Welding wire for improving low-temperature impact performance of welding seam and application of welding wire
By optimizing the welding wire composition and welding process, the problem of unqualified low-temperature impact performance of 09MnNiD steel welds under extreme low-temperature conditions was solved, and the high-low-temperature impact toughness of the welds at -70℃ was improved, satisfying the compressor housing. Low temperature operating conditions require.
Patent Information
- Application Number
- CN202411169208.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-26
AI Technical Summary
Under extreme low temperature conditions, the low-temperature impact performance of the weld of 09MnNiD steel is unqualified, resulting in the compressor case being unable to meet the needs of low-temperature operating conditions. It is mainly due to the burn-out of alloy elements and poor cast structure performance due to the welding heat process.
Optimized wire components (C≤0.12%, Mn0.85~1.30%, Si0.35~0.40%, S≤0.002%, P≤0.003%, Ni3.50%~3.75%, Cu≤0.35%, Mo0. 005~0.010%, Cr0.030~0.040%, V≤0.010%) and welding process, including melting electrode gas protection arc welding, preheating, controlling welding line energy, interlayer temperature and stress relief treatment after welding to ensure weld seams High and low temperature impact toughness at -70°C.
The low-temperature impact performance of the weld is significantly improved. The impact power value of the weld is ≥90J at -70℃, and the average impact power value is 106~108J, which meets the low-temperature working conditions of the compressor case.
Smart Images

Figure CN119016935A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of welding technology, and in particular to a welding wire for improving the low-temperature impact performance of a weld and an application thereof. Background Art
[0002] 09MnNiD steel is a commonly used steel for compressor casings and is also a frequently used steel in the entire structural steel industry. It is generally used in low-temperature conditions and has excellent welding performance. The national standard stipulates that -70℃ is its extreme use temperature. The compressor casings of our factory are often used in extreme temperatures during use. In our performance test of the weld, we found that when the material is used at the extreme temperature, the low-temperature toughness of the weld position will be unqualified, and the impact energy is about 20 to 25J.
[0003] After analyzing the reasons, we found that the compressor casing assembly we used was large and the weld was thick, reaching 280mm. For the welded joints, a large amount of welding heat process will cause the burning of alloy elements in the welding materials, which is not conducive to the transition of alloy elements to the weld. In addition, the welding structure belongs to the cast structure, and the performance is worse than that of the parent material. In addition, when the material is around -70℃, it is close to its low-temperature brittle transition temperature, and it is easy to undergo brittle transition, which greatly reduces the low-temperature impact performance of the material weld. Therefore, when using conventional welding technology to weld thicker compressor casings, it is difficult to achieve a 100% pass rate for low-temperature impact toughness of the weld.
[0004] Such low-temperature impact toughness cannot meet the requirements of low-temperature working conditions of the compressor casing. Summary of the invention
[0005] The present invention aims to solve at least one of the technical problems existing in the prior art or related art.
[0006] To this end, the first aspect of the present invention provides a welding wire for improving the low-temperature impact performance of a weld, wherein the components thereof are, by mass percentage, C≤0.12%, Mn0.85~1.30%, Si0.35~0.40%, S≤0.002%, P≤0.003%, Ni3.50%~3.75%, Cu≤0.35%, Mo0.005~0.010%, Cr0.030~0.040%, V≤0.010%, and the remainder are iron and unavoidable elements.
[0007] Furthermore, its composition by mass percentage is: C≤0.05%, Mn0.85~0.9%, Si0.38~0.40%, S≤0.002%, P≤0.003%, Ni3.55%~3.60%, Cu≤0.10%, Mo0.005~0.006%, Cr0.030~0.035%, V≤0.008%, and the rest are iron and unavoidable elements.
[0008] The second aspect of the present invention provides the application of the welding wire for improving the low temperature impact performance of the weld, which is used for welding ultra-thick plates of 09MnNiD materials to improve the low temperature impact performance of the weld of the ultra-thick plates of 09MnNiD materials.
[0009] Furthermore, the method for welding the ultra-thick plate of 09MnNiD material includes: welding the ultra-thick plate of 09MnNiD material for large compressor casing.
