Preparation method of SOI high-temperature MEMS piezoresistive pressure sensor based on cantilever beam-center dual mass block structure
By designing the cantilever beam-center dual mass structure on the SOI substrate material sheet, the problems of reduced sensitivity and poor stability of traditional MEMS piezoresistive pressure sensors at high temperatures are solved, and higher sensitivity and stability are achieved, and the product is supported Diversification and rapid iteration of species.
Patent Information
- Application Number
- CN202411485673.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-23
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-10-23
AI Technical Summary
Traditional MEMS piezoresistive pressure sensors have problems such as decreased sensitivity, zero point drift and poor long-term stability in high temperature environments.
Using the SOI high-temperature MEMS piezoresistive pressure sensor preparation method based on cantilever beam-center double mass structure, by designing a symmetric cantilever beam-center double mass structure on the SOI substrate material sheet, combining high-precision lithography technology and high-temperature metal The interconnect structure of the material layer optimizes the stress distribution and deformation area, and enhances the sensitivity and stability of the sensor.
It effectively improves the sensitivity and signal strength of the sensor, reduces temperature drift, improves reliability and service life in high-temperature environments, improves dynamic response characteristics, and supports flexible adjustment and rapid iteration of product types.
Smart Images

Figure CN119018848A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of MEMS technology, and in particular to a method for preparing a SOI high-temperature MEMS piezoresistive pressure sensor based on a cantilever beam-central double-mass block structure. Background Art
[0002] Microelectromechanical system (MEMS) pressure sensors have been widely used in modern industry, aerospace, automobile manufacturing and other fields. However, traditional MEMS piezoresistive pressure sensors have problems such as decreased sensitivity, zero drift and poor long-term stability in high temperature environments. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing a SOI high-temperature MEMS piezoresistive pressure sensor based on a cantilever beam-central double-mass block structure, so as to solve the problems of decreased sensitivity, zero point drift and poor long-term stability of traditional MEMS piezoresistive pressure sensors in high temperature environments.
[0004] In order to solve the above technical problems, the present invention provides a method for preparing a SOI high temperature MEMS piezoresistive pressure sensor based on a cantilever beam-central double mass block structure, comprising: Step 1: Provide N <100> , the top silicon thickness is 1.5µm~100µm, the middle oxide layer thickness is 0.2µm~1.2µm, the substrate silicon thickness is 350µm~420µm, and the double-polished SOI substrate material sheet is subjected to a thermal oxidation process in a furnace tube to grow silicon dioxide layers on the front and back of the SOI substrate material sheet respectively; Step 2: Perform N-type isolation barrier structure photolithography process, inject glue, and remove photoresist; Step 3: Perform the photolithography process of the P-type varistor strip structure, inject the tape, and remove the photoresist; Step 4: Perform P-type interconnect structure photolithography process, inject glue, and remove photoresist; Step 5: Using a low-pressure chemical vapor deposition process in the furnace tube, a silicon dioxide layer and a silicon nitride layer are sequentially deposited on the front and back of the device, and an annealing process is performed; contact hole structure photolithography is performed, and the silicon dioxide layer and silicon nitride layer on the front are dry-etched to remove the photoresist; Step 6: Perform a photoresist coating process, a high-temperature metal material layer evaporation process, and a film coating process, and then strip the photoresist to form a metal interconnection structure; or, perform a high-temperature metal material layer sputtering process, a photoresist lithography process, and a metal interconnection structure etching process to remove the photoresist; Step 7: Deposit a passivation protection layer on the front of the device through a plasma enhanced chemical vapor deposition process, perform a passivation protection layer photolithography process, perform a passivation protection layer structure dry etching process, remove the photoresist, and perform an alloy process; Step 8: Perform photolithography of the front cantilever beam-center double-mass block structure and dry etching of the dielectric layer; wet etching of the top silicon of SOI by KOH at a temperature of 70°C to 80°C. The thickness of the top silicon film after wet etching depends on the pressure range requirements of the MEMS pressure sensor product; remove the photoresist; Step 9: Apply protective glue on the front side; Photolithography process of the back dielectric layer, dry etching process of the back dielectric layer, remove the photoresist; Photolithography process of the back cavity deep groove structure, first dry etching of the back cavity deep groove structure, etch out the height difference of the back center mass block structure, the height difference is 5µm~200µm, the dry etching process adopts deep reactive ion etching with a high selectivity of Si to SiO2 of 150:1~220:1, and the etching gas is sulfur hexafluoride; remove the photoresist; Step 10: Second dry etching of the back cavity deep groove structure. The dry etching process adopts deep reactive ion etching with a high selectivity of Si to SiO2 of 150:1~220:1, and the etching gas is sulfur hexafluoride. SOI intermediate oxide layer wet etching process, BOE corrosion rate 100nm / min~1000nm / min, check that the corrosion surface of the back cavity is dehydrated, indicating that the silicon dioxide layer is removed cleanly; remove the photoresist; remove the front protective glue; complete the preparation of SOI high-temperature MEMS piezoresistive pressure sensor based on cantilever beam-central double mass block structure.
