Catalyst for simultaneously catalyzing CO and NOx as well as preparation method and application of catalyst
By using combinations of copper, cerium, lanthanum and other elements in catalyst preparation, the anti-poisoning ability and service life of the catalyst are improved, and the problems of low efficiency and short life of existing catalysts in steel smelting processes are solved.
Patent Information
- Application Number
- CN202411122106.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
It is difficult for existing catalysts to effectively catalyze CO and NOx in steel smelting processes, and there are problems such as insufficient water and sulfur resistance and short service life.
Using a preparation method, including dropping the alkaline solution to the slurry of the active ingredient precursor and the carrier precursor to form a precipitate, then mixing with additives and thickeners, molding after extrusion or coating, drying and calcining, Catalysts for elements such as copper, cerium, and lanthanum are prepared, and the combination of these elements is used to improve catalytic performance and anti-poisoning ability.
It improves the conversion rate of the catalyst to CO and NOx, enhances the resistance to sulfur and water poisoning, and extends the service life of the catalyst.
Smart Images

Figure BDA0004995381310000131
Abstract
Description
Technical Field
[0001] The present invention relates to a method for simultaneously catalyzing CO and NO x Catalyst and preparation method and use thereof. Background Art
[0002] In the steel smelting process, the flue gas emitted during the sintering process is a kind of industrial waste gas with a large volume, concentrated pollutants and high concentrations. The sintering flue gas contains a large number of atmospheric pollutants, mainly CO, NO x , SO2, etc. SO2 contained in sintering flue gas can easily poison the catalyst, causing it to lose oxidation efficiency and greatly damage its service life. Water vapor, other pollutants and heavy metals in sintering flue gas can also easily adhere to the surface of the catalyst, reducing its performance.
[0003] CN118059845A discloses a method for preparing a catalyst for catalytic oxidation of CO, comprising the following steps: S1: providing a catalyst precursor loaded with copper oxide; S2: mixing the catalyst precursor loaded with copper oxide with a first impregnation solution containing a cerium source, and drying to obtain a catalyst precursor; S3: drying and first calcining the catalyst precursor to obtain a catalyst for catalytic oxidation of CO. The catalyst comprises a titanium dioxide carrier and copper oxide and cerium oxide loaded on the titanium dioxide, wherein the mass of the cerium oxide is 0.5-25% of the mass of the titanium dioxide carrier in terms of cerium element. The water and sulfur resistance of the catalyst needs to be improved.
[0004] CN117427655A discloses a method for preparing a denitration catalyst, comprising the following steps: Step 1: reacting a manganese source, an iron source, and an M source with an alkali solution, filtering, washing, and drying to obtain S1; Step 2: fully mixing S1, titanium dioxide, a binder, polyethylene oxide, glass fiber, and deionized water in a kneading mechanism to obtain S2; Step 3: fully kneading S2, bisphenol A, dicyandiamide, and 2-ethyl-4-methylimidazole, extruding to obtain S3, and then drying and calcining S3 to obtain a denitration catalyst. The water and sulfur resistance of the catalyst needs to be improved.
[0005] CN118384896A discloses a method for preparing an efficient low-temperature carbon monoxide removal catalyst, comprising the following steps: dispersing gas phase titanium dioxide P25 powder into anhydrous ethanol, adding glacial acetic acid and tetrabutyl titanate under stirring to obtain pretreated titanium dioxide. Adding graphene oxide and copper nitrate into an ethanol aqueous solution and stirring evenly, adding them dropwise into the pretreated titanium dioxide under stirring, stirring at 60-80°C for 10-30 minutes, adjusting the system pH to 11-12, continuing stirring, centrifuging, filtering, washing, and obtaining loaded titanium dioxide. The loaded titanium dioxide is added to the sodium hydroxide solution and mixed evenly, and the solvent is reacted at 150-160°C, and the solid-liquid separation is performed, and the solid is washed, and then added to water to obtain a doped titanium dioxide suspension; manganese nitrate and cerium nitrate are added to the water and stirred evenly, and the doped titanium dioxide suspension is added dropwise under stirring conditions, and stirred until the precipitation is completely precipitated, and then allowed to stand for 1-5 hours, and the solid-liquid separation is performed, and the solid is washed until neutral, dried, roasted and granulated, and sieved to obtain a low-temperature carbon monoxide removal catalyst. The service life of the catalyst is relatively short. Summary of the invention
[0006] In view of this, an object of the present invention is to provide a method for preparing a catalyst, which can improve the catalyst's x The catalyst has a high sulfur and water poisoning resistance. Furthermore, the catalyst has a long service life. Another object of the present invention is to provide a catalyst for simultaneously catalyzing CO and NO x A further object of the present invention is to provide a use of a catalyst.