[0010] Furthermore, the method for welding the ultra-thick plate of 09MnNiD material for large compressor casing is: using the metal electrode gas shielded arc welding method, welding with the welding wire described in the first aspect of the present invention, and controlling the welding line energy to 24-26KJ / cm.
[0011] Furthermore, the method for welding the ultra-thick plate of 09MnNiD material for large compressor casing also includes: preheating before welding, and the preheating temperature is controlled at 70-120°C.
[0012] Furthermore, the method for welding the ultra-thick plate of 09MnNiD material for large compressor casing also includes: controlling the interlayer temperature during the welding process, and the interlayer temperature is controlled at 70-150°C.
[0013] Furthermore, the method for welding the ultra-thick plate of 09MnNiD material for large compressor casing also includes: welding operation control, controlling the swing width to be less than 3mm during the welding process.
[0014] Furthermore, the method for welding ultra-thick plates of 09MnNiD material for large compressor casings also includes: stress relief treatment after welding, the temperature is 580-620°C, the insulation time is t / 24-26 hours, and the value of t is the maximum thickness of the welded workpiece.
[0015] Furthermore, the welding of the ultra-thick plate of 09MnNiD material for large compressor casing has a weld with an impact energy value of ≥90J at -70°C and an average impact energy value of 106 to 108J.
[0016] Compared with the prior art, the present invention has at least the following beneficial effects:
[0017] The welding wire for improving the low-temperature impact performance of the weld provided by the present invention improves the low-temperature impact performance of the weld by adjusting and optimizing the welding wire composition. The welding wire is used for welding ultra-thick plate casings of large compressors made of 09MnNiD material, thereby improving the low-temperature impact toughness and stability of the welds of the casings of large compressors made of 09MnNiD material. The formed weld has an impact energy value of ≥90J at -70°C, and an average impact energy value of 106-108J. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the detailed description of the preferred embodiments below. The accompanying drawings are only for the purpose of illustrating the preferred embodiments and are not to be considered as limiting the present application. Also, the same reference symbols are used throughout the accompanying drawings to represent the same components. In the accompanying drawings:
[0019] Figure 1 A schematic diagram of the welding groove and assembly provided in an embodiment of the present application.
[0020] Figure 2 This is a test plate sampling diagram provided for the embodiments of the present application.
[0021] Figure 3 This is a weld structure diagram of a conventional welding method of comparative example 1 provided in the embodiments of the present application.
[0022] Figure 4 This is a weld structure diagram after the welding line energy is adjusted in the comparative example 2 provided in the embodiment of the present application.
[0023] In the attached Figure 2 Among them, 1. discarded sample; 2. tensile specimen; 3. side bending specimen; 4. weld impact specimen; 5. metallographic specimen; 6. hardness specimen; 7. parent material impact specimen; 8. test plate weld. DETAILED DESCRIPTION
[0024] In order to better understand the above-mentioned technical scheme, the technical scheme of the embodiments of the present application is described in detail below through the accompanying drawings and specific embodiments. It should be understood that the embodiments of the present application and the specific features in the embodiments are detailed descriptions of the technical scheme of the embodiments of the present application, rather than limitations on the technical scheme of the present application. In the absence of conflict, the embodiments of the present application and the technical features in the embodiments may be combined with each other.
[0025] According to a first aspect of an embodiment of the present invention, a welding wire is provided for improving the low-temperature impact performance of a weld, wherein the components thereof are, by mass percentage, C≤0.12%, Mn0.85-1.30%, Si0.35-0.40%, S≤0.002%, P≤0.003%, Ni3.50%-3.75%, Cu≤0.35%, Mo0.005-0.010%, Cr0.030-0.040%, V≤0.010%, and the remainder are iron and unavoidable elements. Preferably, its composition, by mass percentage, is: C≤0.05%, Mn0.85~0.9%, Si0.38~0.40%, S≤0.002%, P≤0.003%, Ni3.55%~3.60%, Cu≤0.10%, Mo0.005~0.006%, Cr0.030~0.035%, V≤0.008%, and the rest are iron and unavoidable elements.
