, and can inhibit the deterioration of the appearance of the treated object caused by poor appearance such as floating powder and fogging.
[0104] (4) Sealing method
[0105] In the sealing treatment method of the present invention, an article having an anodic oxide film of an aluminum alloy is used as a treated object, and the treated object is immersed in a sealing treatment solution. The article having an anodic oxide film of an aluminum alloy can be subjected to electrolytic coloring, dyeing, etc. as needed, and then fully washed with water, and the treated object is immersed in a sealing treatment solution. Thus, the sealing performance of the anodic oxide film of the aluminum alloy to be treated can be greatly improved.
[0106] In the impregnation process of the sealing treatment method of the present invention, the sealing treatment liquid can be stirred while the article having the anodic oxide film of the aluminum alloy is impregnated. As the stirring method, circulation stirring, air stirring, gas stirring, shaking stirring, etc. are suitable. Among the stirring methods, circulation stirring and gas stirring are preferred, and circulation stirring is more preferred. As the gas stirring, gas stirring using an inactive gas such as nitrogen and argon is suitable.
[0107] In the sealing treatment method of the present invention, circulation stirring is preferred as the stirring method. When air stirring is required on the equipment, gas stirring using an inert gas is preferred from the viewpoint of suppressing turbidity of the sealing treatment liquid.
[0108] The sealing treatment method of the present invention can perform a turbidity removal treatment to remove turbidity in the sealing treatment solution in the process of immersing an article having an anodic oxide film of an aluminum alloy in a sealing treatment solution for an anodic oxide film of an aluminum alloy. In addition, the turbidity removal treatment can be performed in the above-mentioned process, for example, in the idle time before immersing the article in the sealing treatment solution for an anodic oxide film, or when the production line is suspended. By performing the turbidity removal treatment, the appearance degradation of the anodic oxide film caused by poor appearance such as floating powder and fogging due to turbidity can be suppressed.
[0109] In the sealing treatment method of the present invention, there is no particular limitation on the method for removing turbidity, and a conventionally known removal method can be used. As a removal method, filtration removal is suitable. Specifically, part of the sealing treatment liquid is allowed to flow from the tank for sealing treatment into a preparatory tank such as a buffer tank serving as a drug supply and dissolution tank, and the temperature of the sealing treatment liquid is preferably cooled to below 50°C, filtered through a filter, and then returned to the above-mentioned tank for sealing treatment to circulate it, thereby filtering and removing it. In the case where there is no buffer tank in the equipment, filtration removal can be performed by a simple filtration cycle.
[0110] 3. Dye fixation solution
[0111] The present invention can also prepare the above-mentioned sealing treatment liquid containing thickening polysaccharide into a dye fixing treatment liquid. That is, the dye fixing treatment liquid of the present invention can use the above-mentioned " 1. Sealing liquid "
[0112] The dye fixing treatment liquid of the present invention contains a thickening polysaccharide, and when the dye fixing treatment liquid is used, the dye fixing property can be well imparted to the anodic oxidation film of the aluminum alloy, and the sealing property can be imparted.
[0113] pH of dye fixation solution
[0114] The pH of the dye fixing treatment liquid of the present invention is preferably 2.0 to 6.0. The pH of the dye fixing treatment liquid is more preferably about 2.5 to 5.0, and even more preferably about 3.0 to 4.5.
[0115] The dye fixing treatment liquid of the present invention has a pH of 2.0 to 6.0, and when the dye fixing treatment liquid is used, it can provide good dye fixing properties to the anodic oxide film of the aluminum alloy and can provide sealing performance. The pH of the dye fixing treatment liquid of the present invention is preferably adjusted slightly to the acidic side from the perspective of being able to provide good dye fixing properties compared to the above-mentioned sealing treatment liquid.