[0007] The above purpose is achieved through the following technical solutions.
[0008] In one aspect, the present invention provides a method for simultaneously catalyzing CO and NO x The method for preparing a catalyst comprises the following steps:
[0009] (1) adding an alkaline solution dropwise to a first slurry comprising 60 to 95 parts by weight of an active ingredient precursor and 100 to 150 parts by weight of a carrier precursor to obtain a second slurry; aging the second slurry, filtering, and obtaining a precipitate;
[0010] (2) mixing the precipitate with 45 to 75 parts by weight of an additive, 25 to 60 parts by weight of a thickener and water to obtain a slurry;
[0011] (3) Extruding the clay material to obtain a molded clay material;
[0012] (4) drying and calcining the formed clay to obtain a catalyst;
[0013] Or include the following steps:
[0014] (A) adding a basic solution dropwise to a first slurry comprising 120 to 185 parts by weight of an active ingredient precursor and 30 to 70 parts by weight of a carrier precursor to obtain a second slurry;
[0015] (B) adding 40 to 60 parts by weight of an additive and 10 to 50 parts by weight of a thickener to the second slurry to obtain a third slurry;
[0016] (C) coating the third slurry on a glass fiber corrugated board carrier to obtain a loaded carrier;
[0017] (D) drying and calcining the supported carrier to obtain a catalyst;
[0018] Wherein, the active ingredient precursor is selected from one or more of a copper precursor, a cerium precursor, a lanthanum precursor, and a tungsten precursor;
[0019] The carrier precursor is selected from one or more of titanium dioxide, aluminum oxide, and cordierite;
[0020] The additive is selected from one or more of pseudo-boehmite, kaolin, polyvinyl alcohol, and hydroxymethyl cellulose;
[0021] The thickener is selected from one or more of silica sol, xanthan gum and alumina sol;
[0022] The alkaline solution is selected from one or more of aqueous ammonia, ammonium carbonate solution and ammonium bicarbonate solution.
[0023] According to the preparation method of the present invention, preferably, the active ingredient precursor is selected from one of the following:
[0024] (I) 40 to 60 parts by weight of a copper precursor and 20 to 40 parts by weight of a cerium precursor;
[0025] (II) 70 to 90 parts by weight of a copper precursor, 50 to 70 parts by weight of a lanthanum precursor, and 10 to 30 parts by weight of a tungsten precursor.
[0026] According to the preparation method of the present invention, preferably, the carrier precursor is selected from one of the following:
[0027] (I) 40 to 60 parts by weight of titanium dioxide and 70 to 90 parts by weight of aluminum oxide;
[0028] (II) 10 to 30 parts by weight of titanium dioxide and 20 to 40 parts by weight of cordierite.
[0029] According to the preparation method of the present invention, preferably, the additive is selected from one of the following:
[0030] (I) 5 to 20 parts by weight of pseudo-boehmite and 40 to 60 parts by weight of kaolin;
[0031] (II) 10 to 30 parts by weight of polyvinyl alcohol and 20 to 40 parts by weight of hydroxymethyl cellulose.
[0032] According to the preparation method of the present invention, preferably, the thickener is selected from one of the following:
[0033] (I) silica sol;
[0034] (II) 5 to 20 parts by weight of xanthan gum and 10 to 30 parts by weight of aluminum sol.
[0035] According to the preparation method of the present invention, preferably, the concentration of the alkaline solution is 0.05-0.8 mol / L, the volume mass ratio of the alkaline solution to the active ingredient precursor is (1-9): 1 L / g, and the rate of dripping the alkaline solution into the first slurry is 100-500 mL / h.
[0036] According to the preparation method of the present invention, preferably, the drying temperature is 90-150° C., and the drying time is 5-30 hours; the calcination temperature is 400-600° C., and the calcination time is 1-8 hours.
