Preparation method of crosslinked cellulose hard carbon microsphere negative electrode material
By using renewable microcrystalline cellulose to prepare crosslinked cellulose hard carbon microspheres, the problem of small spacing between the negative electrode materials in sodium ion batteries is solved, and a negative electrode material with high specific capacity and high Coulomb efficiency is achieved, which promotes the promotion of The industrial application of sodium ion batteries.
Patent Information
- Application Number
- CN202310607682.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-05-26
AI Technical Summary
There is a lack of a low-cost and excellent performance negative electrode material in sodium ion batteries. Graphite materials are difficult to nest sodium ions due to small spacing, which limits the industrial application of sodium ion batteries.
Renewable microcrystalline cellulose is used as the precursor, and the crystallinity and crosslinking degree of microspheres are adjusted through molecular cross-linking and regeneration strategies, and cross-linked cellulose hard carbon microspheres are prepared through carbonization to form a negative electrode with a through-pore structure. Material.
The prepared crosslinked cellulose hard carbon microsphere negative electrode material has high specific capacity, high Coulomb efficiency and low charging and discharge platform, which is suitable for sodium ion battery applications.
Smart Images

Figure FT_1 
Figure FT_2
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a battery negative electrode material, in particular to a method for preparing a cross-linked cellulose hard carbon microsphere negative electrode material. Background Art
[0002] In recent years, sodium-ion batteries have attracted widespread attention from academia and industry at home and abroad for their advantages such as low cost, high safety and excellent electrochemical performance. Sodium-ion batteries have a similar energy storage mechanism to lithium-ion batteries, and compared with lithium ions, sodium ions are abundant in reserves, have low extraction costs, and have advantages such as high energy density, safety and environmental protection. From the development history of lithium-ion batteries, the research on negative electrode materials has played an important role in promoting the commercialization of lithium-ion batteries. In particular, the emergence of negative electrode materials represented by graphite has directly promoted the commercial application of lithium-ion batteries. However, the spacing between graphite is small, and it is difficult for larger sodium ions to fit into the graphite gap. In order to achieve an industrial breakthrough in sodium-ion batteries, it is necessary to find a negative electrode material that is as low-cost and has excellent performance as the graphite negative electrode of lithium-ion batteries.
[0003] Hard carbon is an amorphous carbon material that is difficult to graphitize. It has a wide range of sources and is usually divided into resin-based carbon, organic polymer pyrolytic carbon, carbon black and biomass carbon. Hard carbon materials have high reversible specific capacity, wide electrochemical window, low sodium insertion voltage, high charge and discharge rate, and are stable at high and low temperatures, have good compatibility with electrolytes, and are not prone to spontaneous combustion. More importantly, the amorphous structure of hard carbon makes its gaps larger and can embed larger sodium ions. Therefore, it is considered to be an ideal negative electrode material for sodium ion batteries. In 2000, Stevens used glucose as a precursor to prepare a hard carbon material with a sodium storage capacity of 300 mAh / g for the first time, and successfully matched it with the positive electrode material. Based on this, the present invention uses renewable microcrystalline cellulose as a precursor, adopts a molecular crosslinking and regeneration strategy, adjusts the crystallinity and crosslinking degree of microcrystalline cellulose microspheres, and then carbonizes them. The prepared crosslinked cellulose hard carbon microspheres have a macroporous structure and a rich microporous structure on a macroscopic scale, which is conducive to the efficient wetting of the electrolyte. Summary of the invention
[0004] A method for preparing a cross-linked cellulose hard carbon microsphere negative electrode material, characterized in that: (1) Preparation of cross-linked cellulose microspheres: 5.0 g NaOH, 4.0 g thiourea, and 50 mL deionized water were added to a 100 mL three-necked flask in sequence, and mechanically stirred in an ice-water bath. Then, 3.0 g microcrystalline cellulose was added, and strong mechanical stirring was performed for 15 to 20 min. Then, 0 to 2.0 mL epichlorohydrin was added to obtain a microcrystalline cellulose solution. At the same time, 40 mL white oil, 80 mL isooctane, 1.0 g Tween 80, and 4.0 g Span 80 were mechanically stirred to prepare an oil phase. 10 mL of the microcrystalline cellulose solution was slowly injected into the oil phase for emulsification into spheres. The temperature was 35°C for 30 to 60 min, and the cross-linked cellulose microspheres were centrifuged. The prepared cross-linked cellulose microspheres were replaced three times with 15 mL isopropanol and 10 mL aqueous solution, and then washed with deionized water until neutral. The cross-linked cellulose microspheres were freeze-dried to obtain cross-linked cellulose microspheres. (2) Preparation of cross-linked cellulose hard carbon microspheres: Weigh 10 g of the cross-linked cellulose microspheres obtained in the previous step and place them in a corundum crucible. Set the protective gas to high-purity argon (99.999% purity). Set the heating rate curve to 50℃ ~ 180℃ for 60 min, 180℃ ~ 230℃ for 1800 min, and 3℃ / min to 900 ~ 1200℃, and keep warm for 1 ~ 2 h; set the cooling rate curve to -3℃ / min to 200℃, then start natural cooling. Finally, wash the obtained cross-linked cellulose hard carbon microspheres with 20% KOH at 70℃ for 2 h, 2 mol / L HCl solution at 60℃ for 15 h, and then wash with deionized water until neutral, and dry at 110℃ for 12 h to obtain cross-linked cellulose hard carbon microspheres.
