A hollow metal oxide @TiO 2 Core-shell structure catalyst and its preparation method and application
Through hollow metal oxide @TiO2 core-shell structure catalyst, the catalyst is prepared using carbon ball template and hydrothermal method, which solves the problem of the reduction of NOx conversion rate of the catalyst at high concentrations of O2 and SO2, and achieves efficient CO reduction NO reaction and resistance Improved sulfur properties.
Patent Information
- Application Number
- CN202111540930.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-12-16
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2041-12-16
Smart Images

Figure HDA0003414280860000011
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalyst material preparation and environmental protection, and specifically relates to a hollow metal oxide@TiO2 core-shell structure catalyst and a preparation method and application thereof. Background Art
[0002] Nitrogen oxides are one of the harmful air pollutants, mainly from thermal power generation, boiler combustion and automobile exhaust, which can cause environmental hazards such as ozone decomposition, acid rain and photochemical smog. Steel sintering flue gas and coke oven flue gas contain a large amount of NOx. Using CO in the flue gas to catalytically reduce NOx is the most economical way, but when high concentrations of O2 exist, CO is more likely to react with O2, and SO2 in the flue gas can easily cause the catalyst to deactivate, resulting in a significant decrease in NOx conversion rate. Therefore, the adsorption behavior of reactants on the catalyst can be effectively regulated by selecting active components and designing catalyst structures, promoting the catalytic reduction of NO by CO, and improving sulfur resistance at the same time.
[0003] In recent years, hollow structures and core-shell catalyst materials have received great attention and have become a research hotspot in the field of catalysis. Hollow materials have unique advantages in catalysis due to their high specific surface area, high porosity, high permeability, low density and other characteristics, and can improve the selectivity of catalytic reactions by accurately controlling the size of the spherical shell aperture. CN106179471A discloses a spherical hollow catalyst for hydrogen production by steam reforming of ethanol and a preparation method thereof. A hollow Beta molecular sieve catalyst for hydrogen production by steam reforming of ethanol is synthesized by using carbon spheres as hard templates and a template-free hydrothermal crystallization method. The ethanol conversion rate reaches 95.8% to 99.8% at 300 to 600°C, and the hydrogen selectivity reaches 63% to 69%. The core-shell components of the core-shell structure material are prone to synergistic effects, and the regulation of catalytic performance is achieved by adjusting the core and shell components and proportions, as well as the particle size and shell thickness. CN104226374A discloses a supported oxide-coated metal core-shell catalyst and a preparation method thereof. The raw gas contains 1% CO and 1% O2, and the space velocity is 15000 mL·h -1 ·g -1 , the CO conversion rate reaches 80% to 90% at 250℃. Summary of the invention
[0004] Due to the characteristics of being cheap, readily available, and multivalent, transition metal oxides are often used as catalysts for CO oxidation and CO catalytic reduction of NO. In view of the effects of O2 and SO2 on the NO conversion rate in the CO catalytic reduction of NO reaction, the present invention provides a hollow metal oxide @ TiO2 core-shell structure catalyst and a preparation method thereof, using carbon spheres as templates and hollow metal oxides with high specific surface area as the core to improve the activity of CO catalytic reduction of NO and reduce the catalytic reaction temperature. At the same time, the characteristics of SO2 being poorly stable and easily decomposed on TiO2 are used to design TiO2 as the shell to improve the sulfur resistance of the catalyst. The present invention has simple operating steps and is easy to control. No expensive agents are used and there are no toxic additives. By adjusting the catalyst cavity size, active component composition, core-shell ratio, etc., the competitive reaction of CO+NO and CO+O2 is regulated, the CO oxidation reaction is inhibited, and the sulfur resistance of the catalyst is improved.
[0005] One aspect of the present invention provides a hollow metal oxide@TiO2 core-shell structure catalyst, wherein the catalyst has a hollow metal oxide as a core and TiO2 as an outer shell.