[0026] In this technical solution, firstly, Ni is an important element that affects the low-temperature impact properties, so we adjusted the Ni content in the welding wire formula. Second, due to the influence of low-melting-point elements on the low-temperature impact properties of welds, the content of low-melting-point elements should be strictly controlled in the welding wire. Third, considering the influence of the Si element, the increase of the Si element will increase the fluidity of the molten weld metal, but due to the generation of non-metallic slag inclusions, the impact toughness will decrease. Fourth, compared with considering a certain element alone, what is more important is the ratio of the two elements, such as the Mn / Si and Mn / S ratios. It should be pointed out that, calculated as a percentage by mass, the content ratio of Mn / Si is greater than 2. The present invention has found that a value of Mn / Si greater than 2 can effectively guarantee impact toughness.
[0027] Finally, through a large number of cladding metal performance tests, the alloy composition of the entire welding wire cladding metal was optimized based on the test results. The main adjustments and principles are as follows:
[0028] 1. Comprehensively adjust the content of Ni, Si, S, P, and Mn alloys: Increase the content of Ni element and adjust the Ni content to 3.5% to 3.75%. The Si content is adjusted to 0.38-0.40%, the S and P contents are adjusted to less than 0.003%, and the Mn content is 0.85-1.30%. The specific principles are as follows: The addition of Ni element helps to increase the content of austenite in the weld, and the effect of Ni element is more significant than that of Mn element. When Ni and Mn elements are added at the same time, the increase in the content of austenite in the weld is more significant. The main reason is that Ni element is an austenite forming and stabilizing element, which can reduce the As and Ms points of steel, increase the chemical stability of the reverse austenite in the weld, and increase the content. The austenitizing effect of Ni element is more significant than that of Mn element, because the increase of reverse austenite is related to the migration of Ni element. When the tempering temperature rises to slightly above the As point, the core of the reverse austenite phase is directly generated in the high Ni zone by shearing, and grows longitudinally along the lath interface into extremely fine needle-shaped reverse austenite. The Ni content has a great influence on the low-temperature impact toughness. The steel of this material is delivered in a normalized state, and the organization is ferrite + a small amount of pearlite. Ni can strengthen the ferrite matrix and refine the pearlite in the steel, which can improve the plasticity and toughness of the material while improving its strength. It is important that Ni can also reduce the low-temperature brittle transition temperature of the steel. In addition, reducing the content of Si in the welding material, the silicon element will increase the non-metallic slag inclusions in the weld, thereby reducing the low-temperature impact performance. At the same time, reducing the content of S and P elements, P element is a harmful element that aggravates the brittleness of steel cooling transformation, S element has a strong affinity with Ni element, and is easy to produce low melting point alloys, reducing the low-temperature impact performance. Through strict control, the content of elements that affect the harmful low-temperature impact in the welded joint is minimized, thereby improving the impact toughness of the welded joint under low-temperature conditions.
[0029] 2. Precise control of other auxiliary elements. First, adding a small amount of auxiliary element Mo can reduce the brittle transition temperature and improve toughness. The increase in Mo content is not good for toughness. At the same time, appropriately increase Cr, Cr and Mo work at the same time, which does not affect toughness while strengthening. Secondly, more strictly control the content of V. V element, especially during the post-weld heat treatment process, will produce coherent carbides, which will reduce impact toughness.
[0030] The second aspect of the embodiment of the present invention provides the application of the above-mentioned welding wire for improving the low-temperature impact performance of the weld, which is used for welding ultra-thick plates of 09MnNiD materials to improve the low-temperature impact performance of the welds of ultra-thick plates of 09MnNiD materials. Ultra-thick plates refer to plates with a thickness greater than 200 mm.
[0031] In some embodiments, the method for welding the ultra-thick plate of 09MnNiD material includes welding the ultra-thick plate of 09MnNiD material for large compressor casing. The welding method of the ultra-thick plate of 09MnNiD material for large compressor casing is: using the metal electrode gas shielded arc welding method, the above-mentioned welding wire is used for welding, and the welding line energy is controlled to be 24-26KJ / cm.