[0005] In one embodiment, in the second step, the implanted ion type is phosphorus, the implantation energy is 80~100keV, the implantation dose is 4E15~9E15, and the implantation angle is 7°~10°; in the third step, the implanted ion type is boron, the implantation energy is 25~80keV, the implantation dose is 1.0E14~9E14, and the implantation angle is 7°~10°; in the fourth step, the implanted ion type is boron, the implantation energy is 25~80keV, the implantation dose is 4E15~9E15, and the implantation angle is 7°~10°.
[0006] In one embodiment, in the fifth step, the thickness of the newly deposited silicon dioxide layer is 0.2µm~0.5µm, the thickness of the silicon nitride layer is 0.1µm~0.2µm; the annealing temperature is 950℃~1200℃, the annealing time is 30min~150min; the contact hole size is 5µm~20µm.
[0007] In one embodiment, the thickness of the high temperature metal material layer is 1µm to 2µm, and the high temperature metal material is selected from platinum, titanium / platinum / gold multilayer structure or nickel-chromium alloy aluminum / copper alloy.
[0008] In one embodiment, in the seventh step, the passivation protective layer material is a single-layer silicon nitride layer or a stack of silicon dioxide and silicon nitride, wherein the stack of silicon dioxide and silicon nitride is a silicon dioxide layer and a silicon nitride layer deposited in sequence on the front side of the substrate material sheet that has completed the sixth step process, and the overall thickness of the passivation protective layer is 0.2µm~1.2µm; the alloy temperature is 400℃~500℃, and the alloy time is 30min~200min.
[0009] The present invention provides a method for preparing a SOI high-temperature MEMS piezoresistive pressure sensor based on a cantilever beam-central double-mass block structure, which has the following beneficial effects: (1) Based on the diaphragm structure design of the traditional MEMS piezoresistive pressure sensor, the present invention cleverly combines the cantilever beam-central dual mass block structure, and designs symmetrical central mass block structures on the front and back sides of the cantilever beam. Compared with the traditional diaphragm structure, the cantilever beam-central dual mass block symmetrical structure design can balance the forces on the front and back sides and better control the deformation area, optimize the stress distribution, avoid the stress concentration problem of large-area diaphragms at high temperatures, make the deformation of the cantilever beam under pressure more uniform, effectively reduce the nonlinear error caused by asymmetric stress, and effectively improve the reliability and service life of the sensor in high temperature environments. Compared with the traditional diaphragm structure and cantilever beam-central single mass block structure, this cantilever beam-central dual mass block innovative structural design can produce greater beam end deformation under the same pressure, improving the sensitivity and signal strength of the sensor; the structure balances the stress changes caused by temperature through symmetrical design, reduces the impact of temperature changes on sensor performance, greatly reduces temperature drift, and improves its stability in high temperature environments, so that the sensor exhibits excellent mechanical and electrical properties at high temperatures; the introduction of the central dual mass block not only increases the mass of the structure, but also improves the dynamic response characteristics of the sensor, making it have better performance in dynamic pressure measurement. In addition, the pressure range of the sensor can be adjusted by changing the corrosion depth of the front cantilever beam and the front central mass block, realizing the pressure range of product types, making the adjustment of product structure design more flexible, covering a wider range of product types, supporting faster product iteration and upgrading, and thus being able to quickly respond to market demand.