[0005] As a preference: (1) A method for preparing a cross-linked cellulose hard carbon microsphere negative electrode material as claimed in claim 1, characterized in that in the process of preparing the cross-linked cellulose microspheres cited in step (2), the equivalent of epichlorohydrin is 1.2 mL; (2) The method for preparing a cross-linked cellulose hard carbon microsphere negative electrode material as claimed in claim 1, characterized in that in the process of preparing the cross-linked cellulose microspheres cited in step (1), the volume ratio of the oil phase to white oil: isooctane is 2:1; (3) The method for preparing a cross-linked cellulose hard carbon microsphere negative electrode material as claimed in claim 1, characterized in that in the process of preparing the cross-linked cellulose hard carbon microspheres cited in step (2), the heating rate curve is 50°C ~ 180°C heating for 60 min, 180°C ~ 230°C heating for 1800 min, 230°C ~ 1200°C heating for 320 min, and 1200°C insulation for 60 min; (4) The method for preparing a cross-linked cellulose hard carbon microsphere negative electrode material as claimed in claim 1, characterized in that in the process of preparing the cross-linked cellulose hard carbon microspheres cited in step (2), the cooling rate curve is set as: 1200℃ ~ 50℃ cooling for 380 min; (5) A method for preparing a cross-linked cellulose hard carbon microsphere negative electrode material as described in claim 1, characterized in that in the process of preparing the cross-linked cellulose hard carbon microspheres cited in step (2), the post-treatment process is washing with 20% KOH at 70°C for 2 hours, washing with 2 mol / L HCl solution at 60°C for 15 hours, then washing with deionized water until neutral, and drying at 110°C for 12 hours.
[0006] The beneficial effects of the present invention are as follows: (1) The present invention uses renewable microcrystalline cellulose as a precursor, destroys the original crystal structure of microcrystalline fibers through molecular cross-linking, reduces the crystallinity of the raw materials, and promotes the formation of pseudo-graphitization domains of hard carbon.
[0007] (2) The cross-linked cellulose hard carbon microsphere negative electrode material prepared by the present invention has high specific capacity for sodium ion batteries, high coulombic efficiency, and low charge and discharge platform. BRIEF DESCRIPTION OF THE DRAWINGS
[0008] Figure 1 : Scanning electron microscope image of the cross-linked cellulose hard carbon microsphere negative electrode material prepared by the method of the present invention; Figure 2 : Constant current charge-discharge curve of cross-linked cellulose hard carbon microspheres prepared by the method of the present invention. DETAILED DESCRIPTION
[0009] The following examples further illustrate the content of the present invention, but should not be construed as limiting the present invention. Without departing from the spirit and essence of the present invention, modifications or substitutions made to the methods, steps or conditions of the present invention all fall within the scope of the present invention.
[0010] Implementation Case 1: Preparation of cross-linked cellulose microspheres: 5.0 g NaOH, 4.0 g thiourea, and 50 mL deionized water were added to a 100 mL three-necked flask, and mechanically stirred in an ice-water bath. Then, 3.0 g microcrystalline cellulose was added, and strong mechanical stirring was performed for 15 to 20 min. Then, 1.2 mL epichlorohydrin was added to obtain a microcrystalline cellulose solution. At the same time, 40 mL white oil, 80 mL isooctane, 1.0 g Tween 80, and 4.0 g Span 80 were mechanically stirred to prepare an oil phase. 10 mL of the microcrystalline cellulose solution was slowly injected into the oil phase for emulsification into spheres. The temperature was 35°C, and the time was 30 to 60 min. The cross-linked cellulose microspheres were replaced three times with 15 mL isopropanol and 10 mL aqueous solution, and then washed with deionized water until neutral, and freeze-dried to obtain cross-linked cellulose microspheres. (2) Preparation of cross-linked cellulose hard carbon microspheres: Weigh 10 g of the cross-linked cellulose microspheres obtained in the previous step and place them in a corundum crucible. Set the protective gas to high-purity argon (99.999% purity). Set the heating rate curve to 50℃ ~ 180℃ for 60 min, 180℃ ~ 230℃ for 1800 min, 230℃ ~ 1200℃ for 323 min, and keep at 1200℃ for 2 h. Set the cooling rate curve to: 1200 ~ 300℃ for 300 min, start natural cooling, and finally wash the obtained cross-linked cellulose hard carbon microspheres with 20% KOH at 70℃ for 2 h, 2 mol / L HCl solution at 60℃ for 15 h, and then wash with deionized water until neutral, and dry at 110℃ for 12 h to obtain cross-linked cellulose hard carbon microspheres.