[0006] Optionally, the specific surface area of the catalyst is 300 to 800 m 2 / g, the cavity size of the inner core is 50-500nm, the core-shell mass ratio is 1:(0.01-0.6), and the outer shell thickness is 10-30nm.
[0007] Optionally, the metal element in the hollow metal oxide is selected from at least one of Ce, Fe, Cu, Mn, Co, Ni, Sn, and Al.
[0008] According to one aspect of the present invention, there is provided a method for preparing the catalyst according to any one of claims 1 to 3, characterized in that it comprises the following steps:
[0009] (1) Preparation of carbon spheres: a soluble carbon source is dissolved in deionized water, subjected to hydrothermal crystallization reaction, cooled to room temperature, centrifuged, and dried to obtain powdered carbon spheres;
[0010] (2) Preparation of metal oxide source solution: Add surfactant, pore-forming agent and complexing agent to an aqueous solution containing soluble metal salt and stir evenly;
[0011] (3) Preparation of metal oxide precursor coated on the surface of carbon spheres: dispersing carbon spheres in deionized water to obtain a suspension, mixing the suspension with a metal oxide source solution, adjusting the pH value to 9-10, stirring, washing, and drying;
[0012] (4) Preparation of hollow metal oxide @ TiO2 core-shell structure catalyst: The metal oxide precursor coated on the surface of the carbon sphere is dispersed in deionized water, and after adding the additive, a soluble titanium source is added dropwise, stirred for 0.5 to 2 hours, and then allowed to stand for aging, washed, filtered, dried, and calcined.
[0013] Optionally, in step (1), the soluble carbon source is selected from at least one of glucose, sucrose and fructose, and the solid-liquid ratio of the soluble carbon source to deionized water is 1:1 to 20;
[0014] The reaction temperature of the hydrothermal crystallization reaction is 120-190°C, and the reaction time is 3-18h;
[0015] The drying condition is 60-120° C. for 4-12 hours;
[0016] The particle size of the powdered carbon spheres is 50 to 500 nm.
[0017] Optionally, in step (2), in the soluble metal salt, the soluble metal cation is selected from at least one of Ce ions, Fe ions, Cu ions, Mn ions, Co ions, Ni ions, Sn ions, and Al ions, and the anion is selected from at least one of nitrate, sulfate, carbonate, acetate, and chloride ions, and the concentration of the soluble metal cation is 0.001 to 0.1 mol / L;
[0018] The mass ratio of the soluble metal salt to the surfactant, pore-forming agent and complexing agent is 1:(1×10 -3 ~1×10 -1 ):(5×10 -3 ~1×10 -1 ):(5×10 -3 ~1×10 -1 );
[0019] The surfactant is selected from at least one of ammonium dodecyl sulfate and sodium hexadecyl sulfonate; the pore-forming agent is selected from at least one of ammonium bicarbonate, benzoic acid and hexadecyltrimethylammonium bromide; and the complexing agent is selected from at least one of hexamethylenetetramine and ethylenediaminetetraacetic acid.
[0020] Optionally, in step (3), the solid-liquid ratio of the carbon spheres to deionized water is 1:30 to 100; and the volume ratio of the suspension to the metal oxide source solution is 1:1 to 5.
[0021] The stirring condition is 40-90° C. for 2-24 hours; the drying condition is 60-120° C. for 4-12 hours;
[0022] In step (3), the pH value is adjusted with alkaline solution, and the alkaline solution is selected from at least one of 1-3 mol / L sodium hydroxide, 1-3 mol / L potassium hydroxide, 15-25% ammonia water, and 10-30% urea.