[0010] (2) The SOI substrate material sheet used in the present invention has excellent high-temperature performance and can maintain stable mechanical and electrical properties under high-temperature conditions. The present invention prepares a cantilever beam structure and a piezoresistive element on the top layer of single-crystal silicon of the SOI substrate material sheet. The SOI substrate material sheet further enhances the electrical insulation and thermal isolation performance of the sensor, reduces the influence of temperature on the electrical performance of the pressure sensor, and especially significantly reduces its zero drift under high-temperature conditions, thereby ensuring the stable operation of the pressure sensor.
[0011] (3) The present invention realizes a SOI high-temperature MEMS piezoresistive pressure sensor based on a cantilever beam-center dual-mass block structure and its preparation method through high-precision double-sided photolithography overlay technology, N-type isolation barrier structure technology, P-type varistor strip structure technology, high-temperature metal material layer interconnection structure technology, front cantilever beam-center dual-mass block structure corrosion technology, back cavity deep groove structure dry etching technology, etc. The cantilever beam-center dual-mass block structure processing method is innovatively designed, and the process method can improve product linearity and change product sensitivity by flexibly adjusting the back island thickness; the process method can flexibly adjust the top single crystal silicon corrosion depth of the front SOI substrate material sheet, and realize a single set of photolithography layout structure to complete the process mode of multiple pressure range chips, which speeds up the R&D cycle and reduces the R&D cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 It is a schematic diagram of the cross-sectional structure of the preparation process of the silicon dioxide layer structure of the SOI double-polished wafer deposited in the furnace tube.
[0013] Figure 2 It is a schematic diagram of the cross-sectional structure of the N-type isolation barrier structure preparation process.
[0014] Figure 3 It is a schematic diagram of the cross-sectional structure of the preparation process of the P-type varistor strip structure.
[0015] Figure 4 It is a schematic diagram of the cross-sectional structure of the preparation process of the P-type interconnect structure.
[0016] Figure 5 It is a schematic diagram of the cross-sectional structure of the contact hole structure preparation process.
[0017] Figure 6 It is a schematic diagram of the cross-sectional structure of the metal interconnect structure preparation process.
[0018] Figure 7 It is a schematic diagram of the cross-sectional structure of the passivation protection layer structure preparation process.
[0019] Figure 8 It is a schematic diagram of the cross-sectional structure of the preparation process of the front cantilever beam-central double mass block structure.
[0020] Fig. 9 This is a schematic diagram of the cross-sectional structure of the first dry etching back cavity deep trench structure preparation process.
[0021] Fig.10 It is a schematic diagram of the cross-sectional structure of the preparation process of a SOI high-temperature MEMS piezoresistive pressure sensor based on a cantilever beam-central double-mass block structure.
[0022] Fig.11 yes Figure 1, 2 , 3, 4, 5, 6, 7, 9, 10 are cross-sectional location diagrams of the cross-sectional structure diagrams.
[0023] Fig.12 yes Figure 8 Schematic diagram of the cross-section location of the cross-section structure diagram. DETAILED DESCRIPTION
[0024] The following is a further detailed description of a method for preparing a SOI high-temperature MEMS piezoresistive pressure sensor based on a cantilever beam-central dual-mass structure proposed by the present invention in combination with the accompanying drawings and specific embodiments. The advantages and features of the present invention will become clearer according to the following description. It should be noted that the accompanying drawings are all in a very simplified form and are not in precise proportions, and are only used to conveniently and clearly assist in explaining the purpose of the embodiments of the present invention.
[0025] The present invention provides a method for preparing a SOI high-temperature MEMS piezoresistive pressure sensor based on a cantilever beam-central double-mass block structure. The specific process flow of the preparation method comprises the following steps: Step 1: Provide N <100> , the top silicon thickness is 1.5µm~100µm, the middle oxide layer thickness is 0.2µm~1.2µm, the substrate silicon thickness is 350µm~420µm, and the double-polished SOI substrate material sheet; through the thermal oxidation process in the furnace tube, silicon dioxide layers are grown on the front and back of the SOI substrate material sheet respectively, and the silicon dioxide layer thickness is 0.1µm~0.2µm, such as Figure 1 shown.