[0116] 4. Dye fixation treatment method
[0117] In the present invention, an article (an article subjected to dyeing treatment) in which the anodic oxide film of the aluminum alloy of the present invention is dyed with a dye can be used as a treatment object. As a dyeing method using a dye, a method of immersing the anodic oxide film in a conventionally known dye aqueous solution is preferably adopted.
[0118] The present invention is also useful as a dye fixing treatment method by using the dye fixing treatment solution (sealing treatment solution) of the present invention. In the dye fixing treatment method of the present invention, an aluminum alloy (or an article containing an aluminum alloy) is subjected to (1) an anodic oxidation treatment (forming an anodic oxidation film), (2) a dyeing treatment, (3) a dye fixing treatment, and (4) a sealing treatment in sequence.
[0119] The dye fixing and pore sealing method of the present invention is a dye fixing and pore sealing method for aluminum alloy, which is characterized by:
[0120] (1) A step of forming an anodic oxide film on an aluminum alloy;
[0121] (2) a step of dyeing the anodized film;
[0122] (3) a step of immersing the anodized film subjected to the dyeing treatment in a dye fixing treatment solution to perform a dye fixing treatment; and
[0123] (4) A step of immersing the anodized film subjected to the dye fixing treatment in a sealing treatment liquid to perform a sealing treatment.
[0124] The dye fixing and sealing methods of the present invention can impart excellent dye fixing properties to an anodic oxide film of an aluminum alloy or an article having an anodic oxide film of an aluminum alloy.
[0125] In the dye fixing and sealing methods of the present invention, the above-mentioned " 2. Sealing method Law "
[0126] (1) Anodizing
[0127] The object to be treated with dye fixing treatment and sealing treatment is an anodic oxide film of aluminum alloy or an article having an anodic oxide film of aluminum alloy. The article having an anodic oxide film of aluminum alloy can be used as the object to be treated and immersed in the dye fixing treatment solution and the sealing treatment solution.
[0128] (2) Dyeing treatment
[0129] The dyeing treatment is preferably performed at 10°C to 70°C.
[0130] As the dye, it is preferable to use a dye commercially available as a dye for anodized aluminum alloy films, and for example, an anionic dye is preferably used.
[0131] The temperature of the aqueous dye solution is preferably about 10° C. to 70° C., more preferably 20° C. to 60° C. The concentration of the dye in the aqueous dye solution and the immersion time may be appropriately set depending on the desired color tone and color concentration.
[0132] When an article in which an anodic oxide film of an aluminum alloy is dyed with a dye is used as a treatment object, it is preferable to perform a dye fixing treatment after dyeing and before sealing treatment in order to impart dye fixability by a sealing treatment liquid.
[0133] (3) Dye fixation treatment
[0134] The present invention can prepare the above-mentioned sealing treatment liquid containing thickening polysaccharide into a dye fixing treatment liquid. That is, the dye fixing treatment liquid of the present invention can use the above-mentioned " 1. Sealing liquid "
[0135] The dye fixing treatment liquid of the present invention contains a thickening polysaccharide, and when the dye fixing treatment liquid is used, the dye fixing property can be well imparted to the anodic oxidation film of the aluminum alloy, and the sealing property can be imparted.
[0136] By adjusting the types and blending of the pH buffer and surfactant in the sealing solution, it is also possible to impart dye fixability using the sealing solution.
[0137] The process of performing the dye fixing treatment and the process of performing the sealing treatment of the following process (4) can be one treatment, that is, can be performed as one treatment. In the present invention, the sealing treatment liquid of the present invention can be used as the dye fixing treatment liquid to perform the dye fixing treatment, and then the sealing treatment liquid for the anodized film of the aluminum alloy of the present invention is used to perform the sealing treatment. At this time, the dye fixing treatment and the sealing treatment can also be prepared into the same treatment liquid and performed as one treatment.
[0138] Alternatively, the dye fixing treatment and the sealing treatment may be performed as separate treatments. In the present invention, the dye fixing treatment solution of the present invention used for the dye fixing treatment and the sealing treatment solution for the anodized film of the aluminum alloy of the present invention used for the sealing treatment may be prepared in different (compositions) and performed as separate treatments.