[0023] Optionally, in step (4), the mass ratio of the metal oxide precursor coated on the surface of the carbon sphere to the additive and the soluble titanium source is 1:(5×10 -3 ~1.5×10 -1 ):(1×10 -2 ~1);
[0024] The auxiliary agent is selected from at least one of citric acid, sodium citrate and ethylene glycol;
[0025] The soluble titanium source is tetrabutyl titanate, and the titanium ion concentration in the mixed solution obtained in step (4) is 1×10 -4 ~1×10 -2 mol / L;
[0026] The static aging time is 2 to 24 hours; the drying condition is drying at 60 to 120° C. for 4 to 12 hours; the calcination temperature is 400 to 600° C., and the calcination time is 3 to 6 hours.
[0027] Optionally, the static aging time is selected from 4h, 6h, 8h, 10h, 12h, 15h, 16h, 18h, 20h, 22h, or any value between any two of the above points.
[0028] Optionally, the calcination temperature is selected from 420°C, 450°C, 470°C, 480°C, 500°C, 530°C, 550°C, 580°C, or any value between any two of the above points;
[0029] The calcination time is selected from 3.5h, 4h, 4.5h, 5h, 5.5h, or any value between any two of the above points.
[0030] One aspect of the present invention provides a use of the above catalyst and the catalyst prepared by the above preparation method in the catalytic reduction of NO by CO.
[0031] Optionally, the reaction temperature of the CO catalytic reduction of NO is 100-300°C, and the space velocity is 10000-50000h -1 The raw gas composition is CO concentration 0.05~1.0%, NO concentration 0.01~0.1%, and N2 is used as the balance gas.
[0032] The characteristics and beneficial effects of the present invention include:
[0033] 1. The size of the carbon spheres prepared by the present invention can be controlled by adjusting the hydrothermal crystallization conditions, the solid-liquid ratio to control the grain size, and the addition of pore-forming agents to increase the specific surface area of the metal oxide, thereby obtaining hollow metal oxide @ TiO2 core-shell structure catalysts with different cavity sizes and high specific surface area.
[0034] 2. The hollow metal oxide@TiO2 core-shell structure catalyst prepared by the present invention may be a single metal oxide or a multi-component composite metal oxide.
[0035] 3. The process of preparing the hollow metal oxide @ TiO2 core-shell structure catalyst of the present invention is simple and easy to control, without using expensive reagents and without any toxic additives.
[0036] 4. The hollow metal oxide @TiO2 core-shell structure catalyst prepared by the present invention can be used for the catalytic reduction of NO by CO, and the coated TiO2 shell structure can significantly improve the sulfur resistance of the catalyst.
[0037] Instruction Manual
[0038] Figure 1 The catalyst obtained in Example 1 is used as an example to evaluate the catalytic activity of CO catalytic reduction of NO. DETAILED DESCRIPTION
[0039] The present invention is described in detail below. The following are only preferred embodiments of the present invention, and the scope of the present invention cannot be limited by them. That is, all equivalent changes and modifications made according to the scope of the patent application of the present invention should belong to the scope covered by the present invention.
[0040] Example 1
[0041] 1. Preparation of carbon spheres: 8 g of glucose was stirred and dissolved in 80 ml of deionized water to form a clear solution, which was then placed in a hydrothermal reactor and maintained at 175 ° C for 8 h. After cooling, a brown turbid liquid was obtained. After centrifugation, it was dried at 70 ° C for 8 h and ground to obtain a brown carbon sphere powder with a particle size of 150-200 nm.
[0042] 2. Preparation of metal oxide source solution: Weigh 18 g aluminum nitrate, 1.8 g iron nitrate, 2.1 g cerium nitrate and dissolve them in 500 mL deionized water, add 0.5 g sodium dodecyl sulfate, 0.9 g ammonium bicarbonate, and 0.6 g hexamethylenetetramine.
[0043] 3. Preparation of metal oxide precursor coated on the surface of carbon spheres: ultrasonically disperse 0.2 g of carbon spheres in 30 mL of deionized water, mix with the metal oxide source solution, add 25% ammonia water to adjust the pH value to 10, stir continuously at 60 ° C for 12 h, cool to room temperature, wash, filter, and dry at 60 ° C for 8 h to obtain the precursor of carbon sphere surface coated with Fe2O3-CeO2-Al2O3.