[0026] Step 2: Perform N-type isolation barrier structure photolithography process, with photoresist injection, the injection ion type is phosphorus (P), the injection energy is 80~100keV, the injection dose is 4E15~9E15, and the injection angle is 7°~10°; remove the photoresist, such as Figure 2 shown.
[0027] Step 3: Perform the P-type varistor strip structure photolithography process, with glue injection, the injection ion type is boron (Boron, B), the injection energy is 25~80keV, the injection dose is 1.0E14~9E14, and the injection angle is 7°~10°; remove the photoresist, such as Figure 3 shown.
[0028] Step 4: Perform P-type interconnect structure photolithography process, with photoresist implantation, the implanted ion type is boron (Boron, B), the implantation energy is 25~80keV, the implantation dose is 4E15~9E15, and the implantation angle is 7°~10°; remove the photoresist, such as Figure 4 shown.
[0029] Step 5: Through the LPCVD (low pressure chemical vapor deposition) process in the furnace tube, a silicon dioxide layer and a silicon nitride layer are deposited on the front and back of the substrate material sheet that has completed the fourth step process. The thickness of the newly deposited silicon dioxide layer is 0.2µm~0.5µm, and the thickness of the silicon nitride layer is 0.1µm~0.2µm; an annealing process is performed, the annealing temperature is 950℃~1200℃, and the annealing time is 30min~150min; contact hole structure lithography is performed, and the contact hole size is 5µm~20µm. The silicon dioxide layer and silicon nitride layer on the front are etched by dry method to remove the photoresist, such as Figure 5 shown.
[0030] Step 6: Perform photoresist coating process, high temperature metal material layer evaporation process coating, lift-off photoresist, and form metal interconnection structure. Alternatively, remove photoresist through high temperature metal material layer sputtering process, photoresist photolithography process, and metal interconnection structure etching process. The thickness of high temperature metal material layer is 1µm~2µm. High temperature metal materials can be selected from platinum (Platinum, Pt), titanium / platinum / gold (Ti / Pt / Au) multilayer structure, nickel-chromium alloy (Nickel-Chromium Alloy, NiCr) aluminum / copper alloy (Al / Cu), etc. Figure 6 shown.
[0031] Step 7: Deposit a passivation protective layer on the front of the substrate material sheet that has completed the sixth step process through the PECVD (plasma enhanced chemical vapor deposition) process. The passivation protective layer material can be a single silicon nitride layer or a stack of silicon dioxide and silicon nitride, wherein the stack of silicon dioxide and silicon nitride is to deposit a silicon dioxide layer and a silicon nitride layer in sequence on the front of the substrate material sheet that has completed the sixth step process. The overall thickness of the passivation protective layer is 0.2µm~1.2µm; perform a passivation protective layer photolithography process, a passivation protective layer structure dry etching process, and remove the photoresist; alloy process, the alloy temperature is 400℃~500℃, the alloy time is 30min~200min, such as Figure 7 shown.
[0032] Step 8: Perform the front cantilever beam-center double-mass block structure photolithography process and dielectric layer dry etching process; SOI top silicon KOH wet etching, the etching temperature is 70℃~80℃, the thickness of the top silicon film after wet etching depends on the pressure range requirements of the MEMS pressure sensor product; remove the photoresist, such as Figure 8 shown.
[0033] Step 9: Apply protective glue on the front side; Photolithography process of the back dielectric layer, dry etching process of the back dielectric layer, remove the photoresist; Photolithography process of the back cavity deep groove structure, first dry etching of the back cavity deep groove structure, etch out the height difference of the back center mass block structure, the height difference is 5µm~200µm, the dry etching process adopts deep reactive ion etching (DRIE) with high selectivity of Si to SiO2 of 150:1~220:1, and the etching gas is sulfur hexafluoride (SF6); remove the photoresist; such as Fig. 9 shown.
