Preparation method of polyhedral micro-nano copper powder

Through the two-step reduction reaction method, the pH value and temperature are adjusted to prepare polyhedral micro-nano copper powder with high dispersion and uniformity, which solves the problems of low yield and agglomeration in the prior art and achieves efficient industrial production.

CN119016739APending Publication Date: 2024-11-26CHONGQING YOUYAN ZHONGYE NEW MATERIAL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411249310.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the existing micro-nano copper powder preparation methods, the yield is low and there is agglomeration phenomenon, making it difficult to meet the efficient requirements of industrial applications.

Method used

Using a two-step reduction reaction method, firstly heat the copper oxide suspension with the preliminary reduction solution to form a copper oxide suspension, and then mix it with the reduction-protective solution for reduction reaction. By adjusting the pH value and temperature control, high dispersion is obtained. polyhedral micro-nano copper powder with uniformity.

Benefits of technology

It significantly improves the yield of micro-nano copper powder to reach more than 95%, reduces agglomeration phenomenon, is simple in process and environmentally friendly, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119016739A_ABST
    Figure CN119016739A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of polyhedral micro-nano copper powder. The preparation method comprises the following steps: S1, preparing copper oxide into a copper oxide suspension; s2, a reducing agent is prepared into a solution, the pH value is adjusted to be alkaline, and a preliminary reduction solution is prepared; s3, respectively heating the copper oxide suspension prepared in the step S1 and the preliminary reduction solution prepared in the step S2 to a reduction reaction temperature, and mixing to prepare a cuprous oxide suspension; s4, a reducing agent and a protective agent are prepared into a solution, the pH value is adjusted to be acidic, and a reduction-protection solution is prepared; s5, respectively heating the cuprous oxide suspension prepared in the step S3 and the reduction-protection solution prepared in the step S4 to a mixing temperature, mixing, and then heating to a reduction reaction temperature to prepare a copper dispersoid; and S6, the copper dispersoid prepared in the step S5 is sequentially washed, dried and ground, and the polyhedral micro-nano copper powder is prepared. According to the scheme, the problem of how to further improve the yield of the polyhedral micro-nano copper powder is solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a method for preparing metal powder from liquid metal compounds, in particular to a method for preparing polyhedral micro-nano copper powder. Background Art

[0002] Micro-nano copper powder retains the good electrical conductivity, thermal conductivity, corrosion resistance, antibacterial and anti-electromigration properties of copper metal while having the characteristics of small size effect, low melting point and high activity. It is widely used in the electronics industry, powder metallurgy components, high-end carbon brushes, high-speed rail brake materials, superhard materials, shielding materials, lubricants, catalysts and medicine.

[0003] The preparation methods of micro-nano copper powder can be divided into solid phase method, gas phase method and liquid phase method according to the state of raw materials. The currently available literature shows that the micro-nano copper powder obtained by the solid phase method has poor uniformity, the particle size and morphology are difficult to control, and impurities are easily introduced, which is difficult to meet the performance requirements of application scenarios in the field of microelectronics. The equipment and process of the gas phase method are relatively complex, the output is small, the production cost is high, and it is difficult to achieve large-scale production. The liquid phase chemical reduction method has a simple process and low cost. It can achieve precise control of the particle size and morphology characteristics of micro-nano copper powder and has broad application prospects in industrial production. Therefore, it is of great value to develop a micro-nano copper powder preparation process with controllable particle size, high crystallinity, good dispersibility and uniformity, and easy mass production through the liquid phase chemical reduction method.

[0004] Chinese patent document CN118106498A discloses a method for preparing polyhedral micro-nano copper powder, comprising the following steps: S1, preparing copper oxide into a copper oxide suspension; S2, preparing a solution with a reducing agent and a protecting agent, adjusting the pH value of the solution to be slightly acidic, and preparing a reducing-protecting solution; S3, heating the copper oxide suspension obtained in step S1 and the reducing-protecting solution obtained in step S2 to a mixing temperature respectively and then mixing them, and continuing to heat to a reduction reaction temperature after mixing to prepare a copper dispersoid; S4, washing, drying and grinding the copper dispersoid prepared in step S3 in sequence to prepare a polyhedral micro-nano copper powder.

[0005] The above preparation method is a solution developed by the applicant earlier. In industrial applications, the final micro-nano copper powder has a small amount of agglomeration, and the yield is generally maintained between 92% and 93%. With the increasing requirements for improving quality and efficiency, how to further reduce the agglomeration phenomenon and improve the yield has become a technical problem that needs to be solved urgently. Summary of the invention

[0006] The purpose of the present invention is to provide a method for preparing polyhedral micro-nano copper powder to solve the problem of how to further improve the yield.

