Preparation method of antimony nano-material with controllable morphology, antimony nano-material and application of antimony nano-material
The morphology of antimony material is regulated by hydrothermal method, and the volume expansion problem of antimony material in sodium ion batteries is solved, and antimony nanomaterial with controllable morphology is prepared, which improves the energy density and cycle stability of the battery and simplifies the process flow. Suitable for mass production.
Patent Information
- Application Number
- CN202411158088.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In sodium ion batteries, antimony materials have serious volume expansion problems during charging and discharging, resulting in damage to the electrode structure, rapid capacity attenuation and poor cycle stability. The existing methods for regulating the micromorphology of antimony materials are complex and lack simple synthesis methods.
Using the hydrothermal method, the antimony source is dissolved in the reaction medium and the reducing agent is added. By adjusting the reaction temperature and time, the morphology of antimony is regulated, and antimony nanomaterials with controllable morphology are prepared, including steps: dissolution, stirring, and water. Thermal reaction, filtration, washing and drying is simple to operate and suitable for large-scale production.
The preparation of antimony nanomaterials with different morphology has been achieved, the energy density and cycle life of antimony materials in sodium ion batteries has been improved, the damage to the electrode structure has been reduced, and the feasibility of commercial applications has been improved.
Smart Images

Figure CN119016736A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of antimony nanomaterials, and in particular relates to a preparation method of an antimony nanomaterial with controllable morphology, an antimony nanomaterial and applications thereof. Background Art
[0002] With the urgent global demand for sustainable development and clean energy, energy storage technology, as a key bridge connecting renewable energy production and consumption, has become increasingly important. As the focus of current energy storage technology, lithium-ion batteries have been widely used in many fields, but their development faces bottlenecks such as limited lithium resources and rising costs. Sodium-ion batteries, with their advantages of abundant resources, low cost, and environmental friendliness, have shown significant cost reduction potential and have become a research hotspot.
[0003] The working principle of sodium-ion batteries is similar to that of lithium-ion batteries, both of which rely on the reversible insertion and extraction of metal ions between the positive and negative electrodes to achieve the storage and release of electrical energy. However, due to the large radius of sodium ions, their diffusion kinetics in electrode materials are slow and can easily cause significant changes in the material structure, especially the volume expansion problem of negative electrode materials during the charging and discharging process. This not only limits the energy density and cycle life of sodium-ion batteries, but also increases the difficulty of their commercial application. In this context, antimony (Sb), as a candidate negative electrode material with high theoretical capacity, has attracted widespread attention in the scientific research community. Antimony materials also face serious volume expansion problems during the charging and discharging process, which leads to adverse consequences such as electrode structure destruction, rapid capacity decay, and poor cycle stability. Therefore, how to regulate the morphology of antimony nanomaterials through effective strategies to optimize their structural characteristics has become the key to improving the negative electrode performance of sodium-ion batteries.
[0004] In current research, in terms of regulating the micromorphology of antimony materials, most methods have disadvantages such as complex processes or the use of dangerous drugs, and there is still a lack of some simple synthesis methods. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide a method for preparing antimony nanomaterials with controllable morphology, antimony nanomaterials and their applications. The preparation method provided by the present invention is simple to operate and easy to expand the production of antimony nanomaterials with different morphologies, which provides a basis for expanding the application of antimony materials in the field of sodium ion batteries and other fields.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a method for preparing an antimony nanomaterial with controllable morphology, comprising the following steps:
[0008] 1) fully dissolving the antimony source in the reaction medium, adding a reducing agent, and stirring evenly to obtain a mixed solution;
[0009] 2) subjecting the mixed solution obtained in step 1) to a hydrothermal reaction, and cooling the mixed solution after the reaction is completed to obtain a first product;
[0010] 3) filtering the first product obtained in step 2) to obtain a second product;
[0011] 4) Washing and drying the second product obtained in step 3) to obtain antimony nanomaterials with controllable morphology.
[0012] Preferably, the antimony source includes antimony chloride, and the reducing agent includes aluminum powder.
[0013] Preferably, the reaction medium comprises ethylene glycol.
[0014] Preferably, the molar ratio of the antimony source to the aluminum powder is 1 to 3:1.
[0015] Preferably, the temperature of the hydrothermal reaction is 120-180° C., and the time of the hydrothermal reaction is 6-12 hours.
[0016] Preferably, the hydrothermal reaction method comprises: transferring the mixed solution obtained in step 1) to a polytetrafluoroethylene liner and placing it in a reaction kettle, and moving the reaction kettle to an electric constant temperature forced air drying oven for heating reaction.
[0017] Preferably, the washing method comprises: washing the second product with anhydrous ethanol, deionized water and anhydrous ethanol in sequence.
[0018] Preferably, the drying temperature is 50-80° C., and the drying time is 8-12 hours.