[0034] Step 10: The back cavity deep groove structure is dry-etched for the second time. The dry-etching process uses deep reactive ion etching (DRIE) with a high selectivity of 150:1~220:1 for Si to SiO2, and sulfur hexafluoride (SF6) is used as the etching gas. The SOI intermediate oxide layer is wet-etched with a BOE etching rate of 100nm / min~1000nm / min. Check that the corrosion surface of the back cavity is dehydrated, indicating that the silicon dioxide layer has been removed cleanly. Remove the photoresist. Remove the front protective glue. Complete the preparation of the SOI high-temperature MEMS piezoresistive pressure sensor based on the cantilever beam-central double-mass block structure, such as Fig.10 shown.
[0035] Fig.11 yes Figure 1 , 2 , 3, 4, 5, 6, 7, 9, 10 section location schematic diagram; Fig.12 yes Figure 8 Schematic diagram of the section location.
[0036] The application of traditional MEMS piezoresistive pressure sensors in high temperatures is limited by structural design and material properties. The present invention provides a method for preparing a SOI high-temperature MEMS piezoresistive pressure sensor based on a cantilever beam-central dual-mass block structure. On the basis of the diaphragm structure design of traditional MEMS piezoresistive pressure sensors, an advanced SOI substrate material sheet is used, and the cantilever beam-central dual-mass block innovative structure is cleverly combined. A symmetrical central mass block is designed on the front and back sides of the cantilever beam, respectively, successfully breaking through these limitations and expanding the application range of the sensor. The present invention realizes a SOI high-temperature MEMS piezoresistive pressure sensor based on a cantilever beam-central dual-mass block structure and a preparation method thereof through high-precision double-sided photolithography overlay process technology, N-type isolation barrier structure process technology, P-type varistor strip structure process technology, high-temperature metal material layer interconnection structure process technology, front cantilever beam-central dual-mass block structure corrosion technology, back cavity deep groove structure dry etching process technology, etc. An innovative cantilever beam-central dual-mass block structure processing method is designed. This process method can improve product linearity and change product sensitivity by flexibly adjusting the back island thickness. This process method can flexibly adjust the top single crystal silicon corrosion depth of the front SOI substrate material sheet, and realize a single set of photolithography pattern structure to complete the process processing mode of various pressure range chips, which speeds up the R&D cycle and reduces R&D costs.
[0037] The above description is only a description of the preferred embodiments of the present invention, and is not intended to limit the scope of the present invention. Any changes or modifications made by a person skilled in the art in the field of the present invention based on the above disclosure shall fall within the scope of protection of the claims.
Claims
1. A method for preparing a SOI high temperature MEMS piezoresistive pressure sensor based on a cantilever beam-central double mass block structure, characterized in that: include: Step 1: Provide N <100> , the top silicon thickness is 1.5µm~100µm, the middle oxide layer thickness is 0.2µm~1.2µm, the substrate silicon thickness is 350µm~420µm, and the double-polished SOI substrate material sheet is subjected to a thermal oxidation process in a furnace tube to grow silicon dioxide layers on the front and back of the SOI substrate material sheet respectively; Step 2: Perform N-type isolation barrier structure photolithography process, inject glue, and remove photoresist; Step 3: Perform the photolithography process of the P-type varistor strip structure, inject the tape, and remove the photoresist; Step 4: Perform P-type interconnect structure photolithography process, inject glue, and remove photoresist; Step 5: Using a low-pressure chemical vapor deposition process in the furnace tube, a silicon dioxide layer and a silicon nitride layer are sequentially deposited on the front and back of the device, and an annealing process is performed; contact hole structure photolithography is performed, and the silicon dioxide layer and silicon nitride layer on the front are dry-etched to remove the photoresist; Step 6: Perform a photoresist coating process, a high-temperature metal material layer evaporation process, and a film coating process, and then strip the photoresist to form a metal interconnection structure; or, perform a high-temperature metal material layer sputtering process, a photoresist lithography process, and a metal interconnection structure etching process to remove