[0037] In another aspect, the present invention provides a method for simultaneously catalyzing CO and NO x A catalyst obtained by the above preparation method.
[0038] In another aspect, the present invention provides the above catalyst for simultaneously catalyzing CO and NO x Uses in.
[0039] According to the use of the present invention, preferably, CO and NO x Exists in gaseous substances, CO concentration is 4000~8000ppm, NO x The concentration is 500-1000ppm; the gaseous substance also contains 100-500ppm SO2 and 10-40vol% water vapor.
[0040] The catalyst obtained by the method of the present invention has a high affinity for CO and NO x The catalyst prepared by the method of the present invention has a high sulfur and water poisoning resistance. Furthermore, the catalyst prepared by the method of the present invention has a long service life. DETAILED DESCRIPTION
[0041] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0042] <Method for preparing catalyst>
[0043] The catalyst of the present invention can be prepared by extrusion molding or coating molding.
[0044] The extrusion molding method mainly includes the following steps: (1) a step of forming a precipitate; (2) a step of obtaining a mud material; (3) a step of molding; and (4) a step of drying and roasting.
[0045] Steps to form a precipitate
[0046] An alkaline solution is added dropwise to a first slurry comprising an active ingredient precursor and a carrier precursor to obtain a second slurry; the second slurry is aged and then filtered to obtain a precipitate.
[0047] The first slurry also includes water. Water can be added to the mixture including the active ingredient precursor and the carrier precursor after uniform mixing, and stirred for 1 to 5 hours; preferably 2 to 3 hours to obtain the first slurry. The amount of water used can be 300 to 700 parts by weight; preferably 400 to 600 parts by weight; more preferably 500 to 550 parts by weight.
[0048] The amount of the active ingredient precursor may be 60 to 95 parts by weight, preferably 70 to 90 parts by weight, and more preferably 80 to 85 parts by weight.
[0049] The amount of the carrier precursor may be 100 to 150 parts by weight, preferably 110 to 140 parts by weight, and more preferably 120 to 130 parts by weight.
[0050] The aging temperature may be 40 to 70° C., preferably 50 to 60° C. The aging time may be 2 to 10 hours, preferably 5 to 8 hours.
[0051] The method may further include drying the precipitate to obtain a dried precipitate. The drying may be performed in an oven. The drying temperature may be 40 to 80° C., preferably 50 to 70° C., and more preferably 60 to 65° C. The drying time may be 15 to 30 hours, preferably 17 to 26 hours, and more preferably 20 to 24 hours.
[0052] Steps to get the clay
[0053] The precipitate is mixed with an additive, a thickener and water to obtain a slurry. The precipitate may be a dried precipitate.
[0054] The amount of the additive can be 45 to 75 parts by weight, preferably 50 to 70 parts by weight, and more preferably 60 to 65 parts by weight.
[0055] The amount of the thickener may be 25 to 60 parts by weight, preferably 30 to 50 parts by weight, and more preferably 40 to 45 parts by weight.
[0056] The amount of water used may be 180 to 300 parts by weight, preferably 200 to 280 parts by weight, and more preferably 240 to 260 parts by weight.
[0057] Forming steps
[0058] The clay material is extruded to obtain a molded clay material. The clay material can be extruded and molded by an extruder. The shape of the molded clay material is not limited, for example, it can be a cylindrical object or a rod-shaped object with a cube or a rectangular parallelepiped cross section.
[0059] Drying and calcining steps
[0060] The molded clay is dried and calcined to obtain a catalyst.
[0061] The drying temperature may be 90 to 150° C., preferably 100 to 140° C., and more preferably 120 to 130° C. The drying time may be 5 to 30 hours, preferably 8 to 10 hours. The drying may be carried out in an oven.
[0062] The calcination temperature may be 400-600° C., preferably 450-550° C., and more preferably 500-520° C. The calcination time may be 1-8 hours, preferably 2-5 hours. The calcination may be carried out in a muffle furnace.
[0063] The coating molding method mainly includes the following steps: (A) the step of obtaining the second slurry; (B) the step of obtaining the third slurry; (C) the step of obtaining the load carrier; and (D) the step of drying and calcining.