[0032] In this technical solution, a consumable gas shielded arc welding method and the welding wire are used to control the welding line energy to 24-26KJ / cm, and the 09MnNiD material ultra-thick plate for large compressor casing is welded. The thickness of the 09MnNiD material ultra-thick plate for large compressor casing is greater than 200mm, and the maximum thickness can reach 332mm. It is further suitable for the 09MnNiD material ultra-thick plate for large compressor casing with a thickness range of 250-332mm, and further suitable for the 09MnNiD material ultra-thick plate for large compressor casing with a thickness range of 280-332mm. In practice, it is widely used in the welding of 09MnNiD material ultra-thick plates for large compressor casings with a thickness range of 250-280mm, which improves the low-temperature impact toughness and stability of the weld. The formed weld has an impact energy value of ≥90J at -70°C, and an average impact energy value of 106-108J. After many tests, it was confirmed that when the thickness of the ultra-thick plate of 09MnNiD material used for the casing of large compressors in our factory was 280mm, the consumable gas shielded arc welding method was adopted, and the above-mentioned welding wire was used for welding, and the welding line energy was controlled to be 24-26KJ / cm. The impact energy value of the formed weld was ≥90J at -70℃, and the average impact energy value was 106-108J. Since 09MnNiD material is a commonly used steel grade, and the welding process is relatively mature and welding defects are not easy to occur, in order to improve production efficiency, the welding line energy often used is very large. This is completely no problem under general use conditions, but on the casing of large compressors, the overall heat input is very large. When used at the critical low temperature, that is, -70℃, excessive welding current and voltage will cause alloy element burnout, coarse weld structure and other phenomena, which is not conducive to the impact performance of the weld. After experimental summary and metallographic structure analysis, it was finally found that when the line energy was controlled at 24-26KJ / cm, the microstructure of the weld was the most uniform and fine. When the line energy is lower than 24KJ / cm, the weld production efficiency is low, the welding process is short-circuited, and the spraying is not achieved, which affects the welding quality; when the line energy is greater than 26KJ / cm, the weld structure is very easy to be coarse. Therefore, it is most appropriate to control the welding line energy to 24~26KJ / cm.
[0033] In some embodiments, the method for welding ultra-thick plates of 09MnNiD material for large compressor casings also includes: preheating before welding, and the preheating temperature is controlled at 70-120°C.
[0034] In this technical solution, proper preheating will slow down the cooling rate of welding, which is conducive to ensuring that the weld produces uniform and fine structures, which will have a good effect on impact toughness. In addition, for plates with extra-large thickness, proper preheating will reduce the sensitivity of material cracks, which is conducive to ensuring the quality of the weld.
[0035] In some embodiments, the method for welding ultra-thick plates of 09MnNiD material for large compressor casings further includes: controlling the interlayer temperature during welding, and the interlayer temperature is controlled at 70-150°C.
[0036] In this technical solution, appropriate interlayer temperature is conducive to ensuring the quality of the weld. If the interlayer temperature is too high, the structure of the weld and the heat-affected zone will be coarse, which will lead to reduced impact performance. If the interlayer temperature is too low, falling below the preheating temperature, the crack tendency of the weld will increase.
[0037] In some embodiments, the method for welding ultra-thick plates of 09MnNiD material for large compressor casings also includes: welding operation control, controlling the swing width to be less than 3 mm during the welding process.
[0038] In this technical solution, for the welding of low-temperature steel, the swing should be appropriately reduced during the welding process, and the swing width range is allowed to be less than 3 mm. This is conducive to fine weld structure, thereby improving the impact performance of the weld.
[0039] In some embodiments, the method for welding ultra-thick plates of 09MnNiD material for large compressor casings also includes: stress relief treatment after welding, the temperature is 580-620°C, the insulation time is t / 24-26 hours, and the value of t is the maximum thickness of the welded workpiece.
[0040] In this technical solution, the stress relief temperature should be controlled at A C 1 below a certain temperature, it can refine the grains and eliminate the internal stress caused by welding. Too low a temperature will affect the effect of refining the grains and eliminating stress. Too high a temperature may cause graphitization of pearlite, which will reduce the performance of the weld. The holding time is controlled at t / 24 to 26 hours. Shortening the time will lead to uneven temperature inside and outside the workpiece and poor heat treatment effect. Too long a time will lead to energy waste.
