Bearing double-end forming and cold rolling expansion manufacturing process
Through the double-end molding and cold-rolling expansion manufacturing process, chemical composition and heat treatment are optimized, and the problem of insufficient stability and durability of bearings under impact loads is solved, and the high toughness and fatigue durability of bearings are significantly improved.
Patent Information
- Application Number
- CN202411135808.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The bearings are instable in stability and durability when subjected to impact loads, and it is difficult for existing manufacturing processes to effectively improve their mechanical properties and fatigue life.
The bearing double-end molding and cold-grinding expansion manufacturing process is adopted, including smelting casting, double-face symmetric forging, diffusion annealing, heat treatment and other steps, optimize the chemical composition, reduce the aluminum content, introduce magnesium, form fine intermetallic compounds, and pass through europium, The synergistic action of cobalt maintains the stability of intermetallic compounds.
It significantly improves the fatigue durability and overall toughness of the bearing, improves the thermal processing performance, reduces the brittle phase, and enhances the mechanical properties of the bearing.
Smart Images

Figure BDA0004999395760000091 
Figure BDA0004999395760000101
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of bearing preparation, and in particular relates to a bearing double-end forming and cold rolling manufacturing process. Background Art
[0002] The main function of automobile wheel hub bearings is to bear weight and provide precise guidance for the rotation of the wheel hub. It bears both axial and radial loads and is a very important component. With the rapid development of the automobile industry, the performance and manufacturing efficiency of bearings have become key factors in improving vehicle performance and reducing costs. Bearings may encounter impact loads during operation, such as when starting, stopping or when the load changes suddenly. Their stability and durability are particularly critical. Therefore, optimizing the manufacturing process of bearings and improving the mechanical properties and fatigue life of bearings have become important research directions in the field of bearing preparation technology. Summary of the invention
[0003] The purpose of the present invention is to provide a bearing double-end forming and cold rolling manufacturing process for improving the toughness and fatigue durability of the bearing.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A bearing double-end forming and cold rolling manufacturing process, comprising the following steps:
[0006] S1. Performing double-sided symmetrical forging on the steel billet after smelting and casting to obtain a forged steel billet;
[0007] S2. The forged steel billet is designed into a bearing ring joint cold-rolled part according to the finished product size of the target bearing ring, and then blanked, upset, formed, punched, cold-rolled and formed using a cold rolling die, heat treated, ground and polished to obtain a finished bearing.
[0008] As a preferred technical solution of the present invention, the smelting and casting refers to melting, casting and diffusion annealing the raw materials in a vacuum furnace at a rated power of 50kW, an operating voltage of 260V and a smelting temperature of 1650-1720°C to obtain a steel billet after smelting and casting.
[0009] As a preferred technical solution of the present invention, the double-sided symmetrical forging includes the following steps:
[0010] S11, placing the steel billet after smelting and casting in a preheating furnace for preheating treatment to eliminate internal stress, improve the forgeability of the material, and make the structure more uniform;
[0011] S12, the preheated steel billet is moved to the forging machine, and pressure is applied simultaneously in a double-sided symmetrical manner for rough forging. Through large deformation forging, the cast structure in the steel billet is further broken, the grains are refined, and the basic shape of the bearing is initially formed. During the forging process, the forging temperature is strictly controlled to be in the range of 900-1100°C to avoid structural defects caused by overheating or overcooling;
[0012] S13. After the rough forging is completed, the steel billet is put back into the annealing furnace for intermediate annealing treatment, which aims to eliminate the internal stress generated during the rough forging process and further homogenize the structure to prepare for the subsequent fine forging;
[0013] S14, double-sided symmetrical precision forging: After intermediate annealing, the plasticity and toughness of the steel billet are significantly improved. At this time, double-sided symmetrical precision forging is carried out. During the precision forging process, the concentricity and parallelism of the inner and outer rings of the bearing are kept consistent to ensure product quality and obtain the forged steel billet.