[0007] In order to achieve the above object, the basic scheme of the present invention provides a method for preparing polyhedral micro-nano copper powder, comprising the following steps: S1, preparing copper oxide into a copper oxide suspension; S2, preparing a reducing agent into a solution, and adjusting the pH value to alkaline to obtain a preliminary reducing solution; S3, heating the copper oxide suspension obtained in step S1 and the preliminary reduction solution obtained in step S2 to the reduction reaction temperature respectively and then mixing them to obtain a cuprous oxide suspension; S4, preparing a solution of a reducing agent and a protecting agent, and adjusting the pH value to acidic to obtain a reducing-protecting solution; S5, heating the cuprous oxide suspension obtained in step S3 and the reduction-protection solution obtained in step S4 to a mixing temperature respectively, mixing them, and then heating them to a reduction reaction temperature to obtain a copper dispersion; S6. Wash, dry and grind the copper dispersion obtained in step S5 in sequence to obtain polyhedral micro-nano copper powder.

[0008] The beneficial effects of this basic scheme are: Preferably, in step S2, the pH value of the preliminary reducing solution is 8-13.

[0009] Preferably, in step S3, the reduction reaction temperature is 70-100° C., and the reduction reaction time is 0.5-3 h.

[0010] Preferably, in step S4, the pH value of the reduction-protection solution is 2-5.

[0011] Preferably, in step S1, the concentration of the copper oxide suspension is 0.2-5 mol / L.

[0012] Preferably, in step S5, the reduction reaction temperature is 70-100° C., and the reduction reaction time is 0.5-3 h.

[0013] Preferably, the reducing agent is ascorbic acid, and the mass ratio of the reducing agent to the copper element in copper oxide is between 1:2 and 6:1.

[0014] Preferably, the protective agent is selected from one or a combination of at least two of polyvinyl pyrrolidone, sorbitol, and sodium citrate, and the mass ratio of the protective agent to the copper element in copper oxide is between 1:1 and 10:1.

[0015] Preferably, the alkaline solution is selected from one of a sodium hydroxide aqueous solution and a potassium hydroxide aqueous solution or a combination of the two, and the concentration of the alkaline solution is 0.1-5 mol / L.

[0016] Preferably, in step S6, the drying is vacuum freeze drying, and the drying time is 6-18 hours.

[0017] The present invention has the following beneficial effects: The present invention uses copper oxide as a raw material and performs a two-step reduction reaction to prepare micro-nano copper powder, so that the obtained micro-nano copper powder has excellent dispersibility and uniformity, effectively controls the phenomenon of particle agglomeration, and has a simple preparation process flow, a yield of more than 95%, is green and environmentally friendly, has little pollution to the environment, and is suitable for large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is an electron microscope image of the copper powder prepared in Example 1 of the method for preparing a polyhedral micro-nano copper powder of the present invention; Figure 2 This is an electron microscope image of the copper powder prepared in Example 2 of the method for preparing a polyhedral micro-nano copper powder of the present invention; Figure 3 This is an electron microscope image of the copper powder prepared in Example 3 of the method for preparing a polyhedral micro-nano copper powder of the present invention; Figure 4 This is an electron microscope image of the copper powder prepared in Example 4 of the method for preparing a polyhedral micro-nano copper powder of the present invention; Figure 5 This is an electron microscope image of the copper powder prepared in Comparative Example 1 of the present invention. DETAILED DESCRIPTION

[0019] 1. Definition 1) Suspension refers to a mixture of insoluble solid particles larger than 100 nanometers suspended in a liquid.

[0020] 2) A reducing agent refers to a substance that loses electrons or has electrons deviated in a redox reaction.

[0021] 2. Various preferred solutions involving the scope that are not described in the claims 1) The concentration of the copper oxide suspension is 0.2-5 mol / L, preferably 0.5-4 mol / L, and further preferably 1.0 mol / L, 1.5 mol / L, 2.0 mol / L, 2.5 mol / L, 3.0 mol / L, etc. 2) The pH value of the preliminary reducing solution is 8-13, preferably 9-12, and further preferably 10, 11, etc.

[0022] 3) The reduction reaction temperature is 70-100°C, preferably 80-90°C, and more preferably 75°C, 85°C, 95°C, etc.

[0023] 4) The reduction reaction time is 0.5-3 h, preferably 1-2.5 h, and further preferably 1.5 h, 2 h, etc.

[0024] 5) The pH value of the reduction-protection solution is 2-5, preferably 3-4.