[0139] In the present invention, when the sealing treatment liquid of the present invention is used for the sealing treatment, the dye fixing treatment can use a commonly available dye fixing liquid. For example, as the dye fixing treatment agent, it is preferred to use a commercially available product for the aluminum alloy anodized film dyeing process (for example, TAC Fixing Agent-2, TAC Sunblock 77-5C, etc. produced by Okuno Pharmaceutical Industry Co., Ltd.).
[0140] In the present invention, when the sealing treatment liquid of the present invention is used as a dye fixing treatment liquid to carry out dye fixing treatment, a commonly available sealing treatment liquid can be used for the sealing treatment.
[0141] For example, as the sealing agent, a commercially available product for use in the aluminum alloy anodized film dyeing process (for example, TOP SEAL NIF and TOP NF SEAL S-205 manufactured by Okuno Chemical Industry Co., Ltd.) is preferably used.
[0142] Liquid temperature for dye fixation
[0143] In the step of immersing the dyed anodized film in a dye fixing treatment solution for dye fixing treatment, the liquid temperature (bath temperature) of the dye fixing treatment solution is preferably about 80° C. to 98° C. The liquid temperature (bath temperature) of the sealing treatment solution is more preferably about 92° C. to 98° C., and further preferably about 95° C. to 98° C.
[0144] In the dye fixing treatment method, by adjusting the temperature of the dye fixing treatment solution, it is possible to impart good dye fixing property to the anodic oxide film of the aluminum alloy and also to impart sealing performance.
[0145] pH of dye fixation solution
[0146] The pH of the dye fixing treatment liquid of the present invention is 2.0 to 6.0. Therefore, when the dye fixing treatment liquid is used, the dye fixing property can be well imparted to the anodic oxide film of the aluminum alloy, and the sealing property can be imparted.
[0147] Dye fixation time
[0148] The dye fixing treatment time can be generally determined according to the film thickness of the anodic oxide film to be treated. The dye fixing treatment time is generally preferably adjusted within a time range of about 3 minutes to 60 minutes.
[0149] It is possible to impart good dye fixation properties to the anodic oxide film of the aluminum alloy and to impart sealing properties.
[0150] (4) Sealing treatment
[0151] Sealing treatment in the above (3) Dye fixation treatment After that, you can use the above " 2. Sealing treatment method "
[0152] 5. Concentrate
[0153] The present invention can also prepare the above-mentioned sealing treatment liquid containing thickening polysaccharide and dye fixing treatment liquid into concentrated liquid.
[0154] The present invention makes the sealing treatment liquid containing thickening polysaccharide and the dye fixing treatment liquid into a concentrated solution with high concentration of each component contained therein, so that transportation and storage become easy. In the present invention, the sealing treatment liquid containing thickening polysaccharide and the dye fixing treatment liquid can be easily prepared by diluting the concentrated solution with a diluent such as water. As the diluent, water is preferably used.
[0155] The concentrated solution of the present invention may contain the same components as the above-mentioned sealing treatment solution containing thickening polysaccharide and dye fixing treatment solution, and the contents of these components may be different. In order to use the concentrated solution of the present invention to prepare the above-mentioned sealing treatment solution containing thickening polysaccharide and dye fixing treatment solution of the present invention, the contents of these components in the concentrated solution can be adjusted.
[0156] The components contained in the concentrate of the present invention may be the same as the thickening polysaccharide contained in the sealing solution and dye fixing solution of the present invention. The concentrate may also be prepared based on the sealing solution and dye fixing solution of the present invention.
[0157] 6. Items that have been treated with dye fixation and sealing
[0158] The present invention is an article which has been sealed using the above-mentioned sealing method.