[0064] Step of obtaining the second slurry
[0065] An alkaline solution is added dropwise to the first slurry including the active ingredient precursor and the carrier precursor to obtain a second slurry.
[0066] The first slurry also includes water. Water can be added to the mixture including the active ingredient precursor and the carrier precursor after uniform mixing, and stirred for 1 to 5 hours; preferably 2 to 3 hours to obtain the first slurry. The amount of water used can be 300 to 700 parts by weight; preferably 400 to 600 parts by weight; more preferably 500 to 550 parts by weight.
[0067] The amount of the active ingredient precursor may be 120 to 185 parts by weight, preferably 140 to 180 parts by weight, and more preferably 150 to 160 parts by weight.
[0068] The amount of the carrier precursor may be 30 to 70 parts by weight, preferably 40 to 60 parts by weight, and more preferably 50 to 55 parts by weight.
[0069] Step of obtaining the third slurry
[0070] Additives and thickeners are added to the second slurry to obtain a third slurry.
[0071] The amount of the additive is 40 to 60 parts by weight, preferably 45 to 55 parts by weight, and more preferably 50 to 55 parts by weight.
[0072] The amount of the thickener is 10 to 50 parts by weight, preferably 20 to 40 parts by weight, and more preferably 30 to 35 parts by weight.
[0073] Steps to obtain the loaded carrier
[0074] The third slurry is coated on the glass fiber corrugated board carrier to obtain a loaded carrier. The third slurry can be coated on the glass fiber corrugated board carrier using a coating machine.
[0075] Drying and calcining steps
[0076] The supported carrier is dried and calcined to obtain a catalyst.
[0077] The drying temperature may be 90 to 150° C., preferably 100 to 140° C., and more preferably 100 to 120° C. The drying time may be 5 to 30 hours, preferably 10 to 25 hours, and more preferably 15 to 20 hours. The drying may be carried out in an oven.
[0078] The calcination temperature may be 400-600° C., preferably 450-550° C., and more preferably 500-520° C. The calcination time may be 1-8 hours, preferably 3-5 hours. The calcination may be carried out in a muffle furnace.
[0079] The active ingredient precursor is selected from one or more of a copper precursor, a cerium precursor, a lanthanum precursor, and a tungsten precursor. The active ingredient precursor can be used in the form of a powder. The active ingredient precursor can be a water-soluble inorganic salt. For example, it can be a nitrate, an acetate, or a tungstate. The copper precursor can be copper nitrate. The cerium precursor can be cerium acetate. The lanthanum precursor can be lanthanum nitrate. The tungsten precursor can be ammonium tungstate.
[0080] In some embodiments, the active ingredient precursor is a copper precursor and a cerium precursor. The amount of the copper precursor is 40 to 60 parts by weight, preferably 45 to 55 parts by weight, and more preferably 50 to 52 parts by weight. The amount of the cerium precursor is 20 to 40 parts by weight, preferably 25 to 35 parts by weight, and more preferably 30 to 32 parts by weight.
[0081] In certain embodiments, the active ingredient precursor is a copper precursor, a lanthanum precursor, and a tungsten precursor. The amount of the copper precursor is 70 to 90 parts by weight, preferably 75 to 85 parts by weight, and more preferably 80 to 82 parts by weight. The amount of the lanthanum precursor is 50 to 70 parts by weight, preferably 55 to 65 parts by weight, and more preferably 60 to 62 parts by weight. The amount of the tungsten precursor is 10 to 30 parts by weight, preferably 15 to 25 parts by weight, and more preferably 20 to 22 parts by weight.
[0082] The composition of the active ingredient precursor can improve the catalyst's performance on CO and NO x Improve the catalytic performance, improve the water and sulfur resistance and the service life of the catalyst.
[0083] The carrier precursor is selected from one or more of titanium dioxide, aluminum oxide, and cordierite. The carrier precursor can be used in the form of powder.
[0084] In some embodiments, the carrier precursor is titanium dioxide and aluminum oxide. The amount of titanium dioxide is 40 to 60 parts by weight, preferably 45 to 55 parts by weight, and more preferably 50 to 52 parts by weight. The amount of aluminum oxide is 70 to 90 parts by weight, preferably 75 to 85 parts by weight, and more preferably 80 to 82 parts by weight.