[0014] As a preferred technical solution of the present invention, the diffusion annealing refers to heating to 1250-1280°C at 5°C / min and keeping the temperature for 10-20h.
[0015] As a preferred technical solution of the present invention, the heat treatment in step S2 includes an annealing process and a tempering process.
[0016] As a preferred technical solution of the present invention, the process parameters of the annealing process are heating at a temperature of 820-920°C for a holding time of 3-5h, furnace cooling to 600°C and air cooling after exiting the furnace.
[0017] As a preferred technical solution of the present invention, the process parameters of the tempering process are heating temperature 600-700°C, holding time 8-10h, and air cooling.
[0018] As a preferred technical solution of the present invention, the preheating treatment in step S11 refers to uniformly heating to 850-900° C. and keeping the temperature for 2-3 hours.
[0019] As a preferred technical solution of the present invention, the temperature of the intermediate annealing in step S13 is 750-800° C., and the holding time is 2-4 hours.
[0020] As a preferred technical solution of the present invention, the chemical composition of the steel billet is calculated according to the weight percentage of the element components, and its chemical composition is as follows:
[0021] C: 0.12-0.19%; Al: 0.011-0.014%; Mg: 0.018-0.028%; Mn: 0.35-0.38%; Cr: 4.4-4.8%; Mo: 1.401-1.405%; V: 0.98-1.02%; Co: 0.024-0.026%; Eu: 0.012-0.013%; the rest are Fe and unavoidable impurity elements.
[0022] Beneficial effects of the present invention:
[0023] The double-end forming and cold rolling manufacturing process of a bearing disclosed in the present invention optimizes the chemical composition, reduces the aluminum content, introduces magnesium, and forms fine and evenly distributed intermetallic compounds, which can effectively withstand alternating loads, thereby improving the fatigue durability of the bearing and reducing the brittle phase in the steel, thereby improving the overall toughness of the bearing steel and improving its hot processing performance; at the same time, the synergistic effect between europium and cobalt in the bearing steel components can maintain the stability of the intermetallic compounds, effectively resist the initiation and expansion of fatigue cracks, thereby significantly improving the fatigue durability of the bearing, and the synergistic effect of cobalt and europium helps to form a uniform metallographic structure, reduce the heterogeneity of the structure, and thus improve the overall performance of the bearing. DETAILED DESCRIPTION
[0024] In order to further illustrate the technical means and effects adopted by the present invention to achieve the predetermined invention purpose, the specific implementation methods, structures, features and effects of the present invention are described in detail below in combination with the embodiments.
[0025] Example 1
[0026] A bearing double-end forming and cold rolling manufacturing process, comprising the following steps:
[0027] S1. Performing double-sided symmetrical forging on the steel billet after smelting and casting to obtain a forged steel billet;
[0028] S2. The forged steel billet is designed into a bearing ring joint cold-rolled part according to the finished product size of the target bearing ring, and then blanked, upset, formed, punched, cold-rolled and formed using a cold rolling die, heat treated, ground and polished to obtain a finished bearing.
[0029] The smelting and casting in step S1 refers to smelting, casting, and diffusion annealing the raw materials in a vacuum furnace at a rated power of 50kW, an operating voltage of 260V, and a smelting temperature of 1650°C to obtain a steel billet after smelting and casting; the diffusion annealing refers to heating to 1250°C at 5°C / min and keeping warm for 10 hours.
[0030] The two-sided symmetrical forging in step S1 includes the following steps:
[0031] S11, placing the steel billet after smelting and casting in a preheating furnace for preheating treatment; the preheating treatment refers to uniformly heating to 850° C. and keeping the temperature for 2 hours;
[0032] S12, moving the preheated steel billet to a forging machine, and performing rough forging in a double-sided symmetrical manner;
[0033] S13, after the rough forging is completed, the steel billet is put back into the annealing furnace for intermediate annealing treatment; the intermediate annealing temperature is 750°C and the holding time is 2h;
[0034] S14. After intermediate annealing, the steel billet is subjected to double-sided symmetrical finish forging to obtain a forged steel billet.