[0159] The present invention is an article which has been subjected to a dye fixing treatment using the above-mentioned dye fixing treatment method and a pore sealing treatment using the above-mentioned pore sealing treatment method.
[0160] The object to be subjected to the dye fixing treatment and the sealing treatment is an anodic oxide film of an aluminum alloy or an article having an anodic oxide film of an aluminum alloy.
[0161] The anodic oxide film of the aluminum alloy is not particularly limited, and a known anodic oxidation method using sulfuric acid, oxalic acid, phosphoric acid, or the like for general aluminum alloys can be suitably used, and an anodic oxide film of the aluminum alloy obtained by such an anodic oxidation method is preferably used.
[0162] The aluminum alloy is not particularly limited, and various aluminum alloys can be used as the object of anodization. As the aluminum alloy, it is preferable to use various aluminum alloy groups represented by JIS-A 1000 to 7000 specified in JIS, cast materials shown in each number section of AC and ADC, and die-cast materials.
[0163] As an anodic oxidation method for aluminum alloy, it is preferable to use, for example, an aqueous solution with a sulfuric acid concentration of about 100 g / L to 400 g / L, set the liquid temperature to about -10°C to 30°C, and apply 0.5 to 4 A / dm 2 A method of performing electrolysis at an anode current density of about 200 Å.
[0164] In the sealing treatment method of the present invention, an article in which an anodic oxide film of an aluminum alloy is electrolytically colored can be the treatment object.
[0165] As the electrolytic coloring method, the method of known coloring technology can be adopted. For example, after anodizing, it can be immersed in an electrolytic coloring bath, and secondary electrolysis is performed, thereby the anodic oxide film is colored. As the electrolytic coloring bath, it is preferred to use a nickel salt-boric acid bath, a nickel salt-tin salt-sulfuric acid bath, etc.
[0166] Example
[0167] The present invention will be described in detail below with reference to Examples and Comparative Examples, but the present invention is not limited to the Examples.
[0168] Anodized aluminum alloy test pieces used in the following examples and comparative examples were prepared under the following production conditions.
[0169] 1. Preparation of anodized test pieces
[0170] (1) Preparation of anodized test piece A
[0171] (With dyeing treatment)
[0172] (1-1) Degreasing treatment
[0173] The aluminum test piece was immersed in a weak alkaline degreasing liquid for 3 minutes for degreasing. The aluminum test piece was a JIS A1050P plate. The weak alkaline degreasing liquid was a 30 g / L aqueous solution of TOP ALCLEAN 101 (trade name) manufactured by Okuno Chemical Industry Co., Ltd. The bath temperature for the degreasing was set at 60°C.
[0174] (1-2) Anodizing
[0175] Next, the sample was washed with water and anodized in an anodizing bath containing sulfuric acid as the main component. The anodizing bath contained 180 g / L of free sulfuric acid and 8 g / L of dissolved aluminum. The anodizing conditions were bath temperature: 20±1°C, anode current density: 1 A / dm 2 , electrolysis time: 30 minutes. An anodic oxide film with a film thickness of about 10 μm was produced. The obtained anodic oxide film was washed with water.
[0176] (1-3) Dyeing treatment
[0177] Next, the sample was immersed in a dyeing treatment liquid at 50° C. for 1 minute, and then washed with water to perform a dyeing treatment. The dyeing treatment liquid was a 1 g / L solution of TAC dye TAC YELLOW 203 manufactured by Okuno Chemical Industry Co., Ltd.
[0178] This is referred to as "anodized test piece A".
[0179] (2) Preparation of anodized test piece B
[0180] (No dyeing)
[0181] (2-1) Degreasing treatment
[0182] The aluminum test piece was immersed in a weak alkaline degreasing liquid for 3 minutes for degreasing. The aluminum test piece was a JIS A1050P plate. The weak alkaline degreasing liquid was a 30 g / L aqueous solution of TOP ALCLEAN 101 (trade name) manufactured by Okuno Chemical Industry Co., Ltd. The bath temperature for the degreasing was set at 60°C.