[0019] The present invention also provides an antimony nano material with controllable morphology prepared by the above preparation method.
[0020] The present invention also provides the use of the above-mentioned morphology-controllable antimony nanomaterial in the preparation of sodium ion batteries.
[0021] The present invention adopts a hydrothermal method, selects a suitable antimony source, a reducing agent and a reaction medium, and adjusts the reaction temperature and time to control the morphology of antimony, thereby solving the problem of complex preparation of antimony nanomaterials with different morphologies. The preparation method provided by the present invention is simple to operate, has good repeatability, and meets the requirements of expanding production. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 XRD patterns of antimony with different morphologies prepared in Examples 1 and 2;
[0023] Figure 2This is a SEM image of the leaf-shaped antimony prepared in Example 1;
[0024] Figure 3 This is a SEM image of the spherical antimony prepared in Example 2;
[0025] Figure 4 This is the rate performance diagram of the spherical antimony prepared in Example 2 for use in sodium ion batteries. DETAILED DESCRIPTION
[0026] The present invention provides a method for preparing an antimony nanomaterial with controllable morphology, comprising the following steps:
[0027] 1) fully dissolving the antimony source in the reaction medium, adding a reducing agent, and stirring evenly to obtain a mixed solution;
[0028] 2) subjecting the mixed solution obtained in step 1) to a hydrothermal reaction, and cooling the mixed solution after the reaction is completed to obtain a first product;
[0029] 3) filtering the first product obtained in step 2) to obtain a second product;
[0030] 4) Washing and drying the second product obtained in step 3) to obtain antimony nanomaterials with controllable morphology.
[0031] In the present invention, the antimony source is preferably antimony chloride. The present invention has no special limitation on the source of the antimony chloride, and any conventional commercial product in the art can be used.
[0032] In the present invention, the reaction medium is preferably ethylene glycol. The present invention has no special limitation on the source of the ethylene glycol, and any conventional commercial product in the art can be used.
[0033] In the present invention, the reducing agent is preferably aluminum powder. The present invention has no special limitation on the source of the aluminum powder, and any conventional commercial product in the art can be used.
[0034] In the present invention, the molar ratio of the antimony source to the aluminum powder is preferably 1 to 3:1, more preferably 2:1.
[0035] The present invention has no particular limitation on the stirring method, and any conventional stirring method in the art may be used.
[0036] In the present invention, the stirring time is preferably 10 to 60 minutes, more preferably 30 minutes.
[0037] In the present invention, the hydrothermal reaction method preferably comprises: transferring the mixed solution obtained in step 1) to a polytetrafluoroethylene liner and placing it in a reaction kettle, and moving the reaction kettle to an electric constant temperature blast drying oven for heating reaction.
[0038] In the present invention, the temperature of the hydrothermal reaction is preferably 120-180° C., more preferably 150° C.; the time of the hydrothermal reaction is preferably 6-12 h, more preferably 10 h.
[0039] The present invention has no particular limitation on the cooling method, and conventional cooling methods in the art may be used.
[0040] In the present invention, the cooling temperature is preferably cooled to room temperature.
[0041] In the present invention, the first product is preferably a powder.
[0042] The present invention has no particular limitation on the washing method. Preferably, the second product is washed with anhydrous ethanol, deionized water, and anhydrous ethanol in sequence.
[0043] The present invention has no particular limitation on the drying method, and any conventional drying method in the art may be used.
[0044] In the present invention, the drying temperature is preferably 50 to 80° C., more preferably 60° C.; the drying time is preferably 8 to 12 h, more preferably 10 h.
[0045] The present invention also provides an antimony nano material with controllable morphology prepared by the above preparation method.
[0046] The present invention also provides the use of the above-mentioned morphology-controllable antimony nanomaterial in the preparation of sodium ion batteries.
[0047] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0048] Example 1
[0049] Fully dissolve 0.008 mol of SbCl3 in 80 ml of ethylene glycol, add 0.004 mol of aluminum powder, stir for 30 minutes to evenly disperse it in the solution, transfer the resulting solution to a polytetrafluoroethylene liner and place it in a reactor, move the reactor to an electric constant temperature blast drying oven, heat to 150°C, and react for 10 hours. After the reaction is completed, cool to room temperature, filter the resulting powder, and wash the collected product with anhydrous ethanol, deionized water, and anhydrous ethanol in turn, and finally dry it in an oven at 60°C for 10 hours to obtain the product.
[0050] Example 2
[0051] Fully dissolve 0.008 mol of SbCl3 in 80 ml of ethylene glycol, add 0.004 mol of aluminum powder, stir for 30 minutes to evenly disperse it in the solution, transfer the resulting solution to a polytetrafluoroethylene liner and place it in a reactor, move the reactor to an electric constant temperature blast drying oven, heat to 180°C, and react for 5 hours. After the reaction is completed, cool to room temperature, filter the resulting powder, and wash the collected product with anhydrous ethanol, deionized water, and anhydrous ethanol in turn, and finally dry it in an oven at 60°C for 10 hours to obtain the product.