[0085] In certain embodiments, the carrier precursor is titanium dioxide and cordierite. The amount of titanium dioxide is 10 to 30 parts by weight, preferably 15 to 25 parts by weight, and more preferably 20 to 22 parts by weight. The amount of cordierite is 20 to 40 parts by weight, preferably 25 to 35 parts by weight, and more preferably 30 to 32 parts by weight.
[0086] The above-mentioned carrier precursor is matched with the active component precursor of the present invention to improve the water resistance and sulfur resistance of the catalyst and increase the service life of the catalyst.
[0087] The additive is selected from one or more of pseudo-boehmite, kaolin, polyvinyl alcohol and hydroxymethyl cellulose.
[0088] In certain embodiments, the additives are pseudo-boehmite and kaolin. The amount of pseudo-boehmite is 5 to 20 parts by weight, preferably 7 to 15 parts by weight, and more preferably 10 to 12 parts by weight. The amount of kaolin is 40 to 60 parts by weight, preferably 45 to 55 parts by weight, and more preferably 50 to 52 parts by weight.
[0089] In some embodiments, the additives are polyvinyl alcohol and hydroxymethyl cellulose. The amount of polyvinyl alcohol is 10 to 30 parts by weight, preferably 15 to 25 parts by weight, and more preferably 20 to 22 parts by weight. The amount of hydroxymethyl cellulose is 20 to 40 parts by weight, preferably 25 to 35 parts by weight, and more preferably 30 to 32 parts by weight.
[0090] The above additives can make the catalyst have appropriate strength and pore structure, and improve the catalyst's performance on CO and NO x Improve the catalytic performance and increase the service life.
[0091] The thickener is selected from one or more of silica sol, xanthan gum and alumina sol.
[0092] In certain embodiments, the thickener is silica sol, and the amount of silica sol used is 20 to 60 parts by weight, preferably 30 to 50 parts by weight, and more preferably 40 to 45 parts by weight.
[0093] In certain embodiments, the thickener is xanthan gum and alumina sol. The amount of xanthan gum is 5 to 20 parts by weight, preferably 7 to 15 parts by weight, and more preferably 10 to 12 parts by weight. The amount of alumina sol is 10 to 30 parts by weight, preferably 15 to 25 parts by weight, and more preferably 20 to 22 parts by weight.
[0094] The alkaline solution is selected from one or more of aqueous ammonia, ammonium carbonate solution, and ammonium bicarbonate solution. In some embodiments, the alkaline solution is aqueous ammonia. In other embodiments, the alkaline solution is ammonium bicarbonate solution.
[0095] The rate of dropping the alkaline solution into the first slurry may be 100 to 500 mL / h, 200 to 250 mL / h, or 400 to 450 mL / h.
[0096] The concentration of the alkaline solution may be 0.05 to 0.8 mol / L, preferably 0.1 to 0.6 mol / L. In certain embodiments, the concentration of the alkaline solution is 0.3 to 0.5 mol / L.
[0097] The volume mass ratio of the alkaline solution to the active ingredient precursor is (1-9): 1 L / g. In some embodiments, the volume mass ratio of the alkaline solution to the active ingredient precursor is (6-7): 1 L / g. In other embodiments, the volume mass ratio of the alkaline solution to the active ingredient precursor is (2-3): 1 L / g.
[0098] Appropriate alkaline solutions can combine with active components to form a special structure, thereby improving the catalytic effect of the catalyst, reducing the impact of SO2, water vapor, dust and heavy metals in gaseous substances on the catalytic performance, and increasing the service life of the catalyst.
[0099] <Catalyst and its use>
[0100] The catalyst of the present invention is prepared by the above method. The catalyst of the present invention has a high affinity for CO and NO xIt has high catalytic activity and service life. After 72 hours of use, the catalyst has a CO removal efficiency of ≥93%; preferably, the CO removal efficiency is ≥94%; the catalyst has a NO removal efficiency of ≥93%. x The removal efficiency of NO is ≥94%; preferably, x The removal efficiency is ≥95%. After 288 hours of use, the removal efficiency of CO is ≥80%; preferably, the removal efficiency of CO is ≥84; the removal efficiency of NO x The removal efficiency of NO is ≥81%; preferably, x The removal efficiency is ≥84%.