[0183] (2-2) Anodizing
[0184] Next, the sample was washed with water and anodized in an anodizing bath containing sulfuric acid as the main component. The anodizing bath contained 180 g / L of free sulfuric acid and 8 g / L of dissolved aluminum. The anodizing conditions were bath temperature: 20±1°C, anode current density: 1 A / dm 2 , Electrolysis time: 30 minutes. An anodic oxide film with a film thickness of about 10 μm was produced. The obtained anodic oxide film was washed with water to obtain an anodic-oxidized aluminum alloy test piece.
[0185] This is referred to as "anodized test piece B".
[0186] 2. Dye fixation and sealing treatment
[0187] (1) Examples 1 to 7
[0188] This is an example in which a sealing treatment has been performed.
[0189] The thickening polysaccharide was blended in the composition shown in Table 1 to prepare the sealing treatment liquid of each example.
[0190] In Example 1, an aqueous solution containing 5 g / L of gum arabic and adjusted to pH = 5.5 was prepared, and the anodized test piece A was immersed in the sealing treatment solution for 30 minutes to perform the sealing treatment.
[0191] The bath temperature of the sealing treatment liquid was 95°C.
[0192] In Examples 2 to 7, as thickening polysaccharides, guar gum (Example 2), propylene glycol alginate (PGA) (Example 3), sodium alginate (SA) (Example 4), pectin (Example 5), gellan gum (Example 6) and carboxymethyl cellulose (CMC) (Example 7) are contained, and the sealing treatment liquid is prepared in the same manner as in Example 1.
[0193] Here, since the anodized test piece A was subjected to a dyeing treatment, the sealing treatment liquid used can be regarded as a dye fixing treatment liquid, and the sealing treatment can be regarded as a dye fixing treatment.
[0194] (2) Examples 8 to 16
[0195] This is an example in which dye fixing treatment and pore sealing treatment were performed.
[0196] Dye fixation treatment
[0197] Thickening polysaccharides were blended in the compositions shown in Table 1 to prepare dye fixing treatment solutions of the respective Examples.
[0198] In Examples 8 and 16, an aqueous solution containing 5 g / L of gum arabic and adjusted to pH = 4.0 was prepared, and the anodized test piece A was immersed in the dye fixing treatment solution for 5 minutes to perform the dye fixing treatment.
[0199] The bath temperature of the dye fixing treatment solution was 95°C.
[0200] In Examples 9 to 14, as thickening polysaccharides, guar gum (Example 9), propylene glycol alginate (PGA) (Example 10), sodium alginate (SA) (Example 11), pectin (Example 12), gellan gum (Example 13) and carboxymethyl cellulose (CMC) (Example 14) are contained, and a dye fixing treatment liquid is prepared in the same manner as in Example 8.
[0201] In Example 15, TAC Fixing Agent-2 manufactured by Okuno Chemical Industries, Ltd. was used as a dye fixing agent.
[0202] Sealing treatment
[0203] The thickening polysaccharide was blended in the composition shown in Table 1 to prepare the sealing treatment liquid of each example.
[0204] In Examples 8 and 15, an aqueous solution containing 5 g / L of gum arabic and adjusted to pH = 5.5 was prepared, and the anodized test piece A was immersed in the sealing treatment solution for 30 minutes to perform the sealing treatment.
[0205] The bath temperature of the sealing treatment liquid was 95°C.
[0206] In Examples 9 to 14, as thickening polysaccharides, guar gum (Example 9), propylene glycol alginate (PGA) (Example 10), sodium alginate (SA) (Example 11), pectin (Example 12), gellan gum (Example 13) and carboxymethyl cellulose (CMC) (Example 14) are contained, and the sealing treatment liquid is prepared in the same manner as in Example 1.
[0207] In Example 16, TOP NF SEAL S-205 manufactured by Okuno Chemical Industries, Ltd. was used as a sealing agent.