[0035] The heat treatment in step S2 includes an annealing process and a tempering process: the process parameters of the annealing process are heating at a temperature of 820°C for a holding time of 3 hours, furnace cooling to 600°C, and air cooling; the process parameters of the tempering process are heating at a temperature of 600°C for a holding time of 8 hours and air cooling.
[0036] The chemical composition of the steel billet is calculated according to the weight percentage of the element components as follows:
[0037] C: 0.12%; Al: 0.011%; Mg: 0.018%; Mn: 0.35%; Cr: 4.4%; Mo: 1.401%; V: 0.98%; Co: 0.024%; Eu: 0.012%; the rest are Fe and unavoidable impurity elements.
[0038] Example 2
[0039] A bearing double-end forming and cold rolling manufacturing process, comprising the following steps:
[0040] S1. Performing double-sided symmetrical forging on the steel billet after smelting and casting to obtain a forged steel billet;
[0041] S2. The forged steel billet is designed into a bearing ring joint cold-rolled part according to the finished product size of the target bearing ring, and then blanked, upset, formed, punched, cold-rolled and formed using a cold rolling die, heat treated, ground and polished to obtain a finished bearing.
[0042] The smelting and casting in step S1 refers to smelting, casting, and diffusion annealing the raw materials in a vacuum furnace at a rated power of 50kW, an operating voltage of 260V, and a smelting temperature of 1685°C to obtain a steel billet after smelting and casting; the diffusion annealing refers to heating to 1265°C at 5°C / min and keeping warm for 15 hours.
[0043] The two-sided symmetrical forging in step S1 includes the following steps:
[0044] S11, placing the steel billet after smelting and casting in a preheating furnace for preheating treatment; the preheating treatment refers to uniformly heating to 875° C. and keeping the temperature for 2.5 hours;
[0045] S12, moving the preheated steel billet to a forging machine, and performing rough forging in a double-sided symmetrical manner;
[0046] S13, after the rough forging is completed, the steel billet is put back into the annealing furnace for intermediate annealing treatment; the intermediate annealing temperature is 775°C and the holding time is 3h;
[0047] S14. After intermediate annealing, the steel billet is subjected to double-sided symmetrical finish forging to obtain a forged steel billet.
[0048] The heat treatment in step S2 includes an annealing process and a tempering process: the process parameters of the annealing process are heating at a temperature of 870°C, holding time of 4 hours, furnace cooling to 600°C, and air cooling; the process parameters of the tempering process are heating at a temperature of 650°C, holding time of 9 hours, and air cooling.
[0049] The chemical composition of the steel billet is calculated according to the weight percentage of the element components as follows:
[0050] C: 0.16%; Al: 0.0125%; Mg: 0.023%; Mn: 0.365%; Cr: 4.6%; Mo: 1.403%; V: 1.00%; Co: 0.025%; Eu: 0.0125%; the rest are Fe and unavoidable impurity elements.
[0051] Example 3
[0052] A bearing double-end forming and cold rolling manufacturing process, comprising the following steps:
[0053] S1. Performing double-sided symmetrical forging on the steel billet after smelting and casting to obtain a forged steel billet;
[0054] S2. The forged steel billet is designed into a bearing ring joint cold-rolled part according to the finished product size of the target bearing ring, and then blanked, upset, formed, punched, cold-rolled and formed using a cold rolling die, heat treated, ground and polished to obtain a finished bearing.
[0055] The smelting and casting in step S1 refers to melting, casting, and diffusion annealing the raw materials in a vacuum furnace at a rated power of 50kW, an operating voltage of 260V, and a smelting temperature of 1720°C to obtain a steel billet after smelting and casting; the diffusion annealing refers to heating to 1280°C at 5°C / min and keeping warm for 20 hours.