[0101] Therefore, the present invention provides a catalyst for catalyzing CO and NO x The catalyst of the present invention has the following uses in CO and NO x It also has good catalytic oxidation effect.
[0102] CO and NO x It can exist in gaseous substances. In gaseous substances, the concentration of CO can be 4000-8000 ppm; preferably 5000-7000 ppm; more preferably 6000-6500 ppm. NO x The concentration may be 500 to 1000 ppm; preferably 600 to 900 ppm; more preferably 700 to 800 ppm.
[0103] The gaseous substance may also contain SO2, water vapor and O2. The concentration of SO2 may be 100-500 ppm, preferably 200-300 ppm. The content of water vapor may be 10-40 vol%, preferably 20-30 vol%. The content of O2 may be 10-25 vol%, preferably 16-20 vol%.
[0104] The gaseous substance may also contain NH3. The concentration of NH3 may be 300 to 700 ppm, preferably 400 to 600 ppm, and more preferably 500 to 550 ppm. The balance gas in the gaseous substance may be N2.
[0105] The catalyst can be used at a temperature of 200 to 400°C, preferably 250 to 350°C, and more preferably 300 to 320°C.
[0106] The catalyst can be heated at a space velocity of 6000 to 15000 h -1 Preferably, the catalyst is used at a space velocity of 8000 to 12000 h -1 More preferably, the catalyst is used at a space velocity of 10000 to 11000 h -1 Use under the conditions of.
[0107] Here is the test method:
[0108] The performance of the catalyst was tested in a fixed bed steel tube reactor (2×2 cm) at atmospheric pressure. The catalyst was cut into pieces with a bottom area of 2 cm 2 , a rectangular sample with a height of 5 cm was tested. The reaction temperature was 300℃ and the air velocity was 10000h -1 The composition of the inlet gas is: CO concentration is 6000ppm, NO x The concentration is 800ppm, the NH3 concentration is 500ppm, the SO2 concentration is 200ppm, the water vapor content is 20vol%, the O2 content is 16vol%, and N2 is the balance gas. The composition of the gas at the reactor outlet is measured at regular intervals, and the catalyst's reaction to CO and NO after different reaction times is calculated. x The gas composition was measured using a Madur infrared flue gas analyzer.
[0109] Example 1
[0110] A uniformly mixed mixture consisting of 50 g of titanium dioxide powder, 80 g of aluminum oxide powder, 50 g of copper nitrate powder and 30 g of cerium acetate powder was added to 500 g of deionized water and stirred for 2.5 hours to obtain a first slurry.
[0111] 500 mL of 0.1 mol / L ammonium bicarbonate solution was added dropwise to the first slurry at a rate of 200 mL / h, and stirred evenly to obtain a second slurry. The second slurry was aged at 50° C. for 6 h, and then filtered to obtain a precipitate. The precipitate was dried in an oven at 60° C. for 24 h to obtain a dried precipitate.
[0112] The dried precipitate, 40 g of silica sol, 10 g of pseudo-boehmite and 50 g of kaolin were mixed evenly, added into 240 g of deionized water, and mixed evenly to obtain mud.
[0113] The clay material is extruded by an extruder to obtain molded clay material.
[0114] The molded clay was dried in an oven at 120° C. for 8 h to obtain a dry clay, and the dry clay was calcined in a muffle furnace at 500° C. for 2 h to obtain a catalyst.
[0115] The properties of the catalysts are shown in Table 1.
[0116] Example 2
[0117] A uniformly mixed mixture consisting of 20 g of titanium dioxide powder, 30 g of cordierite powder, 80 g of copper nitrate powder, 60 g of lanthanum nitrate powder and 20 g of ammonium tungstate powder was added to 500 g of deionized water and stirred for 2.5 hours to obtain a first slurry.
[0118] 400 mL of 0.5 mol / L ammonia water was added dropwise to the first slurry at a rate of 400 mL / h, and the mixture was stirred evenly to obtain a second slurry.
[0119] 20 g of polyvinyl alcohol, 30 g of hydroxymethyl cellulose, 10 g of xanthan gum and 20 g of aluminum sol were added to the second slurry, and the mixture was mixed evenly to obtain a third slurry.
[0120] The third slurry was coated on a glass fiber corrugated board carrier using a coating machine to obtain a loaded carrier.