[0208] The anodized test piece A was subjected to dyeing treatment, dye fixing treatment using a dye fixing treatment liquid, and then sealing treatment using a sealing treatment liquid.
[0209] (3) Examples 17 and 18
[0210] The sealing treatment liquid contained 1 g / L (Example 17) or 10 g / L (Example 18) of gum arabic as a thickening polysaccharide, and the sealing treatment liquid was prepared in the same manner as in Example 1. The sealing treatment was carried out in the same manner as in Example 1.
[0211] (4) Examples 19 and 20
[0212] The dye fixing treatment liquid contained 1 g / L (Example 19) or 10 g / L (Example 20) of gum arabic as a thickening polysaccharide, and a dye fixing treatment liquid was prepared in the same manner as in Example 8. The dye fixing treatment and sealing treatment were carried out in the same manner as in Example 8.
[0213] (5) Examples 21 and 22
[0214] The pH of the sealing treatment liquid was adjusted to pH=3.5 (Example 21) or pH=6.5 (Example 22), and the sealing treatment liquid was prepared in the same manner as in Example 1. The sealing treatment was carried out in the same manner as in Example 1.
[0215] (6) Embodiment 23
[0216] In the sealing treatment, the bath temperature of the sealing treatment liquid was adjusted to 80° C., and the sealing treatment was performed in the same manner as in Example 1.
[0217] (7) Embodiment 24
[0218] In the sealing treatment, the anodized test piece B (without dyeing treatment) was immersed in the sealing treatment liquid for sealing treatment, and the sealing treatment was performed in the same manner as in Example 1.
[0219] (8) Embodiment 25
[0220] In the dye fixing treatment and sealing treatment, the anodized test piece B (no dyeing treatment) is immersed in the dye fixing treatment liquid and the sealing treatment liquid for dye fixing treatment and sealing treatment, and the dye fixing treatment and sealing treatment are performed in the same manner as in Example 8.
[0221] (9) Comparative Examples 1 and 2
[0222] In Comparative Example 1, the anodized test piece A was immersed in boiling water sealing (ion exchange water) at 95° C. (bath temperature) for 30 minutes (immersion time) to perform a sealing treatment.
[0223] In Comparative Example 2, the anodized test piece A was immersed in a sealing treatment liquid (bath temperature 95° C.) consisting of an aqueous solution containing 40 mL / L of a nickel acetate-based sealing agent (TOP SEAL H-298 (trade name) manufactured by Okuno Chemical Industries, Ltd.) and having a pH of 5.5, for sealing treatment.
[0224] (10) Dye fixation and sealing treatment
[0225] In the examples and comparative examples, each anodized test piece was immediately rinsed with tap water for 1 minute after the dye fixing treatment and the pore sealing treatment were performed. Then, the anodized test piece was dried in a dryer and left overnight at room temperature to prepare an anodized test piece after the dye fixing treatment and the pore sealing treatment.
[0226] 3. Evaluation test
[0227] The anodized test pieces after the sealing treatment prepared in Examples were evaluated by the following test methods.
[0228] (1) Sealing degree
[0229] According to JIS H 8683-2:1999 (Test method for sealing degree of anodic oxide films of aluminum and aluminum alloys Part 2: Phosphoric acid-chromic acid aqueous solution immersion test), each test piece after sealing treatment was immersed in phosphoric acid-chromic acid aqueous solution and the mass reduction per unit area of the test piece was measured.
[0230] Evaluation was performed according to the following evaluation criteria.
[0231] ◎: Weight reduction: 10.0 mg / dm 2 the following.
[0232] ○: Weight reduction: 15.0 mg / dm 2 the following.
[0233] △: Weight reduction is 20.0mg / dm2 the following.
[0234] ×: Weight reduction is 20.0 mg / dm 2 above.
[0235] If it is evaluated as ○ in the evaluation, it can be evaluated that there is no problem in actual use.