[0056] The two-sided symmetrical forging in step S1 includes the following steps:
[0057] S11, placing the steel billet after smelting and casting in a preheating furnace for preheating treatment; the preheating treatment refers to uniformly heating to 900° C. and keeping the temperature for 3 hours;
[0058] S12, moving the preheated steel billet to a forging machine, and performing rough forging in a double-sided symmetrical manner;
[0059] S13, after the rough forging is completed, the steel billet is put back into the annealing furnace for intermediate annealing treatment; the intermediate annealing temperature is 750-800°C, and the holding time is 2-4h;
[0060] S14. After intermediate annealing, the steel billet is subjected to double-sided symmetrical finish forging to obtain a forged steel billet.
[0061] The heat treatment in step S2 includes an annealing process and a tempering process: the process parameters of the annealing process are heating at a temperature of 920°C for a holding time of 5 hours, furnace cooling to 600°C and air cooling; the process parameters of the tempering process are heating at a temperature of 700°C for a holding time of 10 hours and air cooling.
[0062] The chemical composition of the steel billet is calculated according to the weight percentage of the element components as follows:
[0063] C: 0.19%; Al: 0.014%; Mg: 0.028%; Mn: 0.38%; Cr: 4.8%; Mo: 1.405%; V: 1.02%; Co: 0.026%; Eu: 0.013%; the rest are Fe and inevitable impurity elements.
[0064] Comparative Example 1
[0065] The difference from Example 2 is that the chemical composition of the steel billet is calculated according to the weight percentage of the element components, and its chemical composition is as follows:
[0066] C: 0.16%; Al: 0.0145%; Mg: 0.023%; Mn: 0.365%; Cr: 4.6%; Mo: 1.403%; V: 1.00%; Co: 0.025%; Eu: 0.0125%; the rest are Fe and unavoidable impurity elements.
[0067] Comparative Example 2
[0068] The difference from Example 2 is that the chemical composition of the steel billet is calculated according to the weight percentage of the element components, and its chemical composition is as follows:
[0069] C: 0.16%; Al: 0.0150%; Mg: 0.023%; Mn: 0.365%; Cr: 4.6%; Mo: 1.403%; V: 1.00%; Co: 0.025%; Eu: 0.0125%; the rest are Fe and unavoidable impurity elements.
[0070] Comparative Example 3
[0071] The difference from Example 2 is that the chemical composition of the steel billet is calculated according to the weight percentage of the element components, and its chemical composition is as follows:
[0072] C: 0.16%; Al: 0.0155%; Mg: 0.023%; Mn: 0.365%; Cr: 4.6%; Mo: 1.403%; V: 1.00%; Co: 0.025%; Eu: 0.0125%; the rest are Fe and unavoidable impurity elements.
[0073] Comparative Example 4
[0074] The difference from Example 2 is that the chemical composition of the steel billet is calculated according to the weight percentage of the element components, and its chemical composition is as follows:
[0075] C: 0.16%; Al: 0.0160%; Mg: 0.023%; Mn: 0.365%; Cr: 4.6%; Mo: 1.403%; V: 1.00%; Co: 0.025%; Eu: 0.0125%; the rest are Fe and unavoidable impurity elements.
[0076] Comparative Example 5
[0077] The difference from Example 2 is that the chemical composition of the steel billet is calculated according to the weight percentage of the element components, and its chemical composition is as follows:
[0078] C: 0.16%; Al: 0.0180%; Mg: 0.023%; Mn: 0.365%; Cr: 4.6%; Mo: 1.403%; V: 1.00%; Co: 0.025%; Eu: 0.0125%; the rest are Fe and unavoidable impurity elements.
[0079] Comparative Example 6
[0080] The difference from Example 2 is that the chemical composition of the steel billet is calculated according to the weight percentage of the element components, and its chemical composition is as follows:
[0081] C: 0.16%; Al: 0.0200%; Mg: 0.023%; Mn: 0.365%; Cr: 4.6%; Mo: 1.403%; V: 1.00%; Co: 0.025%; Eu: 0.0125%; the rest are Fe and unavoidable impurity elements.