[0044] 4. Preparation of hollow metal oxide @TiO2 core-shell structure catalyst: 5g carbon sphere surface coated Fe2O3-CeO2-Al2O3 precursor was ultrasonically dispersed in 150ml deionized water, 0.5g sodium citrate was added, 1.6g tetrabutyl titanate was slowly added dropwise, and the mixture was stirred for 1h, then aged for 8h. After washing and filtration, the mixture was dried at 80℃ for 6h and calcined at 500℃ for 4h to obtain a hollow Fe2O3-CeO2-Al2O3@TiO2 core-shell structure catalyst with a specific surface area of 524.67m 2 / g, the cavity size of the inner core is about 200nm, the core-shell mass ratio is 1:0.08, and the outer shell thickness is about 20nm.
[0045] Example 2
[0046] 1. Preparation of carbon spheres: 6.5 g of glucose was stirred and dissolved in 70 ml of deionized water to form a clear solution, which was then placed in a hydrothermal reactor and maintained at 180°C for 7 hours. A brown turbid liquid was obtained after cooling. After centrifugation, it was dried at 60°C for 8 hours and ground to obtain a brown carbon sphere powder with a particle size of 200-250 nm.
[0047] 2. Preparation of metal oxide source solution: Weigh 18 g aluminum sulfate, 1.8 g manganese acetate, and 2.1 g cerium nitrate and dissolve them in 500 mL deionized water, then add 0.6 g sodium hexadecyl sulfate, 1.2 g benzoic acid, and 0.9 g ethylenediaminetetraacetic acid.
[0048] 3. Preparation of metal oxide precursor coated on the surface of carbon spheres: ultrasonically disperse 0.3 g of carbon spheres in 50 mL of deionized water, mix with the metal oxide source solution, add 2.5 mol / L sodium hydroxide to adjust the pH value to 10, stir continuously at 80 ° C for 5 h, cool to room temperature, wash, filter, and dry at 120 ° C for 4 h to obtain the precursor of carbon sphere surface coated with MnO2-CeO2-Al2O3.
[0049] 4. Preparation of hollow metal oxide @TiO2 core-shell structure catalyst: 5g carbon sphere surface coated MnO2-CeO2-Al2O3 precursor was ultrasonically dispersed in 200ml deionized water, 0.3g citric acid was added, 2g tetrabutyl titanate was slowly added, and the mixture was stirred for 1.5h, then aged for 12h. After washing and filtering, the mixture was dried at 100℃ for 5h and calcined at 500℃ for 4h to obtain a hollow MnO2-CeO2-Al2O3@TiO2 core-shell structure catalyst with a specific surface area of 489.03m 2 / g, the cavity size of the inner core is about 250nm, the core-shell mass ratio is 1:0.1, and the outer shell thickness is about 25nm.
[0050] Example 3
[0051] 1. Preparation of carbon spheres: 10 g of glucose was stirred and dissolved in 80 ml of deionized water to form a clear solution, which was then placed in a hydrothermal reactor and maintained at 170 ° C for 9 hours. After cooling, a brown turbid liquid was obtained. After centrifugation, it was dried at 60 ° C for 10 hours and ground to obtain a brown carbon sphere powder with a particle size of 100-150 nm.
[0052] 2. Preparation of metal oxide source solution: Weigh 12g ferric chloride and 2g cerium carbonate and dissolve them in 500mL deionized water, then add 0.6g sodium dodecyl sulfate, 1.5g hexadecyltetramethylammonium bromide and 0.6g hexamethylenetetramine.
[0053] 3. Preparation of metal oxide precursor coated on the surface of carbon spheres: ultrasonically disperse 0.5 g of carbon spheres in 100 mL of deionized water, mix with the metal oxide source solution, add 30% urea solution, adjust the pH value to 10, stir continuously at 40°C for 18 h, cool to room temperature, wash, filter, and dry at 60°C for 10 h to obtain the precursor of carbon sphere surface coated with CeO2-Fe2O3.