[0236] (2)Pollution resistance
[0237] (Magic test: test for removing attached stains)
[0238] After the sealing treatment, each test piece was left at room temperature for 1 day, and a mark was made on the surface with an oil-based black marker, and the surface was left to stand for 30 seconds. Then, the surface was wiped with a box tissue soaked with water.
[0239] Evaluation was performed according to the following evaluation criteria.
[0240] ◎: The mark can be completely removed.
[0241] ○: The mark can be removed, but some traces remain.
[0242] △: Only a part of the mark could be removed.
[0243] ×: The black color of the mark cannot be removed.
[0244] If it is evaluated as ○ in the evaluation, it can be evaluated that there is no problem in actual use.
[0245] (3) Dye fixation
[0246] The color tones (L*, a*, b*) of the anodized test pieces after dyeing and sealing were measured, and the color difference (ΔE*ab) was calculated from these values. The L*, a*, and b* values were measured using a spectrophotometer CA-3700A (manufactured by Konica Minolta, Inc.).
[0247] The base color is used as the color tone after dyeing (L* 1 , a* 1 , b* 1 ), and the comparison color is used as the color tone after sealing treatment (L* 2 , a* 2 , b* 2 ), the color difference is calculated as follows.
[0248]
[0249] Evaluation was performed according to the following evaluation criteria.
[0250] ◎: ΔE*ab is 1.0 or less.
[0251] ○: ΔE*ab is 3.0 or less.
[0252] Δ: ΔE*ab is 5.0 or less.
[0253] ×: ΔE*ab is 5.0 or more.
[0254] If it is evaluated as ○ in the evaluation, it can be evaluated that there is no problem in actual use.
[0255] (4) Appearance evaluation
[0256] The surface of the anodized test piece after the sealing treatment was visually observed for powdering, fogging, or interference film rainbow caused by these.
[0257] Evaluation was performed according to the following evaluation criteria.
[0258] ◎: No powdering, fogging, or interference film rainbow caused by these occurred, and the appearance was good.
[0259] ○: Powdering, fogging, or interference film rainbow caused by these slightly occurred, but the appearance was not problematic.
[0260] △: Powdering, fogging, or interference film rainbow caused by these occurred, resulting in a slight appearance defect.
[0261] ×: Powder floating, fogging, or interference film rainbow caused by these seriously occurred, resulting in serious appearance defects.
[0262] The results are shown in Tables 1 and 2.
[0263] (5) Abbreviations in Table 1
[0264] PGA: Propylene glycol alginate
[0265] SA: Sodium Alginate
[0266] CMC: Carboxymethyl cellulose
[0267] [Table 1]
[0268]
[0269] [Table 2]
[0270] Table 2 Test piece Processing Sealing degree Pollution resistance Dye fixation Appearance Example 1 A Sealing ○ ◎ ○ ◎ Example 2 A Sealing ○ ◎ ○ ◎ Example 3 A Sealing ○ ◎ ○ ◎ Example 4 A Sealing ○ ◎ ○ ○ Example 5 A Sealing ○ ◎ ○ ◎ Example 6 A Sealing ○ ◎ ○ ◎ Example 7 A Sealing ○ ◎ ○ ◎ Example 8 A Fixing → Sealing ◎ ◎ ◎ ◎ Example 9 A Fixing → Sealing ◎ ◎ ◎ ◎ Example 10 A Fixing → Sealing ◎ ◎ ◎ ◎ Embodiment 11 A Fixing → Sealing ◎ ◎ ◎ ○ Example 12 A Fixing → Sealing ◎ ◎ ◎ ◎ Embodiment 13 A Fixing → Sealing ◎ ◎ ◎ ◎ Embodiment 14 A Fixing → Sealing ◎ ◎ ◎ ◎ Embodiment 15 A Fixing → Sealing ◎ ◎ ◎ ○ Example 16 A Fixing → Sealing ◎ ◎ ◎ ◎ Embodiment 17 A Sealing ○ ◎ ○ ◎ Embodiment 18 A Sealing ○ ◎ ○ ◎ Embodiment 19 A Fixing → Sealing ◎ ◎ ◎ ◎ Embodiment 20 A Fixing → Sealing ◎ ◎ ◎ ◎ Embodiment 21 A Sealing ○ ◎ ○ ◎ Embodiment 22 A Sealing ○ ◎ ○ ◎ Embodiment 23 A Sealing ○ ◎ ○ ◎ Embodiment 24 B Sealing ○ ◎ - ◎ Embodiment 25 B Fixing → Sealing ◎ ◎ - ◎ Comparative Example 1 A Sealing × × × × Comparative Example 2 A Sealing ◎ ◎ ○ ◎