[0052] Example 3
[0053] Fully dissolve 0.008 mol of SbCl3 in 80 ml of ethylene glycol, add 0.004 mol of aluminum powder, stir for 30 minutes to evenly disperse it in the solution, transfer the resulting solution to a polytetrafluoroethylene liner and place it in a reactor, move the reactor to an electric constant temperature blast drying oven, heat to 180°C, and react for 10 hours. After the reaction is completed, cool to room temperature, filter the resulting powder, and wash the collected product with anhydrous ethanol, deionized water, and anhydrous ethanol in turn, and finally dry it in an oven at 60°C for 10 hours to obtain the product.
[0054] Example 4
[0055] The final products obtained in Example 1 and Example 2 were characterized using an X-ray diffractometer. The results are shown in the attached figure. Figure 1 As shown, the obtained curves are well consistent with the standard PDF card of antimony (PDF#35-0732), indicating that the products obtained in Examples 1 and 2 are both antimony.
[0056] Example 5
[0057] The final products obtained in Example 1 and Example 2 were characterized using a scanning electron microscope. The results are shown in the attached Figure 2 , 3 As shown, it can be seen that the morphology of the product obtained in Example 1 is branch-like, and the product obtained in Example 2 is spherical, indicating that antimony with different microscopic morphologies can be obtained by adjusting the reaction temperature and time.
[0058] Example 6
[0059] The antimony powder obtained in Example 2 was mixed with Super P and CMC in a ratio of 7:1.5:1.5 to form a slurry, which was coated on copper foil as the negative electrode. Glass fiber was used as the separator. The electrolyte was 1M NaClO4 in EC:PC=1:1Vol%with5%FEC. A sodium metal sheet was used as the positive electrode. A button half-cell was assembled in an argon-filled glove box. The electrochemical cycle performance was tested by charging and discharging for five cycles at rates of 0.1C, 0.2C, 0.5C, 1C, 2C, and 0.1C, respectively. The results are shown in the attached figure. Figure 4 As shown, it shows that the prepared antimony negative electrode has good cycle performance.
[0060] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing antimony nanomaterials with controllable morphology, characterized in that: The following steps are involved: 1) fully dissolving the antimony source in the reaction medium, adding a reducing agent, and stirring evenly to obtain a mixed solution; 2) subjecting the mixed solution obtained in step 1) to a hydrothermal reaction, and cooling the mixed solution after the reaction is completed to obtain a first product; 3) filtering the first product obtained in step 2) to obtain a second product; 4) Washing and drying the second product obtained in step 3) to obtain antimony nanomaterials with controllable morphology.
2. The method for preparing a morphology-controlled antimony nanomaterial according to claim 1, characterized in that: The antimony source includes antimony chloride, and the reducing agent includes aluminum powder.
3. The method for preparing a morphology-controlled antimony nanomaterial according to claim 1, characterized in that: The reaction medium includes ethylene glycol.
4. The method for preparing a morphology-controlled antimony nanomaterial according to claim 1, characterized in that: The molar ratio of the antimony source to the aluminum powder is 1 to 3:
1.
5. The method for preparing a morphology-controllable antimony nanomaterial according to claim 1, characterized in that: The temperature of the hydrothermal reaction in step 2) is 120-180° C., and the time of the hydrothermal reaction is 6-12 hours.
6. The method for preparing a morphology-controlled antimony nanomaterial according to claim 1, characterized in that: The method for the hydrothermal reaction in step 2) comprises: transferring the mixed solution obtained in step 1) to a polytetrafluoroethylene liner and placing it in a reaction kettle, and moving the reaction kettle to an electric constant temperature blast drying oven for heating and reaction.
7. The method for preparing a morphology-controlled antimony nanomaterial according to claim 1, characterized in that: The washing method in step 4) comprises: washing the second product with anhydrous ethanol, deionized water, and anhydrous ethanol in sequence.
8. The method for preparing a morphology-controllable antimony nanomaterial according to claim 1, characterized in that: The drying temperature in step 4) is 50-80° C. and the drying time is 8-12 hours.
9. The antimony nanomaterial with controllable morphology prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the morphology-controllable antimony nanomaterial according to claim 9 in the preparation of sodium ion batteries.
Citation Information
Patent Citations
Preparation method of negative electrode material nanometer needle-like phosphate antimony
CN110589789A
Antimony and / or bismuth nanosheet, antimonene and / or bismuthene as well as preparation methods and application thereof
CN112792350A
Aluminum conductive paste for solar cell and preparation method of aluminum conductive paste
CN115985548A
Dopant compositions and the method of making to form doped regions in semiconductor materials
US20130178011A1