[0121] The supported carrier was dried in an oven at 100° C. for 20 h to obtain a dried supported carrier. The dried supported carrier was calcined in a muffle furnace at 500° C. for 4 h to obtain a catalyst.
[0122] The properties of the catalysts are shown in Table 1.
[0123] Table 1
[0124]
[0125] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.
Claims
1. A method for simultaneously catalyzing CO and NO x A method for preparing a catalyst, characterized in that: The steps include: (1) adding an alkaline solution dropwise to a first slurry comprising 60 to 95 parts by weight of an active ingredient precursor and 100 to 150 parts by weight of a carrier precursor to obtain a second slurry; aging the second slurry, filtering, and obtaining a precipitate; (2) mixing the precipitate with 45 to 75 parts by weight of an additive, 25 to 60 parts by weight of a thickener and water to obtain a slurry; (3) Extruding the clay material to obtain a molded clay material; (4) drying and calcining the formed clay to obtain a catalyst; Or include the following steps: (A) adding a basic solution dropwise to a first slurry comprising 120 to 185 parts by weight of an active ingredient precursor and 30 to 70 parts by weight of a carrier precursor to obtain a second slurry; (B) adding 40 to 60 parts by weight of an additive and 10 to 50 parts by weight of a thickener to the second slurry to obtain a third slurry; (C) coating the third slurry on a glass fiber corrugated board carrier to obtain a loaded carrier; (D) drying and calcining the supported carrier to obtain a catalyst; Wherein, the active ingredient precursor is selected from one or more of a copper precursor, a cerium precursor, a lanthanum precursor, and a tungsten precursor; The carrier precursor is selected from one or more of titanium dioxide, aluminum oxide, and cordierite; The additive is selected from one or more of pseudo-boehmite, kaolin, polyvinyl alcohol, and hydroxymethyl cellulose; The thickener is selected from one or more of silica sol, xanthan gum and alumina sol; The alkaline solution is selected from one or more of aqueous ammonia, ammonium carbonate solution and ammonium bicarbonate solution.
2. The preparation method according to claim 1, characterized in that: The active ingredient precursor is selected from one of the following: (I) 40 to 60 parts by weight of a copper precursor and 20 to 40 parts by weight of a cerium precursor; (II) 70 to 90 parts by weight of a copper precursor, 50 to 70 parts by weight of a lanthanum precursor, and 10 to 30 parts by weight of a tungsten precursor.
3. The preparation method according to claim 1, characterized in that: The carrier precursor is selected from one of the following: (I) 40 to 60 parts by weight of titanium dioxide and 70 to 90 parts by weight of aluminum oxide; (II) 10 to 30 parts by weight of titanium dioxide and 20 to 40 parts by weight of cordierite.
4. The preparation method according to claim 1, characterized in that: The additive is selected from one of the following: (I) 5 to 20 parts by weight of pseudo-boehmite and 40 to 60 parts by weight of kaolin; (II) 10 to 30 parts by weight of polyvinyl alcohol and 20 to 40 parts by weight of hydroxymethyl cellulose.
5. The preparation method according to claim 1, characterized in that: The thickener is selected from one of the following: (I) silica sol; (II) 5 to 20 parts by weight of xanthan gum and 10 to 30 parts by weight of aluminum sol.
6. The preparation method according to claim 1, characterized in that: The concentration of the alkaline solution is 0.05-0.8 mol / L, the volume mass ratio of the alkaline solution to the active ingredient precursor is (1-9):1 L / g, and the speed of dropping the alkaline solution into the first slurry is 100-500 mL / h.
7. The preparation method according to claim 1, characterized in that: The drying temperature is 90-150°C, and the drying time is 5-30 hours; the calcination temperature is 400-600°C, and the calcination time is 1-8 hours.
8. A method for simultaneously catalyzing CO and NO x A catalyst characterized in that The catalyst is obtained by the preparation method according to any one of claims 1 to 7.
9. The catalyst according to claim 8 catalyzes CO and NO simultaneously x Uses in.
10. The use according to claim 9, characterized in that CO and NO x Exists in gaseous substances, CO concentration is 4000~8000ppm, NO x The concentration is 500-1000ppm; The gaseous substance also contains 100-500 ppm of SO2 and 10-40 vol% of water vapor.