[0271] As can be seen from Tables 1 and 2, the sealing treatment liquid (Example) of the present invention can impart good sealing performance to the anodic oxide film of the aluminum alloy by adding a thickening polysaccharide. The sealing treatment liquid of the present invention can impart good sealing performance to the same degree as when using a sealing treatment liquid containing a nickel salt. The sealing treatment liquid of the present invention can impart excellent stain resistance, dye fixation and excellent dyeing appearance to the anodic oxide film of the aluminum alloy.
[0272] As shown in Tables 1 and 2, the sealing treatment solution (Example) of the present invention can impart excellent dye fixation to the anodic oxidation film of the aluminum alloy and can impart good sealing performance by adding a thickening polysaccharide. It can be seen that the sealing treatment solution of the present invention is also useful as a dye fixing treatment solution.
Claims
1. A method for dye fixing and pore sealing treatment, which is a method for dye fixing and pore sealing treatment of aluminum alloy, characterized in that: have: (1) A step of forming an anodic oxide film on an aluminum alloy; (2) a step of dyeing the anodized film; (3) a step of immersing the anodized film subjected to the dyeing treatment in a dye fixing treatment solution to perform a dye fixing treatment; and (4) a step of immersing the anodized film subjected to the dye fixing treatment in a sealing treatment solution to perform a sealing treatment, The dye fixing treatment liquid and the sealing treatment liquid contain thickening polysaccharides, The content of the thickening polysaccharide in the dye fixing treatment liquid and the sealing treatment liquid is 5 g / L to 50 g / L, In the step (3) of performing the dye fixing treatment, the pH of the dye fixing treatment liquid is 2.0 to 4.
0. In the step (4) of performing the sealing treatment, the pH of the sealing treatment liquid is 4.5 to 9.
0.
2. The method according to claim 1, characterized in that The thickening polysaccharide is at least one selected from the following substances: polysaccharides present in tree sap; Polysaccharides present in the seeds of legumes; Polysaccharides present in seaweed; Polysaccharides present in fruits, leaves and underground stems; fermentation products of microorganisms; and The ingredient is selected from the group consisting of oligoglucosamine, methylcellulose, carboxymethylcellulose, carboxymethylcellulose calcium, carboxymethylcellulose sodium, microfibrous cellulose, chitin, chitosan, sodium starch glycolate and mannan.
3. The method according to claim 1 or 2, characterized in that: The dyeing step (2) is performed at 10°C to 70°C.
4. The method according to claim 1 or 2, characterized in that: In the step (3) of performing the dye fixing treatment, the liquid temperature of the dye fixing treatment liquid is 80°C to 98°C, and in the step (4) of performing the sealing treatment, the liquid temperature of the sealing treatment liquid is 80°C to 98°C.
Citation Information
Patent Citations
Surface treating method for aluminum
JP1979104463A
Surface treating method for aluminum
JP1986027476B2
Lithographic printing original plate
JP2003034090A
Preparation method of anti-corrosion and anti-aging sealing agent
CN109796856A
Lithographic printing original plate
JP2003034091A