[0082] Comparative Example 7
[0083] The difference from Example 2 is that the chemical composition of the steel billet is calculated according to the weight percentage of the element components, and its chemical composition is as follows:
[0084] C: 0.16%; Al: 0.0125%; Mg: 0.030%; Mn: 0.365%; Cr: 4.6%; Mo: 1.403%; V: 1.00%; Co: 0.025%; Eu: 0.0125%; the rest are Fe and inevitable impurity elements.
[0085] Comparative Example 8
[0086] The difference from Example 2 is that the chemical composition of the steel billet is calculated according to the weight percentage of the element components, and its chemical composition is as follows:
[0087] C: 0.16%; Al: 0.0125%; Mg: 0.040%; Mn: 0.365%; Cr: 4.6%; Mo: 1.403%; V: 1.00%; Co: 0.025%; Eu: 0.0125%; the rest are Fe and unavoidable impurity elements.
[0088] Comparative Example 9
[0089] The difference from Example 2 is that the chemical composition of the steel billet is calculated according to the weight percentage of the element components, and its chemical composition is as follows:
[0090] C: 0.16%; Al: 0.0125%; Mg: 0.017%; Mn: 0.365%; Cr: 4.6%; Mo: 1.403%; V: 1.00%; Co: 0.025%; Eu: 0.0125%; the rest are Fe and unavoidable impurity elements.
[0091] Comparative Example 10
[0092] The difference from Example 2 is that the chemical composition of the steel billet is calculated according to the weight percentage of the element components, and its chemical composition is as follows:
[0093] C: 0.16%; Al: 0.0125%; Mg: 0.016%; Mn: 0.365%; Cr: 4.6%; Mo: 1.403%; V: 1.00%; Co: 0.025%; Eu: 0.0125%; the rest are Fe and unavoidable impurity elements.
[0094] Comparative Example 11
[0095] The difference from Example 2 is that the chemical composition of the steel billet is calculated according to the weight percentage of the element components, and its chemical composition is as follows:
[0096] C: 0.16%; Al: 0.0125%; Mg: 0.023%; Mn: 0.365%; Cr: 4.6%; Mo: 1.403%; V: 1.00%; Co: 0; Eu: 0.0375%; the rest are Fe and inevitable impurity elements.
[0097] Comparative Example 12
[0098] The difference from Example 2 is that the chemical composition of the steel billet is calculated according to the weight percentage of the element components, and its chemical composition is as follows:
[0099] C: 0.16%; Al: 0.0125%; Mg: 0.023%; Mn: 0.365%; Cr: 4.6%; Mo: 1.403%; V: 1.00%; Co: 0.0375%; Eu: 0; the rest are Fe and unavoidable impurity elements.
[0100] Performance Testing
[0101] The finished products obtained in Example 1 to Example 3 and Comparative Example 1 to Comparative Example 12 were subjected to comprehensive performance tests, and the test results are shown in Table 1 below.
[0102] Table 1
[0103]
[0104]
[0105] As can be seen from Table 1, the finished bearings obtained in Examples 1-3 of the present application have good toughness and fatigue durability, fine and uniform metallographic structures, and no obvious grain boundary fractures and defects. By optimizing the raw material composition, the bearing steel optimizes the chemical composition, reduces the aluminum content, introduces magnesium, forms fine and uniformly distributed intermetallic compounds, effectively withstands alternating loads, thereby improving the fatigue durability of the bearing, reducing the brittle phase in the steel, thereby improving the overall toughness of the bearing steel, and improving its hot working performance; at the same time, the synergistic effect between europium and cobalt in the bearing steel components can maintain the stability of the intermetallic compounds, effectively resist the initiation and expansion of fatigue cracks, thereby significantly improving the fatigue durability of the bearing, and the synergistic effect of cobalt and europium helps to form a uniform metallographic structure, reduce the inhomogeneity of the structure, and thus improve the overall performance of the bearing.