[0025] 6) The mass ratio of the reducing agent to the copper element in the copper oxide is between 1:2 and 6:1, preferably 1:1, 2:1, 3:1, 4:1, 5:1, etc.

[0026] 7) The mass ratio of the protective agent to the copper element in the copper oxide is between 1:1 and 10:1, preferably 2:1, 3:1, 4:1, 5:1, 6:1, 7:1, 8:1, etc.

[0027] 8) The concentration of the alkaline solution is 0.1-5 mol / L, preferably 0.2 mol / L, 0.3 mol / L, 0.4 mol / L, 0.5 mol / L, 1 mol / L, 2 mol / L, 3 mol / L, 4 mol / L, etc.

[0028] 9) The drying time is 6-18 hours, preferably 8 hours, 10 hours, 12 hours, 14 hours, 16 hours, etc.

[0029] The following is further described in detail through specific implementation methods: Example 1 A method for preparing polyhedral micro-nano copper powder comprises the following steps: S1. Prepare copper oxide suspension by adding copper oxide. Specifically, add 8 g of copper oxide into 0.5 L of water and stir thoroughly to prepare a copper oxide suspension with a concentration of 0.2 mol / L.

[0030] S2, making a reducing agent into a solution, and adjusting the pH value to alkaline, to obtain a preliminary reducing solution. Specifically, 38.4 g of ascorbic acid was added to 0.5 L of water, fully dissolved, and then 0.1 mol / L of sodium hydroxide solution was added to the solution, stirred evenly, and the pH value of the solution was adjusted to 8.0 to obtain a preliminary reducing solution.

[0031] S3, heating the copper oxide suspension obtained in step S1 and the preliminary reduction solution obtained in step S2 to the reduction reaction temperature and mixing them to obtain a cuprous oxide suspension. Specifically, heating the copper oxide suspension obtained in step S1 and the preliminary reduction solution obtained in step S2 to 70° C. and mixing them, stirring them fully and performing a reduction reaction, the reduction reaction time is 1 hour, and obtaining a cuprous oxide suspension.

[0032] S4, the reducing agent and the protective agent are made into a solution, and the pH value is adjusted to acidic to obtain a reducing-protecting solution. Specifically, 38.4g of ascorbic acid and 32g of polyvinyl pyrrolidone are added to 0.5L of water, fully dissolved, stirred evenly, 0.1mol / L of sodium hydroxide solution is added to the solution, and the pH value of the solution is adjusted to 3.0 while stirring continuously to obtain a reducing-protecting solution.

[0033] S5, heating the cuprous oxide suspension obtained in step S3 and the reduction-protection solution obtained in step S4 to a mixing temperature, mixing them, and then heating them to a reduction reaction temperature to obtain a copper dispersion. Specifically, the cuprous oxide suspension obtained in step S3 and the reduction-protection solution obtained in step S4 are heated to 70° C., mixed, fully stirred, and subjected to a reduction reaction, and the reduction reaction time is 1 hour to obtain a copper dispersion.

[0034] S6, washing, drying and grinding the copper dispersion obtained in step S5 in sequence to obtain polyhedral micro-nano copper powder. Specifically, the copper dispersion obtained in step S5 was centrifuged, washed, vacuum freeze-dried at -40°C for 12h and ground in sequence to obtain 6.1g of polyhedral micro-nano copper powder with a yield of 95.99%.

[0035] The prepared polyhedral micro-nano copper powder was imaged by scanning electron microscope, and the imaging results are as follows: Figure 1 As shown, it can be seen that the copper powder has good dispersion and no agglomeration.

[0036] Example 2 A method for preparing polyhedral micro-nano copper powder comprises the following steps: S1. Add 40 g of copper oxide into 0.5 L of water and stir thoroughly to prepare a copper oxide suspension with a concentration of 1 mol / L.

[0037] S2. Add 160 g of ascorbic acid into 0.5 L of water and fully dissolve it. Then add 1 mol / L of sodium hydroxide solution into the solution, stir evenly, and adjust the pH value of the solution to 10.0 to obtain a preliminary reduction solution.

[0038] S3. The copper oxide suspension obtained in step S1 and the preliminary reduction solution obtained in step S2 are heated to 80° C. respectively, mixed, fully stirred and subjected to reduction reaction for 3 hours to obtain a cuprous oxide suspension.

[0039] S4. Add 160 g of ascorbic acid and 96 g of polyvinyl pyrrolidone into 0.5 L of water, fully dissolve, stir evenly, add 0.1 mol / L of sodium hydroxide solution into the solution, stir continuously, adjust the pH value of the solution to 3.0, and prepare a reduction-protection solution.