[0054] 4. Preparation of hollow metal oxide @ TiO2 core-shell structure catalyst: 5g of carbon sphere surface coated CeO2-Fe2O3 precursor was ultrasonically dispersed in 250ml of deionized water, 0.5g of sodium citrate was added, and 1.2g of tetrabutyl titanate was slowly added dropwise. After continuous stirring for 2h, it was allowed to stand for 6h. After washing and filtering, it was dried at 100℃ for 5h and calcined at 500℃ for 4h to obtain a hollow CeO2-Fe2O3@TiO2 core-shell structure catalyst with a specific surface area of 665.88m 2 / g, the cavity size of the inner core is about 150nm, the core-shell mass ratio is 1:0.06, and the outer shell thickness is about 12nm.
[0055] Example 4
[0056] 1. Preparation of carbon spheres: 8 g of glucose was stirred and dissolved in 80 ml of deionized water to form a clear solution, which was then placed in a hydrothermal reactor and maintained at 165 ° C for 10 h. After cooling, a brown turbid liquid was obtained. After centrifugation, it was dried at 120 ° C for 4 h and ground to obtain a brown carbon sphere powder with a particle size of 100-150 nm.
[0057] 2. Preparation of metal oxide source solution: Weigh 18 g of ferric nitrate and dissolve it in 500 mL of deionized water, add 0.5 g of sodium dodecyl sulfate, 1.5 g of hexadecyltetramethylammonium bromide, and 0.9 g of ethylenediaminetetraacetic acid.
[0058] 3. Preparation of metal oxide precursor coated on the surface of carbon spheres: ultrasonically disperse 0.2 g of carbon spheres in 50 mL of deionized water, mix with the metal oxide source solution, add 2.5 mol / L potassium hydroxide solution, adjust the pH value to 10, stir continuously at 90 ° C for 2 h, cool to room temperature, wash, filter, and dry at 60 ° C for 10 h to obtain the precursor of carbon sphere surface coated with Fe2O3.
[0059] 4. Preparation of hollow metal oxide @TiO2 core-shell structure catalyst: 5g carbon sphere surface coated Fe2O3 precursor was ultrasonically dispersed in 200ml deionized water, 0.5g ethylene glycol was added, 1.6g tetrabutyl titanate was slowly added dropwise, and the mixture was stirred for 2h, then aged for 4h. After washing and filtration, the mixture was dried at 100℃ for 6h and calcined at 500℃ for 4h to obtain a hollow Fe2O3@TiO2 core-shell structure catalyst with a specific surface area of 390.23m 2 / g, the cavity size of the inner core is about 150nm, the core-shell mass ratio is 1:0.08, and the outer shell thickness is about 25nm.
[0060] Test Case
[0061] Taking the catalyst obtained in Example 1 as an example, the catalytic activity of CO catalytic reduction of NO was evaluated, as shown in the following figure. Reaction temperature 100-300°C, space velocity 30000h -1 , raw gas composition: CO concentration 0.65%, NO concentration 0.6%, N2 as balance gas, test results are as follows Figure 1 shown.
[0062] The above are only a few embodiments of the present application and do not constitute any form of limitation to the present application. Although the present application is disclosed as above with preferred embodiments, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases and fall within the scope of the technical solution.