[0041] In some embodiments, when the weld of the ultra-thick plate made of 09MnNiD material for large compressor casing is at -70°C, the impact energy value is ≥90J, and the average impact energy value is 106-108J.
[0042] Specifically, the welding wire has the following components by mass percentage: C≤0.12%, Mn0.85~1.30%, Si0.35~0.40%, S≤0.002%, P≤0.003%, Ni3.50%~3.75%, Cu≤0.35%, Mo0.005~0.010%, Cr0.030~0.040%, V≤0.010%, and the rest are iron and unavoidable elements. The welding line energy is controlled at 24~26KJ / cm, the impact energy value of the weld at -70℃ is ≥90J, and the average impact energy value is 106~108KJ / cm.
[0043] The welding wire for improving the low temperature impact performance of the weld and its application of the present invention are discussed below through specific embodiments, as well as embodiment 1, comparative example 1 and comparative example 2.
[0044] The experimental equipment of the embodiments and comparative examples of the present invention include: OTC XD600 welding machine, WDW-3100 multifunctional testing machine, ZWICK RKP450 impact testing machine, KPE3000 hardness testing machine, JB30B impact testing machine, MM6 metallographic microscope, and pit-type heat treatment furnace.
[0045] The test material is 09MnNiD, and the chemical composition of the material is shown in Table 1 (national standard). We use welding test plates to verify the performance of the weld. The test plate size used in the experiment is 500mmX400mmX250mm (two test plates of 500mmX200mmX250mm are welded together). The test plate groove is R15+12°U-shaped, with a blunt edge of 3mm and an assembly gap of 3mm. The welding groove and assembly diagram are shown in Figure 1 .
[0046] Table 1 Chemical composition of 09MnNiD material according to national standard
[0047] Brand C Mn Si Ni Nb S P 09MnNiD ≤0.12 1.2~1.6 0.15~0.50 0.3~0.8 ≤0.040 ≤0.008 ≤0.020
[0048] The present invention has carried out metal electrode gas shielded arc welding (GMAW), stress relief in the furnace, ultrasonic nondestructive testing, and layered sampling inspection on the 09MnNiD material test plate. The sampling diagram of each layer of the test plate is shown in FIG. Figure 2 As shown, it includes: discarded sample 1, tensile specimen 2, side bending specimen 3, weld impact specimen 4, metallographic specimen 5, hardness specimen 6, parent material impact specimen 7. The weld position is shown as test plate weld 8. The test items include yield strength, tensile strength, bending, -70℃ impact work, and the test plate thickness is 250mm.
[0049] We conducted multiple sets of welding process evaluation experiments on 09MnNiD material using different process methods. Finally, we found that under different welding process conditions, the strength (yield strength, tensile strength), bending test, and hardness test values of the test plates were all qualified, but the low-temperature impact energy varied greatly.
[0050] The low temperature impact performance of the compressor casing weld of 09MnNiD material is discussed below through Example 1, Comparative Example 1 and Comparative Example 2.
[0051] Example 1 A welding wire for improving the low-temperature impact performance of a weld and its use in welding ultra-thick plates of 09MnNiD material for large compressor casings.
[0052] The welding wire of Example 1: C≤0.12%, Mn0.85~1.30%, Si0.35~0.40%, S≤0.003%, P≤0.003%, Ni3.50%~3.75%, Cu≤0.35%, Mo0.005~0.010%, Cr0.030~0.040%, V0.008~0.010%.
[0053] The welding method of embodiment 1:
[0054] (1) Preheating: preheat the 09MnNiD material at 80°C.
[0055] (2) Welding: gas metal arc welding is adopted, and the welding wire of Example 1 is used for welding. The welding line energy is controlled to be 24-26 kJ / cm, the interlayer temperature is controlled to be not higher than 150° C. and not lower than the preheating temperature, and the swing during the welding process is reduced, and the swing width range is allowed to be less than 3 mm.
[0056] (3) Stress relief treatment after welding, the temperature is 580 ~ 620 ° C, the time is t / 25 hours, and the t value is equal to the maximum thickness of the welded workpiece.
[0057] Comparative Example 1 Conventional welding wire and conventional welding method used to weld ultra-thick plates of 09MnNiD material for large compressor casings.