[0040] S5. The cuprous oxide suspension obtained in step S3 and the reduction-protection solution obtained in step S4 are heated to 80° C. respectively, mixed, fully stirred and subjected to reduction reaction. The reduction reaction time is 1 hour to obtain a copper dispersion.

[0041] S6, washing, drying and grinding the copper dispersion obtained in step S5 in sequence to obtain polyhedral micro-nano copper powder. Specifically, the copper dispersion obtained in step S5 was centrifuged, washed, vacuum freeze-dried at -40°C for 12h and ground in sequence to obtain 31.1g of polyhedral micro-nano copper powder with a yield of 97.88%.

[0042] The prepared polyhedral micro-nano copper powder was imaged by scanning electron microscope, and the imaging results are as follows: Figure 2 As shown, it can be seen that the copper powder has good dispersion and no agglomeration.

[0043] Example 3 A method for preparing polyhedral micro-nano copper powder comprises the following steps: S1. Add 40 g of copper oxide into 0.5 L of water and stir thoroughly to prepare a copper oxide suspension with a concentration of 1 mol / L.

[0044] S2. Add 128 g of ascorbic acid into 0.5 L of water and fully dissolve it. Then add 1 mol / L of sodium hydroxide solution into the solution and stir evenly. Adjust the pH value of the solution to 13.0 to obtain a preliminary reduction solution.

[0045] S3. The copper oxide suspension obtained in step S1 and the preliminary reduction solution obtained in step S2 are heated to 80° C. respectively, mixed, fully stirred and subjected to reduction reaction for 3 hours to obtain a cuprous oxide suspension.

[0046] S4. Add 128 g of ascorbic acid and 64 g of sorbitol into 0.5 L of water, fully dissolve, stir evenly, add 1 mol / L of sodium hydroxide solution to the solution, stir continuously, adjust the pH value of the solution to 4.0, and prepare a reduction-protection solution.

[0047] S5. The cuprous oxide suspension obtained in step S3 and the reduction-protection solution obtained in step S4 are heated to 80° C. respectively, mixed, fully stirred and subjected to reduction reaction. The reduction reaction time is 1 hour to obtain a copper dispersion.

[0048] S6, washing, drying and grinding the copper dispersion obtained in step S5 in sequence to obtain polyhedral micro-nano copper powder. Specifically, the copper dispersion obtained in step S5 was centrifuged, washed, vacuum freeze-dried at -40°C for 12h and ground in sequence to obtain 30.6g of polyhedral micro-nano copper powder with a yield of 96.31%.

[0049] The prepared polyhedral micro-nano copper powder was imaged by scanning electron microscope, and the imaging results are as follows: Figure 3 As shown, it can be seen that the copper powder has good dispersion and no agglomeration.

[0050] Example 4 A method for preparing polyhedral micro-nano copper powder comprises the following steps: S1. Add 16 g of copper oxide into 0.5 L of water and stir thoroughly to obtain a copper oxide suspension with a concentration of 0.4 mol / L.

[0051] S2. Add 50.8 g of ascorbic acid into 0.5 L of water and fully dissolve it. Then add 4 mol / L of sodium hydroxide solution into the solution and stir evenly. Adjust the pH value of the solution to 9.0 to obtain a preliminary reduction solution.

[0052] S3. The copper oxide suspension obtained in step S1 and the preliminary reduction solution obtained in step S2 are heated to 90° C. respectively, mixed, fully stirred and subjected to reduction reaction. The reduction reaction time is 0.5 h, and a cuprous oxide suspension is obtained.

[0053] S4. Add 50.8 g of ascorbic acid and 50.8 g of polyvinyl pyrrolidone into 0.5 L of water, fully dissolve, stir evenly, add 4 mol / L of sodium hydroxide solution to the solution, stir continuously, adjust the pH value of the solution to 5.0, and prepare a reduction-protection solution.

[0054] S5. The cuprous oxide suspension obtained in step S3 and the reduction-protection solution obtained in step S4 are heated to 90° C. respectively, mixed, fully stirred and subjected to reduction reaction for 0.5 h to obtain a copper dispersion.

[0055] S6, washing, drying and grinding the copper dispersion obtained in step S5 in sequence to obtain polyhedral micro-nano copper powder. Specifically, the copper dispersion obtained in step S5 was centrifuged, washed, vacuum freeze-dried at -40°C for 12h and ground in sequence to obtain 12.3g of polyhedral micro-nano copper powder with a yield of 96.77%.