[0106] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technical personnel in this field can make some changes or modify the technical contents disclosed above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any brief modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution of the present invention.
Claims
1. A bearing double-end forming and cold rolling manufacturing process, It is characterized in that The following steps are involved: S1. Performing double-sided symmetrical forging on the steel billet after smelting and casting to obtain a forged steel billet; S2. The forged steel billet is designed into a bearing ring joint cold-rolled part according to the finished product size of the target bearing ring, and then blanked, upset, formed, punched, cold-rolled and formed using a cold rolling die, heat treated, ground and polished to obtain a finished bearing.
2. A bearing double-end forming and cold rolling manufacturing process according to claim 1, It is characterized in that The smelting and casting refers to melting, casting, and diffusion annealing the raw materials in a vacuum furnace at a rated power of 50 kW, a working voltage of 260 V, and a smelting temperature of 1650-1720° C. to obtain a smelted and cast steel billet.
3. A bearing double-end forming and cold rolling manufacturing process according to claim 1, It is characterized in that The two-sided symmetrical forging comprises the following steps: S11, placing the steel billet after smelting and casting in a preheating furnace for preheating treatment; S12, moving the preheated steel billet to a forging machine, and performing rough forging in a double-sided symmetrical manner; S13, after the rough forging is completed, the steel billet is put back into the annealing furnace for intermediate annealing treatment; S14. After intermediate annealing, the steel billet is subjected to double-sided symmetrical finish forging to obtain a forged steel billet.
4. A bearing double-end forming and cold rolling manufacturing process according to claim 2, It is characterized in that The diffusion annealing refers to heating to 1250-1280° C. at 5° C. / min and then keeping the temperature for 10-20 hours.
5. A bearing double-end forming and cold rolling manufacturing process according to claim 1, It is characterized in that The heat treatment in step S2 includes an annealing process and a tempering process.
6. A bearing double-end forming and cold rolling manufacturing process according to claim 5, It is characterized in that The annealing process parameters are as follows: heating at a temperature of 820-920° C. for 3-5 hours, cooling the furnace to 600° C., and air cooling after exiting the furnace.
7. A bearing double-end forming and cold rolling manufacturing process according to claim 5, It is characterized in that The tempering process parameters are heating temperature 600-700° C., holding time 8-10 hours, and air cooling.
8. A bearing double-end forming and cold rolling manufacturing process according to claim 3, It is characterized in that The preheating treatment in step S11 refers to uniformly heating to 850-900° C. and keeping the temperature for 2-3 hours.
9. A bearing double-end forming and cold rolling manufacturing process according to claim 3, It is characterized in that The intermediate annealing temperature in step S13 is 750-800° C., and the holding time is 2-4 hours.
10. A bearing double-end forming and cold rolling manufacturing process according to claim 1, It is characterized in that The chemical composition of the steel billet is calculated according to the weight percentage of the element components as follows: C: 0.12-0.19%; Al: 0.011-0.014%; Mg: 0.018-0.028%; Mn: 0.35-0.38%; Cr: 4.4-4.8%; Mo: 1.401-1.405%; V: 0.98-1.02%; Co: 0.024-0.026%; Eu: 0.012-0.013%; The rest is Fe and inevitable impurity elements.
Citation Information
Patent Citations
Production method for forging magnesium alloy plate under conditions of temperature reduction and large pressing quantity
CN102581058A
Cold ring rolling forming process for asymmetric shape of hub bearing outer ring and closed cold rolling forming die
CN103341577A
Preparation method of bearing ring
CN107881402A
High-speed high-performance bearing steel and preparation method thereof
CN109825762A
Production method of 3311 N20 carburizing bearing steel forge piece
CN113913688A