Claims
1. A method for preparing a hollow metal oxide @ TiO2 core-shell structure catalyst, characterized in that: The following steps are involved: (1) Preparation of carbon spheres: Dissolve a soluble carbon source in deionized water, perform a hydrothermal crystallization reaction, cool to room temperature, centrifuge, and dry to obtain powdered carbon spheres; (2) Preparation of metal oxide source solution: Add surfactant, pore-forming agent and complexing agent to the aqueous solution containing soluble metal salt and stir evenly; (3) Preparation of metal oxide precursor coated on the surface of carbon spheres: disperse the carbon spheres in deionized water to obtain a suspension, mix the suspension with a metal oxide source solution, adjust the pH value to 9-10, stir, wash and dry; (4) Preparation of hollow metal oxide @ TiO2 core-shell structure catalyst: The metal oxide precursor coated on the surface of carbon spheres is dispersed in deionized water, and after adding the additive, a soluble titanium source is added dropwise, stirred for 0.5-2 hours, and then allowed to stand for aging, washed, filtered, dried, and calcined; The particle size of the powdered carbon spheres is 50-500 nm; The pore-forming agent is selected from at least one of ammonium bicarbonate, benzoic acid or hexadecyltrimethylammonium bromide; In step (1), the solid-liquid ratio of the soluble carbon source to deionized water is 1:1-20; In step (3), the solid-liquid ratio of the carbon spheres to deionized water is 1:30-100; In step (4), the solid-to-liquid ratio of the precursor of the carbon sphere surface coated with metal oxide to deionized water is 1:10-150; The catalyst has a hollow metal oxide as the core and TiO2 as the shell; The specific surface area of the catalyst is 300-800 m 2 / g, the core cavity size is 50~500nm, the core-shell mass ratio is 1:(0.01~0.6), and the shell thickness is 10~30nm.
2. The preparation method according to claim 1, characterized in that: The metal element in the hollow metal oxide is selected from at least one of Ce, Fe, Cu, Mn, Co, Ni, Sn and Al.
3. The preparation method according to claim 1, characterized in that: In step (1), the soluble carbon source is selected from at least one of glucose, sucrose and fructose; The reaction temperature of the hydrothermal crystallization reaction is 120-190°C, and the reaction time is 3-18h; The drying condition is 60-120° C. for 4-12 hours.
4. The preparation method according to claim 1, characterized in that: In step (2), in the soluble metal salt, the soluble metal cation is selected from at least one of Ce ion, Fe ion, Cu ion, Mn ion, Co ion, Ni ion, Sn ion, and Al ion, and the anion is selected from at least one of nitrate, sulfate, carbonate, acetate, and chloride ion, and the concentration of the soluble metal cation is 0.001-0.1 mol / L; The mass ratio of the soluble metal salt to the surfactant, pore-forming agent and complexing agent is 1:(1×10 -3 ~1×10 -1 ):(5×10 -3 ~1×10 -1 ):(5×10 -3 ~1×10 -1 ); The surfactant is selected from at least one of ammonium dodecyl sulfate and sodium hexadecyl sulfonate; and the complexing agent is selected from at least one of hexamethylenetetramine and ethylenediaminetetraacetic acid.
5. The preparation method according to claim 1, characterized in that: In step (3), the volume ratio of the suspension to the metal oxide source solution is 1:1-5; The stirring condition is 40-90° C. for 2-24 hours; the drying condition is 60-120° C. for 4-12 hours; In step (4), the mass ratio of the metal oxide precursor coated on the surface of the carbon sphere to the additive and the soluble titanium source is 1:(5×10 -3 ~1.5×10 -1 ):(1×10 -2 ~1); The auxiliary agent is selected from at least one of citric acid, sodium citrate and ethylene glycol; and the soluble titanium source is tetrabutyl titanate.
6. The preparation method according to claim 1, characterized in that: In step (4), the static aging time is 2 to 24 hours; the drying condition is drying at 60 to 120° C. for 4 to 12 hours; the roasting temperature is 400 to 600° C., and the roasting time is 3 to 6 hours.
7. Use of the catalyst prepared by the preparation method according to any one of claims 1 to 6 in the catalytic reduction of NO by CO.
8. The use according to claim 7, characterized in that: The reaction temperature of the CO catalytic reduction of NO is 100-300° C. and the space velocity is 10000-50000 h -1 , raw gas components: CO concentration 0.05~1.0%, NO concentration 0.01~0.1%, N2 as balance gas.