[0056] The prepared polyhedral micro-nano copper powder was imaged by scanning electron microscope, and the imaging results are as follows: Figure 4 As shown, it can be seen that the copper powder has good dispersion and no agglomeration.

[0057] Comparative Example 1 Comparative Example: This comparative example is to directly react the copper oxide suspension with the reduction-protection solution, and the specific steps are as follows: S1. Add 40 g of copper oxide into 0.5 L of water to prepare a copper oxide suspension with a concentration of 1 mol / L.

[0058] S2. Select ascorbic acid as a reducing agent and select sorbitol as a protecting agent. Add 128 g ascorbic acid and 64 g sorbitol into 0.5 L water, stir to dissolve, add 1 mol / L sodium hydroxide solution into the solution, adjust the pH value of the solution to 4.0, and obtain a reducing-protecting solution.

[0059] S3. The copper oxide suspension prepared in step S1 and the reduction-protection solution prepared in step S2 are heated to 50° C. respectively, the two solutions are mixed, and after sufficient stirring, the mixed solution is heated to 80° C. for reduction reaction. The reduction time is 1 hour to obtain a copper dispersion.

[0060] S4. The copper dispersion prepared in step S3 was centrifuged, washed, freeze-dried at -40°C for 12 h and ground in sequence to obtain 29.7 g of polyhedral micro-nano copper powder with a yield of 92.8%.

[0061] The prepared polyhedral micro-nano copper powder was imaged by scanning electron microscope, and the imaging results are as follows: Figure 5 As shown, it can be seen that the copper powder has agglomeration phenomenon.

[0062] The above is only an embodiment of the present invention, and the common knowledge such as the known specific structure and characteristics in the scheme is not described in detail here. It should be pointed out that for those skilled in the art, several modifications and improvements can be made without departing from the structure of the present invention, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the implementation of the present invention and the practicality of the patent.

Claims

1. A method for preparing polyhedral micro-nano copper powder, It is characterized in that The following steps are involved: S1, preparing copper oxide into a copper oxide suspension; S2, preparing a reducing agent into a solution, and adjusting the pH value to alkaline to obtain a preliminary reducing solution; S3, heating the copper oxide suspension obtained in step S1 and the preliminary reduction solution obtained in step S2 to the reduction reaction temperature respectively and then mixing them to obtain a cuprous oxide suspension; S4, preparing a solution of a reducing agent and a protecting agent, and adjusting the pH value to acidic to obtain a reducing-protecting solution; S5, heating the cuprous oxide suspension obtained in step S3 and the reduction-protection solution obtained in step S4 to a mixing temperature respectively, mixing them, and then heating them to a reduction reaction temperature to obtain a copper dispersion; S6. Wash, dry and grind the copper dispersion obtained in step S5 in sequence to obtain polyhedral micro-nano copper powder.

2. The method for preparing polyhedral micro-nano copper powder according to claim 1, Features: In the step S2, the pH value of the initial reduction solution is 8-13.

3. The method for preparing polyhedral micro-nano copper powder according to claim 2, Features: In step S3, the reduction reaction temperature is 70-100° C., and the reduction reaction time is 0.5-3 h.

4. The method for preparing polyhedral micro-nano copper powder according to claim 3, Features: In step S4, the pH value of the reduction-protection solution is 2-5.

5. The method for preparing polyhedral micro-nano copper powder according to claim 4, Features: In step S1, the concentration of the copper oxide suspension is 0.2-5 mol / L.

6. The method for preparing polyhedral micro-nano copper powder according to claim 5, Features: In step S5, the reduction reaction temperature is 70-100° C., and the reduction reaction time is 0.5-3 h.

7. The method for preparing polyhedral micro-nano copper powder according to claim 6, Features: The reducing agent is ascorbic acid, and the mass ratio of the reducing agent to the copper element in copper oxide is between 1:2 and 6:

1.

8. The method for preparing polyhedral micro-nano copper powder according to claim 7, Features: The protective agent is selected from one of polyvinyl pyrrolidone, sorbitol, sodium citrate or a combination of at least two thereof, and the mass ratio of the protective agent to the copper element in copper oxide is between 1:1 and 10:

1.

9. The method for preparing polyhedral micro-nano copper powder according to claim 8, Features: The alkaline solution is selected from a sodium hydroxide aqueous solution, a potassium hydroxide aqueous solution, or a combination of the two, and the concentration of the alkaline solution is 0.1-5 mol / L.

10. The method for preparing polyhedral micro-nano copper powder according to claim 9, Features: In step S6, the drying is vacuum freeze drying, and the drying time is 6-18 hours.