the photoresist; Step 7: Deposit a passivation protection layer on the front of the device by plasma enhanced chemical vapor deposition process, perform passivation protection layer photolithography process, and perform passivation protection layer structure dry etching process to remove the photoresist; Carry out alloying process; Step 8: Perform photolithography of the front cantilever beam-center double-mass block structure and dry etching of the dielectric layer; wet etching of the top silicon of SOI by KOH at a temperature of 70°C to 80°C. The thickness of the top silicon film after wet etching depends on the pressure range requirements of the MEMS pressure sensor product; remove the photoresist; Step 9: Apply protective glue on the front; Back dielectric layer photolithography process, back dielectric layer dry etching process, removal of photoresist; Back cavity deep groove structure photolithography process, the first dry etching of the back cavity deep groove structure, etching out the height difference of the back center mass block structure, the height difference is 5µm~200µm, the dry etching process adopts deep reactive ion etching with a high selectivity of Si to SiO2 of 150:1~220:1, and the etching gas is sulfur hexafluoride; Removing photoresist; Step 10: The back cavity deep groove structure is dry-etched for the second time. The dry-etching process uses deep reactive ion etching with a high selectivity of 150:1~220:1 for Si to SiO2, and sulfur hexafluoride is used as the etching gas. The SOI intermediate oxide layer is wet-etched with a BOE etching rate of 100nm / min~1000nm / min. Check that the corrosion surface of the back cavity is dehydrated, indicating that the silicon dioxide layer has been removed completely. Removing photoresist; Remove the front protective glue; The preparation of SOI high-temperature MEMS piezoresistive pressure sensor based on cantilever beam-central double mass block structure has been completed.
2. The method for preparing the SOI high temperature MEMS piezoresistive pressure sensor based on the cantilever beam-central dual mass block structure according to claim 1, characterized in that: In the second step, the implanted ion type is phosphorus, the implantation energy is 80~100keV, the implantation dose is 4E15~9E15, and the implantation angle is 7°~10°; in the third step, the implanted ion type is boron, the implantation energy is 25~80keV, the implantation dose is 1.0E14~9E14, and the implantation angle is 7°~10°; in the fourth step, the implanted ion type is boron, the implantation energy is 25~80keV, the implantation dose is 4E15~9E15, and the implantation angle is 7°~10°.
3. The method for preparing the SOI high temperature MEMS piezoresistive pressure sensor based on the cantilever beam-central dual mass block structure according to claim 1, characterized in that: In the fifth step, the thickness of the newly deposited silicon dioxide layer is 0.2µm~0.5µm, and the thickness of the silicon nitride layer is 0.1µm~0.2µm; the annealing temperature is 950℃~1200℃, and the annealing time is 30min~150min; the contact hole size is 5µm~20µm.
4. The method for preparing the SOI high temperature MEMS piezoresistive pressure sensor based on the cantilever beam-central dual mass block structure according to claim 1, characterized in that: The thickness of the high temperature metal material layer is 1µm-2µm, and the high temperature metal material is selected from platinum, titanium / platinum / gold multilayer structure or nickel-chromium alloy aluminum / copper alloy.
5. The method for preparing the SOI high temperature MEMS piezoresistive pressure sensor based on the cantilever beam-central dual mass block structure according to claim 1, characterized in that: In the seventh step, the passivation protective layer material is a single-layer silicon nitride layer or a stack of silicon dioxide and silicon nitride, wherein the stack of silicon dioxide and silicon nitride is a silicon dioxide layer and a silicon nitride layer deposited in sequence on the front side of the substrate material sheet that has completed the sixth step process, and the overall thickness of the passivation protective layer is 0.2µm~1.2µm; the alloy temperature is 400℃~500℃, and the alloy time is 30min~200min.
Citation Information
Patent Citations
Dielectric isolation piezoresistive pressure sensor and method for manufacturing same
CN102998037A
MEMS piezoresistive pressure sensor and production method thereof
CN105716750A
Pressure sensor, pressure sensor module, electronic apparatus, and moving body
CN108622844A
Micromechanical resonant pressure sensor and manufacturing method thereof
CN113063529A
Micro-pressure MEMS pressure sensor chip and preparation method thereof
CN114414110A
Cited By
SOI-based high-efficiency preparation method and system for low-null-drift pressure chip