[0058] The difference between Comparative Example 1 and Example 1 lies in the welding wire and the welding method, which are as follows:
[0059] Welding wire of comparative example 1: According to the standard, the welding material corresponding to the 09MnNiD material is ASTMA5.28 ER80S-Ni3 (conventional welding wire), which specifies the content range of alloy elements C, Mn, Si, S, P, Ni, and Cu in the welding wire cladding metal. See Table 2 for details.
[0060] Table 2 Chemical composition of welding wire deposited metal by mass percentage
[0061]
[0062] Welding method of comparative example 1 (conventional welding method):
[0063] (1) Preheating, same as in Example 1.
[0064] (2) Welding: The difference from Example 1 is that the welding wire of Comparative Example 1 is used for welding, and the welding line energy is controlled to be 27-31.5 KJ / cm.
[0065] (3) Stress relief treatment after welding is the same as in Example 1.
[0066] Comparative Example 2 Conventional welding wire and improved welding method thereof are used to weld ultra-thick plates of 09MnNiD material for large compressor casings.
[0067] The difference between Comparative Example 2 and Example 1 lies in the welding wire. The welding wire of Comparative Example 2 is the same as that of Comparative Example 1, and the welding method of Comparative Example 2 is the same as that of Example 1.
[0068] Results and Discussion:
[0069] The impact energy values of the welds of Example 1, Comparative Example 1 and Comparative Example 2 are shown in Table 3:
[0070] Table 3 Impact test data
[0071] project -70℃ impact value(J) Comparative Example 1 (Conventional Welding Method and Conventional Welding Wire) 26 / 19 / 22 / 21 / 25 / 16 / 21 / 23 / 22 Comparative Example 2 (Improved Welding Method and Conventional Welding Wire) 59 / 41 / 46 / 35 / 43 / 55 / 62 / 55 / 58 Embodiment 1 (Improving welding method and adjusting welding wire composition) 90 / 98 / 118 / 100 / 120 / 116 / 112 / 112 / 96
[0072] It can be seen from the impact test data of Comparative Examples 1 and 2 that after the linear energy is adjusted, the impact value of the weld at -70°C is increased from an average value of 21.7J and a minimum value of 16J to an average value of 50.4J and a minimum value of 35J. Such impact toughness is basically qualified, but the value is not too high. Since the low-temperature performance of the parent material is qualified and only the low-temperature performance of the weld is unqualified, in order to improve the operating stability of the compressor unit, we have deeply explored the influence of the welding material composition on the impact work of the weld. It can be seen from Example 1 that after the linear energy and the composition of the welding wire are adjusted, the impact value of the weld at -70°C is increased to an average value of 106.9 and a minimum value of 90J.
[0073] Comparative Example 1 The weld structure of the conventional welding method is as follows Figure 3 As shown, the weld structure of the improved welding method of comparative example 2 (after adjusting the line energy) is as follows Figure 4 It should be noted that the weld structure diagram is significantly affected by the amount of line energy. Figure 3 It can be seen that the conventional welding method ( Figure 3 ) Welding seam structure improved welding method ( Figure 4 ) has obvious growth and irregular distribution, which proves that under large line energy, due to the increase of original heat input, the residence time in the high temperature zone becomes longer and the cooling rate becomes slower, which leads to the increase of non-equilibrium transformation organization and grain growth. Figure 4 The ferrite matrix of the weld is uniform and fine, with a large amount of acicular ferrite. The acicular ferrite is distributed at a large angle, avoiding the coarse structure and small heat input, which can avoid alloy burning and is beneficial to improving the low-temperature impact performance of the weld.
[0074] In summary, after multiple groups of experimental demonstrations, it was found that according to the method of improving the low-temperature impact performance of the weld according to the present invention, after controlling the line energy and adjusting the welding wire composition, the -70°C impact performance of the weld of the 09MnNiD material was greatly improved, from a small amount of unqualified to all qualified. After the optimization of the line energy, the average value of the -70°C impact energy was 50.4J (minimum 35J), and after further optimization of the welding wire composition, the average value of the -70°C impact energy reached 106.9J (minimum 90J). After multiple tests and demonstrations, the stability is good, and there has never been a situation lower than 90J, which fully meets the standard regulations and use requirements.