[0011] Implementation Case 2: Half-cell assembly and testing, preparation of negative electrode sheet: 0.92 g cross-linked cellulose hard carbon microspheres, 0.03 g SuperP, 0.10 g 1.5 wt% sodium carboxymethyl cellulose solution, 0.07 g 40 wt% styrene-butadiene rubber solution, 0.60 g deionized water, homogenization for 20 min, using a four-sided preparation device, the slurry is evenly applied to the surface of a single-sided polished copper foil with a thickness of 100 μm, dried at 105°C for 8 h, and the sheet diameter is 12 mm; preparation of positive electrode sheet: metallic sodium is pressed to a thickness of 0.8 mm using a roller press, and the sheet diameter is 12 mm; button battery assembly order (from bottom to top): positive electrode shell, spring, gasket, sodium sheet, glass fiber separator, sodium hexafluorophosphate electrolyte (1 mol / L NaPF6 dissolved in ethylene carbonate: ethylene carbonate, volume ratio of 1:1), negative electrode sheet, negative electrode shell. All assembly processes were performed in an anaerobic chamber (O2 concentration ≤ 0.5 ppm, water concentration ≤ 0.1 ppm).
Claims
1. A method for preparing a cross-linked cellulose hard carbon microsphere negative electrode material, characterized in that The steps include: (1) Preparation of cross-linked cellulose microspheres: 5.0 g NaOH, 4.0 g thiourea, and 50 mL deionized water were added to a 100 mL three-necked flask in sequence, and mechanically stirred in an ice-water bath. Then, 3.0 g microcrystalline cellulose was added. After strong mechanical stirring for 15 to 20 min, 1.2 mL epichlorohydrin was added to obtain a microcrystalline cellulose solution. At the same time, 40 mL white oil, 80 mL isooctane, 1.0 g Tween 80, and 4.0 g Span 80 were mechanically stirred to prepare an oil phase. 10 mL of the microcrystalline cellulose solution was slowly injected into the oil phase for emulsification into spheres. The temperature was 35 °C for 30 to 60 min, and the prepared cross-linked cellulose microspheres were replaced three times with 20 mL isopropanol / water solution (isopropanol: water volume ratio of 4:1), and then washed with deionized water until neutral, and freeze-dried to obtain cross-linked cellulose microspheres. (2) Preparation of cross-linked cellulose hard carbon microspheres: 10 g The cross-linked cellulose microspheres obtained in the previous step were placed in a corundum crucible, and the protective gas was set to high-purity argon (99.999% purity). The heating rate curve was set to 50℃ ~ 180℃ for 60 min, 180℃ ~ 230℃ for 1800 min, 230℃ ~ 1200℃ for 320 min, and 1200℃ for 60 min. The cooling rate curve was set to: 1200℃ ~ 50℃ for 380 min. Finally, the obtained cross-linked cellulose hard carbon microspheres were washed with 20% KOH at 70℃ for 2h, washed with 2 mol / L HCl solution at 60℃ for 15h, and then washed with deionized water until neutral, and dried at 110℃ for 12h to obtain cross-linked cellulose hard carbon microspheres.
2. The method for preparing a negative electrode material of cross-linked cellulose hard carbon microspheres according to claim 1, characterized in that In the process of preparing cross-linked cellulose microspheres cited in step (1), the equivalent amount of epichlorohydrin was 1.2 mL.
3. The method for preparing a negative electrode material of cross-linked cellulose hard carbon microspheres according to claim 1, characterized in that In the process of preparing cross-linked cellulose microspheres cited in step (1), the volume ratio of white oil to isooctane in the oil phase is 2:
1.
4. The method for preparing a negative electrode material of cross-linked cellulose hard carbon microspheres according to claim 1, characterized in that In the process of preparing cross-linked cellulose hard carbon microspheres cited in step (2), the heating rate curve is 50°C ~ 180°C heating for 60 min, 180°C ~ 230°C heating for 1800 min, 230°C ~ 1200°C heating for 320 min, and keeping at 1200°C for 60 min.
5. The method for preparing a negative electrode material of cross-linked cellulose hard carbon microspheres according to claim 1, characterized in that In the process of preparing cross-linked cellulose hard carbon microspheres cited in step (2), the cooling rate curve is set as: 1200℃ ~ 50℃ cooling for 380 min.
6. The method for preparing a negative electrode material of cross-linked cellulose hard carbon microspheres according to claim 1, characterized in that In the process of preparing cross-linked cellulose hard carbon microspheres cited in step (2), the post-treatment process is washing with 20% KOH at 70°C for 2h, washing with 2mol / L HCl solution at 60°C for 15h, then washing with deionized water until neutral, and drying at 110°C for 12h.
Citation Information
Patent Citations
Preparation method of active carbon uniformly doped with metal
CN108190885A
Gas separation method
JP2020014978A
KR20200021214A