[0075] The present invention adjusts the proportion of alloy elements in the welding wire, adjusts the welding heat input, combines the control of preheating temperature and interlayer temperature, welding operation requirements and post-weld stress relief heat treatment process, and ultimately greatly improves the low-temperature impact toughness of 09MnNiD material under critical conditions (-70°C). The low-temperature use safety and stability of the unit are guaranteed. A new technical model is provided for improving the welding performance of the compressor casing and 09MnNiD material used at -70°C. The present invention has been applied to the welding of compressor casings in many large projects such as the Lanzhou Petrochemical Project, Tarim Project, Guangzhou Petrochemical Project, Hainan Petrochemical Project, and Ningxia Baofeng Project of Shenyang Blower Group, with good feedback and improved casing safety and quality. The method involved in the present invention is simple and easy to implement, providing a feasible direction for the use of 09MnNiD materials in low-temperature conditions in other industries.
[0076] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0077] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A welding wire for improving the low temperature impact performance of a weld, characterized in that: Its composition by mass percentage is: C≤0.12%, Mn0.85~1.30%, Si0.35~0.40%, S≤0.002%, P≤0.003%, Ni3.50%~3.75%, Cu≤0.35%, Mo0.005~0.010%, Cr0.030~0.040%, V≤0.010%, and the rest are iron and unavoidable elements.
2. The welding wire for improving low temperature impact performance of welds according to claim 1, characterized in that: Its composition by mass percentage is: C≤0.05%, Mn0.85~0.9%, Si0.38~0.40%, S≤0.002%, P≤0.003%, Ni3.55%~3.60%, Cu≤0.10%, Mo0.005~0.006%, Cr0.030~0.035%, V≤0.008%, and the rest are iron and unavoidable elements.
3. An application of welding wire for improving low temperature impact performance of welds, characterized in that: The welding wire for improving the low-temperature impact performance of the weld as described in claim 1 or 2 is used for welding ultra-thick plates of 09MnNiD materials to improve the low-temperature impact performance of the weld of the ultra-thick plates of 09MnNiD materials.
4. The use of the welding wire for improving the low temperature impact performance of the weld according to claim 3, characterized in that: The method for welding the ultra-thick plate made of 09MnNiD material includes: the method for welding the ultra-thick plate made of 09MnNiD material for a large compressor casing.
5. The use of the welding wire for improving the low temperature impact performance of the weld according to claim 4, characterized in that: The method for welding the ultra-thick plate of 09MnNiD material for large compressor casing is as follows: The method adopts the metal electrode gas shielded arc welding method, adopts the welding wire described in claim 1 or 2 to carry out welding, and controls the welding line energy to be 24-26 KJ / cm.
6. The use of the welding wire for improving the low temperature impact performance of the weld according to claim 5, characterized in that: The method for welding the ultra-thick plate of 09MnNiD material for a large compressor casing also includes: Preheat before welding, and control the preheating temperature at 70-120℃.
7. The use of the welding wire for improving the low temperature impact performance of the weld according to claim 5, characterized in that: The method for welding the ultra-thick plate of 09MnNiD material for a large compressor casing also includes: The interlayer temperature is controlled during the welding process, and the interlayer temperature is controlled at 70-150℃.
8. The use of the welding wire for improving the low temperature impact performance of the weld according to claim 5, characterized in that: The method for welding the ultra-thick plate of 09MnNiD material for a large compressor casing also includes: Welding operation control, control the swing width during welding to less than 3mm.
9. The use of the welding wire for improving the low temperature impact performance of the weld according to claim 5, characterized in that: The method for welding the ultra-thick plate of 09MnNiD material for a large compressor casing also includes: After welding, stress relief treatment is carried out at a temperature of 580-620°C and a holding time of t / 24-26 hours, where the value of t is the maximum thickness of the welded workpiece.
10. The use of the welding wire for improving the low temperature impact performance of the weld according to claim 5, characterized in that: The welding method is used for welding the ultra-thick plate of 09MnNiD material for large compressor casings. The formed weld has an impact energy value of ≥90J at -70°C, and an average impact energy value of 106-108J.